Magnetically-driven liquid metal micron robot as well as preparation method and application thereof
Through the combined structure of liquid metal skeleton, magnetic particles and polymer layers, the external magnetic field is used to control the movement of micro-robots, which solves the problem of insufficient adaptability of solid micro-nano robots in biological environments and realizes operation in complex environments. Stable, controllable movement and biocompatibility, it has a wide range of therapeutic applications for neurological diseases.
Patent Information
- Application Number
- CN202410901234.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-05
AI Technical Summary
Existing micro-nano robots are mainly composed of solid materials, resulting in insufficient adaptability in biological environments, which may have unpredictable effects on organisms, and are difficult to achieve precise control in complex environments.
Using a combined structure of a liquid metal skeleton, magnetic particles and polymer layers, the movement direction and speed of the microrobot are controlled by an external magnetic field, and a magnetically driven liquid metal microrobot with controllable size is prepared using ultrasonic method.
It achieves stable and controllable movement in a biological environment, has good biocompatibility and efficient therapeutic application prospects, especially in the field of wireless remote treatment of neurological diseases.
Smart Images

Figure CN118769264A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of micron device preparation, and in particular relates to a magnetically driven liquid metal micron robot and a preparation method and application thereof. Background Art
[0002] A micro-nano robot is a micro-nano device that can convert other forms of energy into kinetic energy at the micro-nano scale and can move autonomously.
[0003] At present, most micro-nano robots are mainly composed of solid micro-nano structures. However, the inherent mechanical property limitations of these rigid solid materials limit their adaptability, and when they encounter mismatches with the target environment, especially in biological environments, they may cause unpredictable effects on organisms. Therefore, it is urgent to develop a new magnetically driven liquid metal micro-robot to solve the shortcomings of existing micro-nano robots in application. Summary of the invention
[0004] The purpose of the present invention is to provide a magnetically driven liquid metal micro robot and its preparation method and application. The magnetically driven liquid metal micro robot in the present invention has certain stability, controllable size, good biocompatibility, fast movement speed, controllable movement direction, and controllable movement mode. Therefore, it has broad application prospects in the field of wireless remote treatment of neurological diseases in various complex biological environments.
[0005] In a first aspect, the present invention provides a magnetically driven liquid metal micro-robot, comprising a liquid metal skeleton, magnetic particles and a polymer layer; wherein the magnetic particles are distributed inside the liquid metal skeleton, and the polymer layer is coated on the surface of the liquid metal skeleton.
[0006] In the present invention, the inventors have discovered that liquid metal has good fluidity and high surface tension. Liquid metal is used as a skeleton and magnetic particles are evenly distributed inside it. The resulting magnetically driven liquid metal micro-robot can move in a directed manner under the action of an external magnetic field. Furthermore, a high molecular polymer layer is coated on the surface of the liquid metal to prevent the magnetically driven liquid metal micro-robot from agglomerating and improve the stability of the magnetically driven liquid metal micro-robot.
[0007] In some embodiments, the particle size of the magnetically driven liquid metal microrobot is 0.1-200 μm, for example, it can be 0.1 μm, 1 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm or other values within this range.
[0008] In the present invention, by controlling the particle size of the magnetically driven liquid metal micro-robot within different ranges, it is beneficial to apply the magnetically driven liquid metal micro-robot in different complex biological environments.
[0009] In some embodiments, the particle size of the magnetic particles is 10-1000 nm, for example, it can be 10 nm, 20 nm, 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, 550 nm, 600 nm, 650 nm, 700 nm, 750 nm, 800 nm, 850 nm, 900 nm, 950 nm, 1000 nm or other values within this range.
[0010] In some preferred embodiments, the particle size of the magnetic particles is 100 nm.
[0011] In the present invention, by controlling the particle size of the magnetic particles within a specific range, the magnetic particles can more efficiently enter the interior of the liquid metal skeleton and be more evenly distributed in the interior of the liquid metal skeleton.
[0012] In some embodiments, the mass ratio of magnetic particles to liquid metal is 1:(5-30), for example, 1:5, 1:10, 1:15, 1:20, 1:25, 1:30 or other ratios within this range.
[0013] In some preferred embodiments, the mass ratio of magnetic particles to liquid metal is 1:10.
