Composite fiber-ceramic-phenolic aerogel integrated material and preparation method thereof

By introducing a composite fiber-ceramic structure into phenolic aerogels to form a multi-layer material structure, the problem of poor ablation resistance of phenolic aerogels at high temperatures is solved, and stable heat insulation and thermal insulation in higher aerodynamic thermal environments are achieved. Anti-ablative properties.

CN118769630APending Publication Date: 2024-10-15HUBEI SANJIANG AEROSPACE GRP HONGYANG ELECTROMECHANICAL
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411125499.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The ablation resistance of phenolic aerogels deteriorates rapidly at aerodynamic thermal ambient temperatures above 1000°C, making it difficult to meet the requirements of high-speed aircraft for higher aerodynamic thermal ambient temperatures.

Method used

A composite fiber-ceramic-phenolic airgel integrated material is used, and an upper layer of the first fiber-reinforced ceramic material, a middle layer of the first fiber-reinforced composite material, and a lower layer of the second fiber-reinforced phenolic aerogel are arranged in the material. The combination of ceramics and phenolic aerogel improves the material's high-temperature ablation resistance and thermal insulation properties.

Benefits of technology

It is achieved that while maintaining light weight and good thermal insulation properties, the high-temperature ablation resistance of phenolic aerogels is significantly improved, the weight of the material is reduced, and the overall performance stability of the material is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118769630A_ABST
    Figure CN118769630A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of light heat prevention and insulation integrated materials, in particular to a composite fiber-ceramic-phenolic aerogel integrated material and a preparation method. The integrated material comprises an upper layer containing a first fiber reinforced ceramic material, a middle layer containing a first fiber reinforced composite material and a lower layer containing second fiber reinforced phenolic aerogel, the upper layer is arranged on the upper surface of the middle layer, and the lower layer is arranged on the lower surface of the middle layer; the heat-conducting property of the first fiber is higher than that of the second fiber; the raw materials of the composite material comprise ceramic and phenolic aerogel. The surface density of the middle layer is not less than the surface density of the lower layer; the high-temperature ablation resistance and the heat insulation performance of the phenolic aerogel can be effectively improved through the upper layer of the first fiber reinforced ceramic material, the middle layer of the first fiber reinforced composite material and the lower layer containing the second fiber reinforced phenolic aerogel; in addition, most of the integrated materials are light fiber materials, so that the weight of the integrated materials can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of preparation of lightweight heat-insulating integrated materials, and in particular to a composite fiber-ceramic-phenolic aerogel integrated material and a preparation method thereof. Background Art

[0002] Phenolic aerogel is a nanoporous lightweight material. It is an ideal lightweight thermal insulation integrated thermal protection material that is widely used in high-speed aircraft. Phenolic aerogel has good anti-ablation performance, good thermal insulation performance and good structural performance at aerodynamic thermal environment temperatures below 1000°C. However, with the development of high-speed aircraft, the requirements for high-speed aircraft are becoming more stringent. For example, faster flight speeds, longer flight distances and higher aerodynamic thermal environment temperatures are required at this stage. These requirements will cause high-speed aircraft to be at aerodynamic thermal environment temperatures above 1000°C. However, the anti-ablation performance of phenolic aerogel deteriorates rapidly at aerodynamic thermal environment temperatures above 1000°C.

[0003] Therefore, it is of great significance to improve the high-temperature ablation resistance of phenolic aerogel while maintaining light weight, good thermal insulation and structural properties, so as to develop a new type of lightweight ceramic-phenolic aerogel composite thermal insulation integrated material. Summary of the invention

[0004] The present application provides a composite fiber-ceramic-phenolic aerogel integrated material and a preparation method to solve the following technical problem: how to improve the high-temperature ablation resistance of phenolic aerogel.

[0005] In a first aspect, the present application provides a composite fiber-ceramic-phenolic aerogel integrated material, the integrated material comprising: an upper layer containing a first fiber-reinforced ceramic material, an intermediate layer containing a first fiber-reinforced composite material, and a lower layer containing a second fiber-reinforced phenolic aerogel; the upper layer is arranged on the upper surface of the intermediate layer, and the lower layer is arranged on the lower surface of the intermediate layer;

[0006] The thermal conductivity of the first fiber is greater than the thermal conductivity of the second fiber;

[0007] The raw materials of the composite material include ceramics and phenolic aerogel;

[0008] The surface density of the upper layer ≥ the surface density of the middle layer ≥ the surface density of the lower layer.

[0009] Optionally, the first fiber includes carbon fiber, and the second fiber includes at least one of the following:

[0010] Quartz chopped fibers, quartz wool, mullite, alkali-free fibers and aluminum silicate fiber felt.

[0011] Optionally, the raw materials of the ceramic meet the following requirements in parts by weight: silicon powder: 10 to 20 parts, carbon powder: 2 to 6 parts, aluminum oxide powder: 8 to 15 parts, zirconium carbide powder: 5 to 15 parts, water: 50 to 70 parts;

[0012] The particle size of the ceramic is 3 μm to 5 μm.

[0013] Optionally, the thickness of the integrated material is ≥15 mm;

[0014] The comprehensive density of the integrated material is less than 1g / cm 3 The surface linear ablation rate of the integrated material is less than 0.5 μm / s, and the comprehensive thermal conductivity of the integrated material is less than 0.1 W / (m·K).