[0014] In some embodiments, the liquid metal includes at least one of gallium, indium, tin, and zinc.
[0015] In the present invention, the liquid metal may, for example, include only gallium, or only indium, or only tin, or only zinc, or an alloy composed of at least one of gallium, indium, tin and zinc, for example, it may be a gallium-indium binary alloy, or a gallium-tin binary alloy, or a gallium-zinc binary alloy, or an indium-tin binary alloy, or an indium-zinc binary alloy, or a tin-zinc binary alloy, or a gallium-indium-tin ternary alloy, or a gallium-indium-zinc ternary alloy, or an indium-tin-zinc ternary alloy, or a gallium-indium-tin-zinc ternary alloy, or a gallium-indium-tin-zinc quaternary alloy, and in the above alloys, the mass ratio of each metal can be conventionally adjusted according to actual use needs.
[0016] In some preferred embodiments, the liquid metal is a gallium-indium alloy.
[0017] In some embodiments, the magnetic particles include at least one element of iron, cobalt, nickel, and gadolinium.
[0018] In the present invention, the magnetic particles may include, for example, only iron, or only cobalt, or only nickel, or only gadolinium, or may be oxides of iron, cobalt, nickel and gadolinium, such as ferrosoferric oxide.
[0019] In some preferred embodiments, the magnetic particles are iron powder.
[0020] In the present invention, the magnetic particles can sense the external magnetic field and generate magnetic response, so that the robot can generate directional movement or change the robot's movement speed. Specifically, the magnetic particles can generate directional movement of the robot by responding to the external oscillating magnetic field or rotating magnetic field. Changing the magnetic field strength and frequency can also change the robot's movement speed. The magnetic field control direction is real-time and can accurately control the movement direction.
[0021] In some embodiments, the high molecular polymer includes at least one of polypropylene, polydopamine, polypyrrole, polyaniline, polymethyl methacrylate, polystyrene, polyamide, polyacrylonitrile, polybutylene, polyethylene oxide, polyimide, polyethylene glycol, polyvinyl pyrrolidone, polyvinyl alcohol, polyacrylic acid and polyacrylamide.
[0022] In some preferred embodiments, the high molecular weight polymer is polyvinyl pyrrolidone. In some more preferred embodiments, the molecular weight of polyvinyl pyrrolidone is 3000-1300000, for example, it can be 3000, 5000, 10000, 20000, 30000, 40000, 50000, 60000, 70000, 80000, 90000, 95000, 100000, 110000, 1200000, 1300000 or other values within this range.
[0023] In some more preferred embodiments, the molecular weight of polyvinylpyrrolidone is 95,000.
[0024] In a second aspect, the present invention provides a method for preparing a magnetically driven liquid metal micro-robot as described in any of the above items, comprising the following steps: providing liquid metal and a polymer acid solution respectively; adding the liquid metal to the acid solution, and then adding magnetic particles to obtain magnetic liquid metal; adding the magnetic liquid metal to the polymer acid solution, and obtaining a magnetically driven liquid metal micro-robot after ultrasonic treatment.
[0025] In the present invention, a magnetically driven liquid metal micrometer robot with controllable size and certain structural stability is prepared by ultrasonic method. The preparation process is simple, the preparation process can prepare liquid metal micrometer robots in large quantities, and the size of the magnetically driven liquid metal micrometer robot can be controlled by regulating the ultrasonic time and ultrasonic power.
[0026] In some embodiments, in the provided high molecular weight polymer acid solution, the acid solution comprises a hydrochloric acid solution.
[0027] In the present invention, the acid solution may be any conventional acid solution in the prior art, such as a sulfuric acid solution, a nitric acid solution or a hydrochloric acid solution. In the present invention, a hydrochloric acid solution is preferred.
[0028] In some preferred embodiments, the pH value of the polymer acid solution is 1-5, for example, 1, 2, 3, 4, 5 or other values within the range.
[0029] In some more preferred embodiments, the pH value of the high molecular weight polymer acid solution is 3.
[0030] In some embodiments, during the preparation of the magnetic liquid metal, the acid solution includes a hydrochloric acid solution.
[0031] In the present invention, the acid solution may be any conventional acid solution in the prior art, such as a sulfuric acid solution, a nitric acid solution or a hydrochloric acid solution. In the present invention, a hydrochloric acid solution is preferred.
[0032] In some preferred embodiments, the concentration of the hydrochloric acid solution is 0.5-5 mol / L, for example, it can be 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, 5 mol / L or other values within this range.
[0033] In some more preferred embodiments, the concentration of the hydrochloric acid solution is 5 mol / L.
[0034] In the present invention, during the preparation process of the magnetic liquid metal, the addition of a hydrochloric acid solution can remove the oxide layer on the surface of the liquid metal, thereby obtaining a liquid metal with a smooth and bright surface.
[0035] In a third aspect, the present invention provides the use of any of the magnetically driven liquid metal micro-robots described above in wireless remote treatment of neurological diseases.
[0036] In the present invention, the magnetically driven liquid metal micro-robot can pass through narrow channels, deform and pass through a simulated in vitro blood-brain barrier, and magnetically stimulate nerve cells under the condition of a rotating magnetic field under the control of an external magnetic field. Therefore, it has good application prospects in the wireless remote treatment of neurological diseases.
[0037] Compared with the prior art, the present invention has the following advantages: 1) The magnetically driven liquid metal micro-robot in the present invention has certain stability, controllable size, good biocompatibility, fast movement speed, controllable movement direction, and controllable movement mode. Therefore, it has broad application prospects in the field of wireless remote treatment of neurological diseases in various complex biological environments; 2) Due to the mechanical properties of magnetic nanoparticles, the magnetically driven liquid metal micro-robot of the present invention can respond to external magnetic fields and can achieve precise control of movement direction and speed in oscillating and rotating magnetic fields; 3) Since liquid metal is non-toxic and bio-friendly, the magnetically driven liquid metal micro-robot in the present invention has excellent performance in the field of disease treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 Schematic diagram of the preparation process of the magnetically driven liquid metal micro robot in the present invention; Figure 2 The transmission electron microscope image and elemental analysis image of the magnetically driven liquid metal micro-robot prepared in Example 1 of the present invention; Figure 3 This is a scanning electron microscope image of the material prepared in Example 1 of the present invention without being screened by a magnet; Figure 4 This is a scanning electron microscope image of the magnetically driven liquid metal micro robot prepared in Comparative Example 1 of the present invention; Figure 5 This is a graph of the movement speeds of magnetically driven liquid metal micro-robots with different particle sizes (4 μm, 7 μm, 10 μm, and 15 μm) prepared in Example 1 of the present invention under the same magnetic field conditions; Figure 6 It is a time-lapse diagram of the movement of magnetically driven liquid metal micro-robots with different particle sizes (4 μm, 7 μm, 10 μm, 15 μm) prepared in Example 1 of the present invention under the same magnetic field conditions; Figure 7 This is a result diagram of the magnetically driven liquid metal micro-robot with a particle size of 10 μm prepared in Example 1 of the present invention climbing over an obstacle with a height of 40 μm under the action of a rotating magnetic field; Figure 8 This is a result diagram of the magnetically driven liquid metal micro-robot with a particle size of 15 μm prepared in Example 1 of the present invention passing through a narrow channel of 10 μm under the combined action of a rotating magnetic field and a simulated flow field; Fig. 9 This is a fluorescence microscope image of the magnetically driven liquid metal micro-robot prepared in Example 5 of the present invention activating nerve cells under the action of magnetic force. DETAILED DESCRIPTION
[0039] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] The experimental methods without specific conditions in the examples are usually carried out according to conventional conditions and conditions described in the manual, or according to conditions recommended by the manufacturer. The general equipment, materials, reagents, etc. used are all available from commercial channels unless otherwise specified.
[0041] See also Figure 1 , which is a schematic diagram of the preparation process of the magnetically driven liquid metal micro-robot in the present invention. Specifically, liquid metal and polymer acid solution are provided respectively; the liquid metal is added to the acid solution, and then magnetic particles are added to obtain magnetic liquid metal; the magnetic liquid metal is added to the polymer acid solution, and after ultrasonic treatment, a magnetically driven liquid metal micro-robot is obtained. The prepared magnetically driven liquid metal micro-robot includes a liquid metal skeleton, magnetic particles and a polymer layer; wherein the magnetic particles are distributed inside the liquid metal skeleton, and the polymer layer is coated on the surface of the liquid metal skeleton.