[0015] In a second aspect, the present application provides a method for preparing the integrated material according to the first aspect, the method comprising:

[0016] preparing a first fiber preform;

[0017] Performing surface pretreatment on the first fiber preform in a non-oxidizing atmosphere, and then performing surface modification on the surface pretreated first fiber preform to obtain a modified first fiber preform;

[0018] Using ceramic slurry to brush and dry the coating on the modified first fiber preform to form a ceramic slurry layer on the surface of the modified first fiber preform, and then sintering the modified first fiber preform after the coating is dried to obtain a fiber layer containing a ceramic layer;

[0019] Using a second fiber preform to perform needle punching composite on the fiber layer containing the ceramic layer to obtain a composite fiber preform;

[0020] Using a phenolic resin solution to perform resin transfer molding on the composite fiber preform to perform a sol-gel reaction, and then drying the obtained sol-gel at normal pressure to obtain a composite fiber-ceramic-phenolic aerogel integrated material;

[0021] Wherein, the modifier used for the surface modification includes phenolic resin and / or furan resin;

[0022] The first fiber preform is a needle-punched felt containing first fibers;

[0023] The second fiber preform includes a fiber mat of second fibers;

[0024] The surface density of the first fiber preform is 0.3 g / cm 3 ~0.8g / cm 3 The surface density of the second fiber preform is 0.1 g / cm 3~0.3g / cm 3 .

[0025] Optionally, the surface pretreatment temperature is 1200° C. to 1600° C., and the surface pretreatment time is 0.5 h to 3 h;

[0026] The surface modification includes a modification curing stage and a modification thermal stage. The temperature of the curing stage is 90°C to 180°C, the temperature of the modification thermal stage is 1600°C to 2000°C, and the time of the modification thermal stage is 0.5h to 3h.

[0027] Optionally, the coating is dried at a temperature of 70°C to 150°C, and the coating is dried for 0.5h to 2h;

[0028] The sintering includes a heating section, a heat preservation section and a cooling section using protective gas, the terminal temperature of the heating section is 1600°C to 2000°C, the time of the heat preservation section is 1h to 5h, the temperature of the cooling section is 500°C to 800°C, and the cooling rate of the cooling section is 2°C / min to 5°C / min;

[0029] The flow rate of the protective gas is 30 mL / min to 100 mL / min.

[0030] Optionally, the heating section includes a first heating section, a second heating section and a third heating section, the terminal temperature of the first heating section is 300°C to 500°C, and the heating rate of the first heating section is 2°C / min to 5°C / min; the terminal temperature of the second heating section is 600°C to 1000°C, and the heating rate of the second heating section is 1°C / min to 3°C / min; the terminal temperature of the third heating section is 1600°C to 2000°C, and the heating rate of the third heating section is 8°C / min to 15°C / min.

[0031] Optionally, the weight m1 of the phenolic resin in the phenolic resin solution and the weight m2 of the phenolic resin solution satisfy the relationship: m1:m2=(0.1:1)-(0.5:1);

[0032] The phenolic resin solution includes a curing agent, and the added amount m3 of the curing agent and the weight m2 of the phenolic resin solution satisfy the relationship: m3:m2=(0.08:1)~(0.15:1).

[0033] Optionally, the temperature of the sol-gel reaction is 80° C. to 150° C., and the time of the sol-gel reaction is 20 h to 50 h.

[0034] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0035] An embodiment of the present application provides a composite fiber-ceramic-phenolic aerogel integrated material, the integrated material comprising: an upper layer comprising a first fiber-reinforced ceramic material, an intermediate layer comprising a first fiber-reinforced composite material, and a lower layer comprising a second fiber-reinforced phenolic aerogel; the upper layer is arranged on the upper surface of the intermediate layer, and the lower layer is arranged on the lower surface of the intermediate layer; the thermal conductivity of the first fiber is greater than the thermal conductivity of the second fiber; the raw materials of the composite material include ceramics and phenolic aerogel; the surface density of the upper layer ≥ the surface density of the intermediate layer ≥ the surface density of the lower layer. The thermal conductivity of the first fiber is generally greater than that of the second fiber, which can promote the upper layer containing the first fiber reinforced ceramic material to have good anti-ablation performance, and the lower layer containing the second fiber reinforced phenolic aerogel to have good thermal insulation performance. In addition, the surface density of the upper layer can be ≥ the surface density of the middle layer ≥ the surface density of the lower layer, which can promote the upper layer to have good density. The upper layer with good density can effectively isolate active oxygen to avoid the active oxygen from diffusing into the middle layer, thereby promoting the middle layer to have normal performance; the middle layer contains the first fiber reinforced composite material, and the raw materials of the composite material can include ceramics and phenolic aerogel to promote the middle layer to have a large number of porous structures, and the middle layer with a large number of porous structures can improve the high temperature resistance, thermal insulation performance and structural performance of the middle layer, thereby effectively improving the high temperature anti-ablation performance and thermal insulation performance of the phenolic aerogel through the upper layer of the first fiber reinforced ceramic material, the middle layer of the first fiber reinforced composite material and the lower layer containing the second fiber reinforced phenolic aerogel; in addition, most of the integrated material is lightweight fiber material, which can reduce the weight of the integrated material. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0037] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0038] Figure 1 A product schematic diagram of a composite fiber-ceramic-phenolic aerogel integrated material provided in an embodiment of the present application;

[0039] Figure 2 A schematic flow chart of a method for preparing an integrated material provided in an embodiment of the present application;

[0040] Figure 3A schematic diagram of the principle of preparing an integrated material provided in an embodiment of the present application;

[0041] Among them, 1 is a first fiber preform, 2 is a fiber layer containing a ceramic layer, 3 is a composite fiber preform, and 4 is a composite fiber-ceramic-phenolic aerogel integrated material. DETAILED DESCRIPTION

[0042] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0043] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be understood as a rigid limitation on the scope of the present application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within the range; for example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which applies regardless of the range; in addition, whenever a numerical range is indicated in this document, it is meant to include any cited numbers (fractions or integers) within the indicated range.