[0042] Example 1 A method for preparing a magnetically driven liquid metal micro robot comprises the following steps: 1) Gallium and indium are heated in a mass ratio of 3:1 to form a gallium-indium alloy, and then 0.05 g of the gallium-indium alloy is weighed and dropped into 5 mL of a 1 mol / L hydrochloric acid solution to obtain a solution A; 2) Weigh 0.005 g of 100 nm iron powder, add it to solution A, and shake vigorously until the liquid metal is completely soaked in the liquid metal to obtain solution B; 3) Weigh 1 g of polyvinyl pyrrolidone with an average molecular weight of 95,000, add it to 100 mL of deionized water, stir for 12 h, add hydrochloric acid, adjust the pH value to 3, and obtain solution C. Pipette out the magnetic liquid metal in solution B with a rubber-tipped dropper, add it dropwise to solution C, ultrasonicate at 100 W ultrasonic power for 10 min, and use a magnet to screen to obtain a magnetically driven liquid metal micro robot.
[0043] After testing, the particle size distribution of the magnetically driven liquid metal micro-robot is 0.5μm-15μm.
[0044] Continuing to refer to the preparation method in Example 1, changing the ultrasonic power and time, magnetically driven liquid metal micrometer robots of different particle sizes are obtained. Specifically, at a 100W ultrasonic power, ultrasonic wave is applied for 5 minutes, and a magnetically driven liquid metal micrometer robot with a particle size distribution of 3μm-30μm can be obtained by screening with a magnet; at a 150W ultrasonic power, ultrasonic wave is applied for 10 minutes, and a magnetically driven liquid metal micrometer robot with a particle size distribution of 0.2μm-10μm can be obtained by screening with a magnet; at a 200W ultrasonic power, ultrasonic wave is applied for 10 minutes, and a magnetically driven liquid metal micrometer robot with a particle size distribution of 0.1μm-4μm can be obtained by screening with a magnet.
[0045] The magnetically driven liquid metal micro robot in this embodiment was tested by transmission electron microscopy and elemental analysis. The results are as follows: Figure 2 shown.
[0046] from Figure 2 It can be seen that the prepared magnetically driven liquid metal micro-robot has a spherical structure. Elemental analysis shows that the liquid metal containing magnetic particles has been successfully prepared.
[0047] The material prepared in this example without magnet screening was tested by scanning electron microscopy, and the results were as follows: Figure 3 shown.
[0048] from Figure 3 It can be seen that the surface of the prepared sample is very smooth and there are no iron nanoparticles on the surface.
[0049] Example 2 A method for preparing a magnetically driven liquid metal micro robot comprises the following steps: 1) Gallium and indium are heated in a mass ratio of 3:1 to form a gallium-indium alloy, and then 0.05 g of the gallium-indium alloy is weighed and dropped into 5 mL of a 1 mol / L hydrochloric acid solution to obtain a solution A; 2) Weigh 0.01 g of 100 nm iron powder, add it to solution A, and shake vigorously until the liquid metal is completely soaked in the liquid metal to obtain solution B; 3) Weigh 1 g of polyvinyl pyrrolidone with an average molecular weight of 95,000, add it to 100 mL of deionized water, stir for 12 h, add hydrochloric acid, adjust the pH value to 3, and obtain solution C. Pipette out the magnetic liquid metal in solution B with a rubber-tipped dropper, add it dropwise to solution C, ultrasonicate at 100 W ultrasonic power for 10 min, and use a magnet to screen to obtain a magnetically driven liquid metal micro robot.
[0050] After testing, the particle size distribution of the magnetically driven liquid metal micro-robot is 0.5μm-15μm.