[0044] In this document, the terms including "including" and "including" mean "including but not limited to". Relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. "And / or" describes the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone; where A and B can be singular or plural. "At least one" means one or more, and "plurality" means two or more; "at least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single or plural items; for example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple. Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0045] Figure 1 A product schematic diagram of a composite fiber-ceramic-phenolic aerogel integrated material provided in an embodiment of the present application is exemplarily shown;

[0046] like Figure 1 As shown, the embodiment of the present application provides a composite fiber-ceramic-phenolic aerogel integrated material, the integrated material comprising: an upper layer containing a first fiber-reinforced ceramic material, an intermediate layer containing a first fiber-reinforced composite material, and a lower layer containing a second fiber-reinforced phenolic aerogel; the upper layer is arranged on the upper surface of the intermediate layer, and the lower layer is arranged on the lower surface of the intermediate layer;

[0047] The thermal conductivity of the first fiber is greater than the thermal conductivity of the second fiber;

[0048] The raw materials of the composite material include ceramics and phenolic aerogel;

[0049] The surface density of the upper layer ≥ the surface density of the middle layer ≥ the surface density of the lower layer.

[0050] It should be noted that the first fibers mainly form the upper layer in the form of needle felt, while the second fibers mainly form the lower layer in the form of fiber felt.

[0051] It should be noted that a jagged interface can be formed between the upper layer and the middle layer through various materials, and a jagged interface can be formed between the middle layer and the lower layer through various materials, thereby improving the interface bonding ability between the upper layer, the middle layer and the lower layer, thereby improving the stability of the integrated material.

[0052] In some optional embodiments, the first fiber includes carbon fiber, and the second fiber includes at least one of the following:

[0053] Quartz chopped fibers, quartz wool, mullite, alkali-free fibers and aluminum silicate fiber felt;

[0054] In these embodiments, the first fiber may include carbon fiber, which can be used to effectively improve the thermal conductivity of the upper layer. In addition, the second fiber may include at least one of: quartz chopped fiber, quartz wool, mullite, alkali-free fiber and aluminum silicate fiber felt. The second fiber can be used to promote the lower layer to have poor thermal conductivity, thereby promoting the lower layer to have good thermal insulation properties.

[0055] In some optional embodiments, the raw materials of the ceramic meet the following requirements in parts by weight: silicon powder: 10 to 20 parts, carbon powder: 2 to 6 parts, aluminum oxide powder: 8 to 15 parts, zirconium carbide powder: 5 to 15 parts, water: 50 to 70 parts;

[0056] The particle size of the ceramic is 3 μm to 5 μm;

[0057] In these optional embodiments, the raw materials of the ceramic can meet the following requirements: the weight proportion of silicon powder can be 10 to 20 parts, the weight proportion of carbon powder can be 2 to 6 parts, the weight proportion of aluminum oxide powder can be 8 to 15 parts, the weight proportion of zirconium carbide powder can be 5 to 15 parts, and the weight proportion of water can be 50 to 70 parts, which can promote the effective combination of the ceramic with the first fiber and the composite material, thereby promoting the uniform dispersion of the ceramic slurry on the first fiber or the composite material, so as to effectively improve the thermal conductivity of the upper layer and the thermal insulation and structural properties of the middle layer; in addition, the particle size of the ceramic can be 3μm to 5μm, which can promote the ceramic to be fully mixed with the first fiber and the composite material, respectively, so as to effectively improve the thermal conductivity of the upper layer and the thermal insulation and structural properties of the middle layer.

[0058] The weight proportions of the silicon powder may be 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts or 20 parts.

[0059] The weight proportion of the carbon powder can be 2 parts, 3 parts, 4 parts, 5 parts or 6 parts.

[0060] The weight proportions of the alumina powder can be 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts or 15 parts.

[0061] The weight proportions of the zirconium carbide powder can be 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts or 15 parts.

[0062] The weight parts of the water can be 50 parts, 51 parts, 52 parts, 53 parts, 54 parts, 55 parts, 56 parts, 57 parts, 58 parts, 59 parts, 60 parts, 61 parts, 62 parts, 63 parts, 64 parts, 65 parts, 66 parts, 67 parts, 68 parts, 69 parts or 70 parts.

[0063] The particle size of the ceramic may be 3 μm, 4 μm or 5 μm.

[0064] In some optional embodiments, the thickness of the integrated material is ≥15 mm;

[0065] The comprehensive density of the integrated material is less than 1g / cm 3 , the surface line ablation rate of the integrated material is less than 0.5 μm / s, and the comprehensive thermal conductivity of the integrated material is less than 0.1 W / (m·K);

[0066] In these optional embodiments, the thickness of the integrated material is generally ≥ 15 mm, and the overall density of the integrated material is generally < 1 g / cm 3 , and the surface line ablation rate of the integrated material is generally <0.5μm / s, and the comprehensive thermal conductivity of the integrated material is generally <0.1W / (m·K), which can explain that the integrated material has the advantages of light weight, good anti-ablation performance and good thermal insulation performance.

[0067] Figure 2 A schematic diagram of a method for preparing an integrated material provided in an embodiment of the present application is exemplarily shown;

[0068] Figure 3 A schematic diagram of the principle of preparing an integrated material provided in an embodiment of the present application is exemplarily shown;

[0069] Based on a general inventive concept, such as Figure 2 and Figure 3 As shown, the embodiment of the present application provides a method for preparing the integrated material, the method comprising:

[0070] S1. Preparing a first fiber preform;

[0071] S2. Pre-treating the surface of the first fiber preform in a non-oxidizing atmosphere, and then surface-modifying the surface of the pre-treated first fiber preform to obtain a modified first fiber preform;

[0072] S3. brushing the modified first fiber preform with a ceramic slurry and drying the coating to form a ceramic slurry layer on the surface of the modified first fiber preform, and then sintering the modified first fiber preform after the coating is dried to obtain a fiber layer containing a ceramic layer;

[0073] S4. Using a second fiber preform to perform needle punching on the fiber layer containing the ceramic layer to obtain a composite fiber preform;

[0074] S5. Using a phenolic resin solution to perform resin transfer molding on the composite fiber preform to perform a sol-gel reaction, and then drying the obtained sol-gel at normal pressure to obtain a composite fiber-ceramic-phenolic aerogel integrated material;

[0075] Wherein, the modifier used for the surface modification includes phenolic resin and / or furan resin;

[0076] The first fiber preform is a needle-punched felt containing first fibers;

[0077] The second fiber preform includes a fiber mat of second fibers;

[0078] The surface density of the first fiber preform is 0.3 g / cm 3 ~0.8g / cm 3 The surface density of the second fiber preform is 0.1 g / cm 3 ~0.3g / cm 3 .

[0079] This method is a method for preparing the above-mentioned integrated material. The specific composition and composition information of the integrated material can refer to the above-mentioned embodiment. Since this method adopts part or all of the technical solutions of the above-mentioned embodiment, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiment, which will not be described one by one here.

[0080] It should be noted that the modifier used for the surface modification may include phenolic resin and / or furan resin, which can modify the surface of the first fiber preform into oleophilic and hydrophilic properties in a non-oxidizing atmosphere, thereby facilitating the subsequent brushing of the ceramic slurry on the surface of the modified first fiber preform to obtain a uniformly distributed ceramic slurry layer.

[0081] It should be noted that the surface density of the first fiber preform can be 0.3 g / cm 3 ~0.8g / cm 3 , and the surface density of the second fiber preform may be 0.1 g / cm 3 ~0.3g / cm 3, which can enable the first fiber preform and the second fiber preform to have sufficient pore structure to accommodate the ceramic slurry and the phenolic resin solution. Sufficient ceramic slurry and phenolic resin solution can, on the one hand, obtain an integrated material of the upper layer, the middle layer and the lower layer, and on the other hand, improve the high-temperature ablation resistance and thermal insulation performance of the integrated material.

[0082] The surface density of the first fiber preform may be 0.3 g / cm 3 , 0.4g / cm 3 , 0.5g / cm 3 , 0.6g / cm 3 or 0.8g / cm 3 .

[0083] The surface density of the second fiber preform may be 0.1 g / cm 3 , 0.2g / cm 3 or 0.3g / cm 3 .

[0084] It should be noted that the brushing can be performed in a single-layer brushing manner or in a gradient brushing manner to obtain multiple layers of ceramic material with different distribution degrees.

[0085] It should be noted that the non-oxidizing atmosphere may be a vacuum atmosphere or an argon atmosphere.

[0086] It should be noted that the coating drying is carried out entirely in a drying oven, while the atmospheric pressure drying is carried out in stages. Specifically, atmospheric pressure drying can be divided into natural atmospheric pressure drying and oven atmospheric pressure drying. The time of the natural atmospheric pressure drying can be 48h to 96h, the temperature of the oven atmospheric pressure drying can be 40℃ to 90℃, and the time of the oven atmospheric pressure drying can be 12h to 48h.

[0087] In some optional embodiments, the surface pretreatment temperature is 1200° C. to 1600° C., and the surface pretreatment time is 0.5 h to 3 h;

[0088] The surface modification includes a modification curing stage and a modification thermal stage, the temperature of the curing stage is 90°C to 180°C, the temperature of the modification thermal stage is 1600°C to 2000°C, and the time of the modification thermal stage is 0.5h to 3h;

[0089] In these embodiments, the surface pretreatment temperature can be 1200°C to 1600°C, and the surface pretreatment time can be 0.5h to 3h, which can effectively heat the first fiber preform to facilitate the subsequent surface modification; in addition, the surface modification can include a modification curing stage and a modification thermal stage, and the temperature of the curing stage can be 90°C to 180°C, and the temperature of the modification thermal stage can be 1600°C to 2000°C, and the time of the modification thermal stage can be 0.5h to 3h, which can promote the modifier to effectively modify the first fiber of the first fiber preform to promote complete modification of the first fiber preform.

[0090] The temperature of the surface pretreatment may be 1200°C, 1250°C, 1300°C, 1350°C, 1400°C, 1450°C, 1500°C, 1550°C or 1600°C.

[0091] The surface pretreatment time can be 0.5 h, 1.0 h, 1.5 h, 2.0 h, 2.5 h or 3.0 h.

[0092] The temperature of the curing stage may be 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C or 180°C.

[0093] The temperature of the modification thermal stage may be 1600°C, 1650°C, 1700°C, 1750°C, 1800°C, 1850°C, 1900°C, 1950°C or 2000°C.

[0094] The time of the modification thermal stage can be 0.5 h, 1.0 h, 1.5 h, 2.0 h, 2.5 h or 3.0 h.

[0095] In some optional embodiments, the coating is dried at a temperature of 70°C to 150°C, and the coating is dried for 0.5h to 2h;

[0096] The sintering includes a heating section, a heat preservation section and a cooling section using protective gas, the terminal temperature of the heating section is 1600°C to 2000°C, the time of the heat preservation section is 1h to 5h, the temperature of the cooling section is 500°C to 800°C, and the cooling rate of the cooling section is 2°C / min to 5°C / min;

[0097] The flow rate of the protective gas is 30 mL / min to 100 mL / min;

[0098] In these embodiments, the coating drying temperature can be 70°C to 150°C, and the coating drying time can be 0.5h to 2h, which can effectively remove moisture from the ceramic material after brushing, so as to facilitate subsequent sintering to obtain a dense ceramic layer structure; in addition, the sintering can include a heating section, a heat preservation section and a cooling section using a protective gas, and the terminal temperature of the heating section can be 1600°C to 2000°C, and the time of the heat preservation section can be 1h to 5h, and the temperature of the cooling section can be 500°C to 800°C, and the cooling rate of the cooling section can be 2°C / min to 5°C / min, which can enable the ceramic material to form a dense ceramic layer during the sintering process and avoid defects in the ceramic layer caused by temperature fluctuations; in addition, the flow rate of the protective gas can be 30mL / min to 100mL / min, which can effectively promote the overall sintering in an air-isolated environment to avoid oxygen and nitrogen in the air affecting the molding of the ceramic layer.