[0051] Example 3 A method for preparing a magnetically driven liquid metal micro robot comprises the following steps: 1) Gallium and indium are heated in a mass ratio of 3:1 to form a gallium-indium alloy, and then 0.05 g of the gallium-indium alloy is weighed and dropped into 5 mL of a 1 mol / L hydrochloric acid solution to obtain a solution A; 2) Weigh 0.015 g of 100 nm iron powder, add it to solution A, and shake vigorously until the liquid metal is completely soaked in the liquid metal to obtain solution B; 3) Weigh 1 g of polyvinyl pyrrolidone with an average molecular weight of 95,000, add it to 100 mL of deionized water, stir for 12 h, add hydrochloric acid, adjust the pH value to 3, and obtain solution C. Pipette out the magnetic liquid metal in solution B with a rubber-tipped dropper, add it dropwise to solution C, ultrasonicate at 100 W ultrasonic power for 10 min, and use a magnet to screen to obtain a magnetically driven liquid metal micro robot.
[0052] After testing, the particle size distribution of the magnetically driven liquid metal micro-robot is 0.5μm-15μm.
[0053] Example 4 A method for preparing a magnetically driven liquid metal micro robot comprises the following steps: 1) Gallium and indium are heated in a mass ratio of 3:1 to form a gallium-indium alloy, and then 0.05 g of the gallium-indium alloy is weighed and dropped into 5 mL of a 2 mol / L hydrochloric acid solution to obtain a solution A; 2) Weigh 0.005 g of 1 μm iron powder, add it to solution A, and shake vigorously until the liquid metal is completely soaked in the liquid metal to obtain solution B; 3) Weigh 1 g of polyvinyl pyrrolidone with an average molecular weight of 95,000, add it to 100 mL of deionized water, stir for 12 h, add hydrochloric acid, adjust the pH value to 3, and obtain solution C. Pipette out the magnetic liquid metal in solution B with a rubber-tipped dropper, add it dropwise to solution C, ultrasonicate at 100 W ultrasonic power for 10 min, and use a magnet to screen to obtain a magnetically driven liquid metal micro robot.
[0054] After testing, the particle size distribution of the magnetically driven liquid metal micro-robot is 0.5μm-15μm.
[0055] Example 5 A method for preparing a magnetically driven liquid metal micro robot comprises the following steps: 1) Gallium and indium are heated in a mass ratio of 3:1 to form a gallium-indium alloy, and then 0.05 g of the gallium-indium alloy is weighed and dropped into 5 mL of a 1 mol / L hydrochloric acid solution to obtain a solution A; 2) Weigh 0.005 g of 100 nm iron powder, add it to solution A, and shake vigorously until the liquid metal is completely soaked in the liquid metal to obtain solution B; 3) Weigh 1 g of polyvinyl pyrrolidone with an average molecular weight of 95,000, add it to 100 mL of deionized water, stir for 12 h, add hydrochloric acid, adjust the pH value to 3, and obtain solution C. Pipette out the magnetic liquid metal in solution B with a rubber-tipped dropper, add it dropwise to solution C, ultrasonicate at 200 W ultrasonic power for 10 min, and use a magnet to screen to obtain a magnetically driven liquid metal micro robot.
[0056] After testing, the particle size distribution of the magnetically driven liquid metal micro-robot is 0.1μm-4μm.
[0057] Example 6 A method for preparing a magnetically driven liquid metal micro robot comprises the following steps: 1) Gallium and indium are heated in a mass ratio of 3:1 to form a gallium-indium alloy, and then 0.05 g of the gallium-indium alloy is weighed and dropped into 5 mL of a 1 mol / L hydrochloric acid solution to obtain a solution A; 2) Weigh 0.005 g of 100 nm ferrosoferric oxide and add it to solution A. Shake vigorously until the liquid metal is completely soaked in the liquid metal to obtain solution B. 3) Weigh 1 g of polyvinyl pyrrolidone with an average molecular weight of 95,000, add it to 100 mL of deionized water, stir for 12 h, add hydrochloric acid, adjust the pH value to 3, and obtain solution C. Pipette out the magnetic liquid metal in solution B with a rubber-tipped dropper, add it dropwise to solution C, ultrasonicate at 100 W ultrasonic power for 10 min, and use a magnet to screen to obtain a magnetically driven liquid metal micro robot.
[0058] After testing, the particle size distribution of the magnetically driven liquid metal micro-robot is 0.5μm-15μm.