[0099] The coating may be dried at a temperature of 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C.

[0100] The coating can be dried for 0.5 h, 1.0 h, 1.5 h or 2.0 h.

[0101] The terminal temperature of the temperature rising section may be 1600°C, 1650°C, 1700°C, 1750°C, 1800°C, 1850°C, 1900°C, 1950°C or 2000°C.

[0102] The insulation period can be 1.0h, 1.5h, 2.0h, 2.5h, 3.0h, 3.5h, 4.0h, 4.5h or 5.0h.

[0103] The temperature of the temperature reduction section may be 500°C, 550°C, 600°C, 650°C, 700°C, 750°C or 800°C.

[0104] The cooling rate of the cooling section can be 2°C / min, 2.5°C / min, 3.0°C / min, 3.5°C / min, 4.0°C / min, 4.5°C / min or 5.0°C / min.

[0105] The flow rate of the shielding gas may be 30 mL / min, 40 mL / min, 50 mL / min, 60 mL / min, 70 mL / min, 80 mL / min, 90 mL / min or 100 mL / min.

[0106] It should be noted that the protective gas can be a high-purity inert gas, such as argon.

[0107] In some optional embodiments, the heating section includes a first heating section, a second heating section and a third heating section, the terminal temperature of the first heating section is 300°C to 500°C, and the heating rate of the first heating section is 2°C / min to 5°C / min; the terminal temperature of the second heating section is 600°C to 1000°C, and the heating rate of the second heating section is 1°C / min to 3°C / min; the terminal temperature of the third heating section is 1600°C to 2000°C, and the heating rate of the third heating section is 8°C / min to 15°C / min;

[0108] In these embodiments, the heating section may include a first heating section, a second heating section and a third heating section, and the terminal temperature of the first heating section may be 300°C to 500°C, and the heating rate of the first heating section may be 2°C / min to 5°C / min, and the terminal temperature of the second heating section may be 600°C to 1000°C, and the heating rate of the second heating section may be 1°C / min to 3°C / min, and the terminal temperature of the third heating section may be 1600°C to 2000°C, and the heating rate of the third heating section may be 8°C / min to 15°C / min, and the ceramic material may be effectively combined with the surface of the modified first fiber preform in the heating section to sinter to form a ceramic layer on the surface of the modified first fiber preform.

[0109] The terminal temperature of the first temperature rising section may be 300°C, 350°C, 400°C, 450°C or 500°C.

[0110] The heating rate of the first heating stage may be 2°C / min, 3°C / min, 4°C / min or 5°C / min.

[0111] The terminal temperature of the second temperature rising section may be 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C or 1000°C.

[0112] The heating rate of the second heating stage may be 1°C / min, 2°C / min or 3°C / min.

[0113] The terminal temperature of the third temperature rising section may be 1600°C, 1650°C, 1700°C, 1750°C, 1800°C, 1850°C, 1900°C, 1950°C or 2000°C.

[0114] The heating rate of the third heating section may be 8°C / min, 9°C / min, 10°C / min, 11°C / min, 12°C / min, 13°C / min, 14°C / min or 15°C / min.

[0115] In some optional embodiments, the weight m1 of the phenolic resin in the phenolic resin solution and the weight m2 of the phenolic resin solution satisfy the relationship: m1:m2=(0.1:1)-(0.5:1);

[0116] The phenolic resin solution includes a curing agent, and the added amount m3 of the curing agent and the weight m2 of the phenolic resin solution satisfy the relationship: m3:m2=(0.08:1)~(0.15:1).

[0117] In these embodiments, the weight m1 of the phenolic resin in the phenolic resin solution and the weight m2 of the phenolic resin solution can satisfy the relationship: m1:m2=(0.1:1)~(0.5:1), which can promote the presence of a sufficient amount of phenolic acid resin in the phenolic resin solution, and the sufficient amount of phenolic resin can form a sufficient amount of phenolic gel in the sol-gel reaction process, and the sufficient amount of phenolic gel can promote the formation of the middle layer and the lower layer; in addition, the phenolic resin solution can include a curing agent, and the added amount m3 of the curing agent and the weight m2 of the phenolic resin solution can satisfy the relationship: m3:m2=(0.08:1)~(0.15:1); which can promote the phenolic resin solution to have a sufficient amount of curing agent, and the sufficient amount of curing agent can promote the rapid formation of the phenolic resin, so as to promote the formation of the middle layer and the lower layer.

[0118] The weight m1 of the phenolic resin in the phenolic resin solution and the weight m2 of the phenolic resin solution may satisfy the relationship: m1:m2=0.1:1, 0.2:1, 0.3:1, 0.4:1 or 0.5:1.

[0119] The added amount m3 of the curing agent and the weight m2 of the phenolic resin solution can satisfy the relationship: m3:m2=0.08:1, 0.09:1, 0.10:1, 0.11, 0.12:1, 0.13:1, 0.14:1 or 0.15:1.

[0120] In some optional embodiments, the temperature of the sol-gel reaction is 80° C. to 150° C., and the time of the sol-gel reaction is 20 h to 50 h;

[0121] In these embodiments, the sol-gel reaction temperature may be 80° C. to 150° C., and the sol-gel reaction time may be 20 h to 50 h, which may enable the phenolic resin solution to form an intermediate layer and a lower layer on the surface of the composite fiber preform.

[0122] The temperature of the sol-gel reaction may be 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C.

[0123] The sol-gel reaction time can be 20 h, 25 h, 30 h, 35 h, 40 h, 45 h or 50 h.