[0059] Example 7 A method for preparing a magnetically driven liquid metal micro robot comprises the following steps: 1) Gallium and indium are heated in a mass ratio of 3:1 to form a gallium-indium alloy, and then 0.05 g of the gallium-indium alloy is weighed and dropped into 5 mL of a 1 mol / L hydrochloric acid solution to obtain a solution A; 2) Weigh 0.005 g of 20 nm ferrosoferric oxide and add it to solution A. Shake vigorously until the liquid metal is completely soaked in the liquid metal to obtain solution B. 3) Weigh 1 g of polyvinyl pyrrolidone with an average molecular weight of 95,000, add it to 100 mL of deionized water, stir for 12 h, add hydrochloric acid, adjust the pH value to 3, and obtain solution C. Pipette out the magnetic liquid metal in solution B with a rubber-tipped dropper, add it dropwise to solution C, ultrasonicate at 100 W ultrasonic power for 10 min, and use a magnet to screen to obtain a magnetically driven liquid metal micro robot.
[0060] After testing, the particle size distribution of the magnetically driven liquid metal micro-robot is 0.5μm-15μm.
[0061] Example 8 A method for preparing a magnetically driven liquid metal micro robot comprises the following steps: 1) Gallium: indium: tin are heated in a mass ratio of 7:2:1 to form a gallium-indium-tin alloy, and then 0.05 g of the gallium-indium-tin alloy is weighed and dropped into 5 mL of a 1 mol / L hydrochloric acid solution to obtain a solution A; 2) Weigh 0.005 g of 100 nm iron powder, add it to solution A, and shake vigorously until the liquid metal is completely soaked in the liquid metal to obtain solution B; 3) Weigh 1 g of polyvinyl pyrrolidone with an average molecular weight of 95,000, add it to 100 mL of deionized water, stir for 12 h, add hydrochloric acid, adjust the pH value to 3, and obtain solution C. Pipette out the magnetic liquid metal in solution B with a rubber-tipped dropper, add it dropwise to solution C, ultrasonicate at 150 W ultrasonic power for 10 min, and use a magnet to screen to obtain a magnetically driven liquid metal micro robot.
[0062] After testing, the particle size distribution of the magnetically driven liquid metal micro-robot is 0.2μm-10μm.
[0063] Example 9 A method for preparing a magnetically driven liquid metal micro robot comprises the following steps: 1) Gallium: indium: tin are heated in a mass ratio of 7:2:1 to form a gallium-indium-tin alloy, and then 0.05 g of the gallium-indium-tin alloy is weighed and dropped into 5 mL of a 1 mol / L hydrochloric acid solution to obtain a solution A; 2) Weigh 0.005 g of 100 nm iron powder, add it to solution A, and shake vigorously until the liquid metal is completely soaked in the liquid metal to obtain solution B; 3) Weigh 1 g of polyvinyl pyrrolidone with an average molecular weight of 95,000, add it to 100 mL of deionized water, stir for 12 h, add hydrochloric acid, adjust the pH value to 3, and obtain solution C. Pipette out the magnetic liquid metal in solution B with a rubber-tipped dropper, add it dropwise to solution C, ultrasonicate at 200 W ultrasonic power for 10 min, and use a magnet to screen to obtain a magnetically driven liquid metal micro robot.
[0064] After testing, the particle size distribution of the magnetically driven liquid metal micro-robot is 0.1μm-4μm.
[0065] Example 10 A method for preparing a magnetically driven liquid metal micro robot comprises the following steps: 1) Gallium: indium: tin are heated in a mass ratio of 7:2:1 to form a gallium-indium-tin alloy, and then 0.05 g of the gallium-indium-tin alloy is weighed and dropped into 5 mL of a 1 mol / L hydrochloric acid solution to obtain a solution A; 2) Weigh 0.005 g of 100 nm iron powder, add it to solution A, and shake vigorously until the liquid metal is completely soaked in the liquid metal to obtain solution B; 3) Weigh 1 g of polyvinyl pyrrolidone with an average molecular weight of 1300000, add it to 100 mL of deionized water, stir for 12 h, add hydrochloric acid, adjust the pH value to 3, and obtain solution C. Pipette out the magnetic liquid metal in solution B with a rubber-tipped dropper, add it dropwise to solution C, ultrasonicate at 100 W ultrasonic power for 10 min, and use a magnet to screen to obtain a magnetically driven liquid metal micro robot.
[0066] After testing, the particle size distribution of the magnetically driven liquid metal micro-robot is 0.5μm-15μm.