[0124] It should be noted that the phenolic resin solution is a low-density phenolic resin solution, and the solvent used in the phenolic resin solution may include at least one of the following:

[0125] Ethanol, isopropanol and ethylene glycol; the phenolic resin solution can use hexamethylenetetramine as a curing agent.

[0126] It should be noted that, in the resin transfer molding process, the sealed mold cavity needs to be evacuated to below 0.01 MPa first, and then the phenolic resin solution is added, and the injection pressure can be 0.05 MPa to 0.3 MPa.

[0127] The present application is further described below in conjunction with specific examples. The experimental methods in the following examples that do not specify specific conditions are usually measured according to industry standards; if there are no corresponding industry standards, they are carried out according to common international standards, conventional conditions, or conditions recommended by the manufacturer.

[0128] Example 1

[0129] like Figure 1 As shown, a composite fiber-ceramic-phenolic aerogel integrated material comprises: an upper layer containing a first fiber-reinforced ceramic material, an intermediate layer containing a first fiber-reinforced composite material, and a lower layer containing a second fiber-reinforced phenolic aerogel; the upper layer is arranged on the upper surface of the intermediate layer, and the lower layer is arranged on the lower surface of the intermediate layer;

[0130] The thermal conductivity of the first fiber is greater than the thermal conductivity of the second fiber;

[0131] The raw materials of the composite materials include ceramics and phenolic aerogels;

[0132] The surface density of the upper layer ≥ the surface density of the middle layer ≥ the surface density of the lower layer.

[0133] The first fiber is a carbon chopped fiber, and the second fiber is a mullite fiber.

[0134] In terms of weight, the raw materials of the ceramics meet the following requirements: silicon powder: 20 parts, carbon powder: 5 parts, aluminum oxide powder: 8 parts, zirconium carbide powder: 10 parts, water: 57 parts;

[0135] The particle size of the ceramic is 3 μm to 5 μm.

[0136] like Figure 2 and Figure 3 As shown, a method for preparing an integrated material comprises:

[0137] S1. Preparing a first fiber preform of 10 mm;

[0138] S2. The first fiber preform is subjected to surface pretreatment in a non-oxidizing atmosphere, and then the surface of the first fiber preform subjected to surface pretreatment is modified to obtain a modified first fiber preform;

[0139] S3. brushing and drying the modified first fiber preform with a ceramic slurry, repeating the process 3 times to form a ceramic slurry layer on the surface of the modified first fiber preform, and then sintering the modified first fiber preform after drying the coating to obtain a fiber layer containing a ceramic layer;

[0140] S4. Using a 20 mm second fiber preform, the non-ceramic surface of the fiber layer containing the ceramic layer is needle-punched to obtain a composite fiber preform;

[0141] S5. The composite fiber preform was subjected to resin transfer molding using a phenolic resin solution, the injection pressure of the phenolic resin solution was 0.1 MPa, to carry out a sol-gel reaction, and then the obtained sol-gel was dried at normal pressure to obtain a composite fiber - ceramic - phenolic aerogel integrated material;

[0142] Wherein, the modifier used for surface modification includes liquid furan resin;

[0143] The first fiber preform is a needle-punched felt containing first fibers;

[0144] The second fiber preform includes a fiber mat of second fibers;

[0145] The surface density of the first fiber preform is 0.6 g / cm 3 The surface density of the second fiber preform is 0.15 g / cm 3 .

[0146] The surface pretreatment temperature is 1600°C and the surface pretreatment time is 2h;

[0147] The surface modification includes a modification curing stage and a modification thermal stage. The temperature of the curing stage is 100°C, the temperature of the modification thermal stage is 1600°C, and the time of the modification thermal stage is 2.0h.

[0148] The coating drying temperature is 100°C and the coating drying time is 2h;

[0149] The sintering process includes a heating section, a holding section and a cooling section using high-purity argon as a protective gas. The terminal temperature of the heating section is 1800°C, the holding time is 2 hours, the temperature of the cooling section is 500°C, and the cooling rate of the cooling section is 5°C / min.

[0150] The flow rate of the protective gas was 60 mL / min.

[0151] The heating section includes a first heating section, a second heating section and a third heating section. The terminal temperature of the first heating section is 300°C, and the heating rate of the first heating section is 5°C / min; the terminal temperature of the second heating section is 700°C, and the heating rate of the second heating section is 2°C / min; the terminal temperature of the third heating section is 1800°C, and the heating rate of the third heating section is 15°C / min.

[0152] The weight m1 of the phenolic resin in the phenolic resin solution and the weight m2 of the phenolic resin solution satisfy the relationship: m1:m2=0.3:1; the solvent used in the phenolic resin solution is a mixture of ethylene glycol and ethanol, and the curing agent used in the phenolic resin solution is hexamethylenetetramine;

[0153] The amount of curing agent added m3 and the weight of the phenolic resin solution m2 satisfy the relationship: m3:m2=0.15:1;

[0154] The temperature of the sol-gel reaction is 120°C, and the time of the sol-gel reaction is 24h.

[0155] Normal pressure drying is divided into natural drying section and blast drying section. The time of natural drying section is 72h, the temperature of blast drying section is 50℃, and the time of blast drying is 48h.

[0156] Example 2

[0157] Based on the contents disclosed in Example 1, the following modifications are further made:

[0158] The thickness of the second fiber preform was 25 mm.

[0159] The brushing and coating drying were repeated 5 times.

[0160] The filling pressure of the phenolic resin solution is 0.2Mpa.

[0161] The first fiber is carbon chopped fiber, and the second fiber is composite fiber of quartz chopped fiber and quartz wool.

[0162] In terms of weight, the raw materials of the ceramics meet the following requirements: silicon powder: 12 parts, carbon powder: 3 parts, aluminum oxide powder: 10 parts, zirconium carbide powder: 5 parts, water: 70 parts;

[0163] The modifiers used for surface modification include liquid phenolic resin;

[0164] The surface density of the first fiber preform is 0.8 g / cm 3 The surface density of the second fiber preform is 0.12 g / cm 3 .

[0165] The surface pretreatment temperature was 1600°C and the surface pretreatment time was 1 h;

[0166] The surface modification includes a modification curing stage and a modification thermal stage. The temperature of the curing stage is 150°C, the temperature of the modification thermal stage is 1800°C, and the time of the modification thermal stage is 1.0h.

[0167] The coating drying temperature is 140°C and the coating drying time is 1h;

[0168] The sintering process includes a heating section, a holding section and a cooling section using high-purity argon as the protective gas. The terminal temperature of the heating section is 2000°C, the holding time is 1 hour, the temperature of the cooling section is 800°C, and the cooling rate of the cooling section is 2°C / min.

[0169] The flow rate of the protective gas was 80 mL / min.

[0170] The heating section includes a first heating section, a second heating section and a third heating section. The terminal temperature of the first heating section is 500°C, and the heating rate of the first heating section is 3°C / min; the terminal temperature of the second heating section is 900°C, and the heating rate of the second heating section is 1°C / min; the terminal temperature of the third heating section is 2000°C, and the heating rate of the third heating section is 10°C / min.

[0171] The weight m1 of the phenolic resin in the phenolic resin solution and the weight m2 of the phenolic resin solution satisfy the relationship: m1:m2=0.45:1;

[0172] The amount of curing agent added m3 and the weight of the phenolic resin solution m2 satisfy the relationship: m3:m2=0.10:1;

[0173] The temperature of the sol-gel reaction is 100°C, and the time of the sol-gel reaction is 48h.

[0174] Normal pressure drying is divided into natural drying section and blast drying section. The time of natural drying section is 96 hours, the temperature of blast drying section is 80℃, and the time of blast drying is 24 hours.

[0175] Example 3

[0176] Based on the contents disclosed in Example 1, the following modifications are further made:

[0177] The thickness of the first fiber preform is 15 mm;

[0178] The thickness of the second fiber preform was 15 mm.

[0179] The filling pressure of the phenolic resin solution is 0.15Mpa.

[0180] The first fibers are carbon chopped fibers, and the second fibers are aluminum silicate fibers.

[0181] In terms of weight, the raw materials of the ceramics meet the following requirements: silicon powder: 15 parts, carbon powder: 4 parts, aluminum oxide powder: 10 parts, zirconium carbide powder: 10 parts, water: 61 parts;

[0182] The modifier used for surface modification includes liquid furan resin;

[0183] The surface density of the first fiber preform is 0.45 g / cm 3 The surface density of the second fiber preform is 0.12 g / cm 3 .

[0184] The surface pretreatment temperature is 1200°C and the surface pretreatment time is 2h;

[0185] The surface modification includes a modification curing stage and a modification thermal stage. The temperature of the curing stage is 120°C, the temperature of the modification thermal stage is 1800°C, and the time of the modification thermal stage is 2.0h.

[0186] The coating drying temperature is 80°C and the coating drying time is 2h;

[0187] The sintering process includes a heating stage, a heat preservation stage and a cooling stage using high-purity argon as a protective gas. The terminal temperature of the heating stage is 1800°C, the time of the heat preservation stage is 3 hours, the temperature of the cooling stage is 800°C, and the cooling rate of the cooling stage is 3°C / min.

[0188] The flow rate of the protective gas was 50 mL / min.

[0189] The heating section includes a first heating section, a second heating section and a third heating section. The terminal temperature of the first heating section is 500°C, and the heating rate of the first heating section is 3°C / min; the terminal temperature of the second heating section is 800°C, and the heating rate of the second heating section is 2°C / min; the terminal temperature of the third heating section is 1800°C, and the heating rate of the third heating section is 10°C / min.

[0190] The weight m1 of the phenolic resin in the phenolic resin solution and the weight m2 of the phenolic resin solution satisfy the relationship: m1:m2=0.30:1; the solvent used in the phenolic resin solution is a mixture of ethylene glycol and ethanol.

[0191] The amount of curing agent added m3 and the weight of the phenolic resin solution m2 satisfy the relationship: m3:m2=0.15:1;

[0192] The temperature of the sol-gel reaction is 80°C, and the time of the sol-gel reaction is 48h.

[0193] Normal pressure drying is divided into natural drying section and blast drying section. The time of natural drying section is 60 hours, the temperature of blast drying section is 80℃, and the time of blast drying is 48 hours.

[0194] Comparative Example 1

[0195] Based on the contents disclosed in Example 1, the following modifications are further made:

[0196] No ceramic material is added, so that no ceramic layer is compounded.

[0197] Comparative Example 2

[0198] Based on the contents disclosed in Example 1, the following modifications are further made:

[0199] No second fiber preform was used.

[0200] Related experiments and effect data:

[0201] The properties of the integrated materials obtained in each embodiment and comparative example were statistically analyzed, and the results are shown in Table 1.

[0202] Table 1 Performance of the integrated materials obtained in various embodiments and comparative examples

[0203]

[0204]

[0205] As can be seen from Table 1, a composite fiber-ceramic-phenolic aerogel integrated material provided in an embodiment of the present application can effectively improve the high-temperature ablation resistance and thermal insulation performance of the phenolic aerogel through an upper layer of a first fiber-reinforced ceramic material, an intermediate layer of a first fiber-reinforced composite material, and a lower layer containing a second fiber-reinforced phenolic aerogel; in addition, the integrated material uses mostly lightweight fiber materials, which can reduce the weight of the integrated material.