[0067] Embodiment 11 A method for preparing a magnetically driven liquid metal micro robot comprises the following steps: 1) Gallium: indium is heated at a mass ratio of 3:1 to form a gallium-indium-tin alloy, and then 0.05 g of the gallium-indium-tin alloy is weighed and dropped into 5 mL of a 1 mol / L hydrochloric acid solution to obtain a solution A; 2) Weigh 0.005 g of 100 nm iron powder, add it to solution A, and shake vigorously until the liquid metal is completely soaked in the liquid metal to obtain solution B; 3) Weigh 1 g of polyvinyl alcohol with an average molecular weight of 13000-23000, add it to 100 mL of deionized water, stir for 12 h, add hydrochloric acid, adjust the pH value to 3, and obtain solution C. Pipette out the magnetic liquid metal in solution B with a rubber-tipped dropper, add it dropwise to solution C, ultrasonicate at 100 W ultrasonic power for 10 min, and use a magnet to screen to obtain a magnetically driven liquid metal micro robot.
[0068] After testing, the particle size distribution of the magnetically driven liquid metal micro-robot is 0.5μm-15μm.
[0069] Example 12 A method for preparing a magnetically driven liquid metal micro robot comprises the following steps: 1) Gallium: indium is heated at a mass ratio of 3:1 to form a gallium-indium-tin alloy, and then 0.05 g of the gallium-indium-tin alloy is weighed and dropped into 5 mL of a 1 mol / L hydrochloric acid solution to obtain a solution A; 2) Weigh 0.005 g of 100 nm iron powder, add it to solution A, and shake vigorously until the liquid metal is completely soaked in the liquid metal to obtain solution B; 3) Weigh 1 g of polyethylene glycol with an average molecular weight of 4000, add it to 100 mL of deionized water, stir for 12 h, add hydrochloric acid, adjust the pH value to 3, and obtain solution C. Pipette out the magnetic liquid metal in solution B with a rubber-tipped dropper, add it dropwise to solution C, ultrasonicate at 100 W ultrasonic power for 10 min, and use a magnet to screen to obtain a magnetically driven liquid metal micro robot.
[0070] After testing, the particle size distribution of the magnetically driven liquid metal micro-robot is 0.5μm-15μm.
[0071] Comparative Example 1 The preparation method of the magnetically driven liquid metal micro-robot in this comparative example is basically the same as that in Example 1, except that solution C does not contain polyvinyl pyrrolidone but is only a hydrochloric acid aqueous solution with a pH value of 3.
[0072] The magnetically driven liquid metal micro robot prepared in this comparative example was tested by scanning electron microscopy, and the results are as follows: Figure 4 shown.
[0073] from Figure 4 It can be seen that the magnetically driven liquid metal micro-robots prepared in the comparative example are aggregated together, and it is impossible to obtain a single magnetically driven liquid metal micro-robot.
[0074] Performance Testing The magnetically driven liquid metal micro-robots with different particle sizes (4 μm, 7 μm, 10 μm, and 15 μm) prepared in Example 1 were tested for movement speed under a magnetic field strength of 10 mT and a magnetic field frequency of 5 Hz. The results are as follows: Figure 5 shown.
[0075] from Figure 5 It can be seen that as the particle size of the magnetically driven liquid metal micro-robot increases, the movement speed of the magnetically driven liquid metal micro-robot becomes faster.
[0076] The magnetically driven liquid metal micro-robots with different particle sizes (4 μm, 7 μm, 10 μm, and 15 μm) prepared in Example 1 were subjected to a motion delay test at a magnetic field strength of 10 mT and a magnetic field frequency of 5 Hz. The results are as follows: Figure 6 shown.
[0077] from Figure 6It can be seen that the larger the size of the magnetically driven liquid metal micro-robot, the faster its movement speed.
[0078] The magnetically driven liquid metal micro robot with a particle size of 15 μm prepared in Example 1 was tested to climb over an obstacle of 40 μm in height under the action of a rolling magnetic field with a magnetic field intensity of 10 mT and a magnetic field frequency of 5 Hz. The results are as follows: Figure 7 shown.
[0079] from Figure 7 It can be seen that the magnetically driven liquid metal micro-robot prepared by the present invention can climb over obstacles as high as 40 μm.
[0080] The magnetically driven liquid metal micro robot with a particle size of 15 μm prepared in Example 1 was tested to pass through a narrow channel of 10 μm under the combined action of a magnetic field strength of 10 mT, a magnetic field frequency of 5 Hz, and a simulated flow field velocity of 50 μL / min. The results are as follows: Figure 8 shown.
[0081] from Figure 8 It can be seen that the magnetically driven liquid metal micro-robot prepared by the present invention can pass through narrow channels.
[0082] The magnetically driven liquid metal micro-robots with different particle sizes (4 μm, 7 μm, 10 μm, and 15 μm) prepared in Example 1 were tested for fluorescence staining of activated nerve cells under the action of magnetic force. The results are as follows: Fig. 9 shown.
[0083] from Fig. 9 It can be seen that the magnetically driven liquid metal micro-robot prepared by the present invention can activate nerve cells.
[0084] In summary, the magnetically driven liquid metal microrobot prepared by the present invention has certain stability, controllable size, good biocompatibility, fast movement speed, controllable movement direction, and controllable movement mode. Therefore, it has broad application prospects in the field of wireless remote treatment of neurological diseases in various complex biological environments.
[0085] It should be noted that the above embodiments all belong to the same inventive concept, and the description of each embodiment has its own focus. For matters that are not described in detail in some embodiments, reference may be made to the description in other embodiments.
[0086] The above-mentioned embodiments only express the implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A magnetically driven liquid metal micro robot, It is characterized in that It includes a liquid metal skeleton, magnetic particles and a high molecular polymer layer; The magnetic particles are distributed inside the liquid metal skeleton, and the high molecular polymer layer is coated on the surface of the liquid metal skeleton.
2. The magnetically driven liquid metal micro robot according to claim 1, It is characterized in that The particle size of the magnetically driven liquid metal micro-robot is 0.1-200 μm.
3. The magnetically driven liquid metal micro robot according to claim 1, It is characterized in that The particle size of the magnetic particles is 10-1000 nm.
4. The magnetically driven liquid metal micro robot according to claim 1, It is characterized in that The liquid metal includes at least one of gallium, indium, tin and zinc.
5. The magnetically driven liquid metal micro robot according to claim 1, It is characterized in that The magnetic particles include at least one element of iron, cobalt, nickel and gadolinium.
6. The magnetically driven liquid metal micro robot according to claim 1, It is characterized in that The high molecular polymer includes at least one of polypropylene, polydopamine, polypyrrole, polyaniline, polymethyl methacrylate, polystyrene, polyamide, polyacrylonitrile, polybutylene, polyethylene oxide, polyimide, polyethylene glycol, polyvinyl pyrrolidone, polyvinyl alcohol, polyacrylic acid and polyacrylamide.
7. A method for preparing a magnetically driven liquid metal micro robot as claimed in any one of claims 1 to 6, It is characterized in that The steps include: Provide liquid metal and high molecular polymer acid solution respectively; adding the liquid metal into an acid solution, and then adding magnetic particles to obtain magnetic liquid metal; The magnetic liquid metal is added into the high molecular polymer acid solution, and after ultrasonic treatment, a magnetically driven liquid metal micro robot is obtained.
8. The preparation method according to claim 7, It is characterized in that In the provided high molecular polymer acid solution, the acid solution comprises a hydrochloric acid solution.
9. The preparation method according to claim 7, It is characterized in that In the preparation process of the magnetic liquid metal, the acid solution includes a hydrochloric acid solution.
10. Application of the magnetically driven liquid metal micro robot as claimed in any one of claims 1 to 6 in wireless remote treatment of neurological diseases.
Citation Information
Patent Citations
Magnetic control motor based on liquid metal, manufacturing method thereof and application thereof
CN105071688A
Method for preparing transformable robot through composition of shape memory alloy and liquid metal
CN105904470A
Polydimethylsiloxane / liquid metal composite material and preparation method and application thereof
CN110861119A
Liquid metal-polymer composite soft actuator and preparation method thereof
CN113043288A
High-performance thermal interface material with anisotropy and preparation method thereof
CN114539723A
Cited By
Preparation method and application of liquid metal-based magnetorheological droplet robot
CN120326588A