[0206] In addition, the composite fiber-ceramic-phenolic aerogel integrated material provided in the embodiment of the present application has the advantages of light weight (comprehensive density of the sample is less than 1g / cm 3 ), good ablation resistance (surface linear ablation rate of the sample <0.5μm / s) and good thermal insulation performance (comprehensive thermal conductivity of the sample <0.1W / (m·K), making it an ideal integrated material with ablation resistance and high thermal insulation.

[0207] The above is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. It will be apparent to those skilled in the art that various modifications to these embodiments are possible, and the general principles defined in the present application can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to these embodiments shown in the present application, but will conform to the widest scope consistent with the principles and novel features applied for by the present application.

Claims

1. A composite fiber-ceramic-phenolic aerogel integrated material, characterized in that: The integrated material comprises: an upper layer containing a first fiber-reinforced ceramic material, an intermediate layer containing a first fiber-reinforced composite material, and a lower layer containing a second fiber-reinforced phenolic aerogel; the upper layer is arranged on the upper surface of the intermediate layer, and the lower layer is arranged on the lower surface of the intermediate layer; Wherein, the thermal conductivity of the first fiber is greater than the thermal conductivity of the second fiber; The raw materials of the composite material include ceramics and phenolic aerogel; The surface density of the upper layer ≥ the surface density of the middle layer ≥ the surface density of the lower layer.

2. The integrated material according to claim 1, characterized in that: The first fiber comprises carbon fiber, and the second fiber comprises at least one of the following: Quartz chopped fibers, quartz wool, mullite, alkali-free fibers and aluminum silicate fiber felt.

3. The integrated material according to claim 1, characterized in that: In parts by weight, the raw materials of the ceramic meet the following requirements: silicon powder: 10 to 20 parts, carbon powder: 2 to 6 parts, aluminum oxide powder: 8 to 15 parts, zirconium carbide powder: 5 to 15 parts, water: 50 to 70 parts; The particle size of the ceramic is 3 μm to 5 μm.

4. The integrated material according to claim 1, characterized in that: The thickness of the integrated material is ≥15mm; The comprehensive density of the integrated material is less than 1g / cm 3 The surface linear ablation rate of the integrated material is less than 0.5 μm / s, and the comprehensive thermal conductivity of the integrated material is less than 0.1 W / (m·K).

5. A method for preparing the integrated material according to any one of claims 1 to 4, characterized in that: The method comprises: preparing a first fiber preform; Performing surface pretreatment on the first fiber preform in a non-oxidizing atmosphere, and then performing surface modification on the surface pretreated first fiber preform to obtain a modified first fiber preform; Using ceramic slurry to brush and dry the coating on the modified first fiber preform to form a ceramic slurry layer on the surface of the modified first fiber preform, and then sintering the modified first fiber preform after the coating is dried to obtain a fiber layer containing a ceramic layer; Using a second fiber preform to perform needle punching composite on the fiber layer containing the ceramic layer to obtain a composite fiber preform; Using a phenolic resin solution to perform resin transfer molding on the composite fiber preform to perform a sol-gel reaction, and then drying the obtained sol-gel at normal pressure to obtain a composite fiber-ceramic-phenolic aerogel integrated material; Wherein, the modifier used for the surface modification includes phenolic resin and / or furan resin; The first fiber preform is a needle-punched felt containing first fibers; The second fiber preform includes a fiber mat of second fibers; The surface density of the first fiber preform is 0.3 g / cm 3 ~0.8g / cm 3 The surface density of the second fiber preform is 0.1 g / cm 3 ~0.3g / cm 3 .

6. The preparation method according to claim 5, characterized in that: The surface pretreatment temperature is 1200°C to 1600°C, and the surface pretreatment time is 0.5h to 3h; The surface modification includes a modification curing stage and a modification thermal stage. The temperature of the curing stage is 90°C to 180°C, the temperature of the modification thermal stage is 1600°C to 2000°C, and the time of the modification thermal stage is 0.5h to 3h.

7. The preparation method according to claim 5, characterized in that: The coating is dried at a temperature of 70°C to 150°C, and the coating is dried for 0.5h to 2h; The sintering includes a heating section, a heat preservation section and a cooling section using protective gas, the terminal temperature of the heating section is 1600°C to 2000°C, the time of the heat preservation section is 1h to 5h, the temperature of the cooling section is 500°C to 800°C, and the cooling rate of the cooling section is 2°C / min to 5°C / min; The flow rate of the protective gas is 30 mL / min to 100 mL / min.

8. The preparation method according to claim 7, characterized in that: The heating section includes a first heating section, a second heating section and a third heating section. The terminal temperature of the first heating section is 300°C to 500°C, and the heating rate of the first heating section is 2°C / min to 5°C / min; the terminal temperature of the second heating section is 600°C to 1000°C, and the heating rate of the second heating section is 1°C / min to 3°C / min; the terminal temperature of the third heating section is 1600°C to 2000°C, and the heating rate of the third heating section is 8°C / min to 15°C / min.

9. The preparation method according to claim 5, characterized in that: The weight m1 of the phenolic resin in the phenolic resin solution and the weight m2 of the phenolic resin solution satisfy the relationship: m1:m2=(0.1:1)-(0.5:1); The phenolic resin solution includes a curing agent, and the added amount m3 of the curing agent and the weight m2 of the phenolic resin solution satisfy the relationship: m3:m2=(0.08:1)~(0.15:1).

10. The preparation method according to claim 5, characterized in that: The temperature of the sol-gel reaction is 80° C. to 150° C., and the time of the sol-gel reaction is 20 h to 50 h.

Citation Information

Patent Citations

  • Carbon based enhanced ablation-resistant phenolic aerogel material and preparation method thereof

    CN110981524A

  • Surface anti-scouring low-density ablation heat-proof material and preparation method thereof

    CN112538233A

  • Flexible phenolic aldehyde / silicon composite aerogel ablation thermal protection composite material and preparation method thereof

    CN117756445A