Preparation method of lithium iron phosphate material, positive plate and battery

By adding metal powder to the lithium iron phosphate precursor and performing a sintering process, its heat shrinkage properties are used to tightly shrink the lithium iron phosphate particles, which solves the problem of insufficient compaction density of the lithium iron phosphate cathode material and achieves density improvement and process simplification. .

CN118771333AActive Publication Date: 2024-10-15XTC NEW ENERGY MATERIALS(XIAMEN) LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310372742.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-15
Estimated Expiration
2043-04-10

AI Technical Summary

Technical Problem

The volumetric energy density of lithium iron phosphate cathode materials is not high. The existing methods to increase the compaction density are cumbersome and have limited effects, and the material properties deteriorate.

Method used

Metal powder (such as antimony powder or bismuth powder) is added to the lithium iron phosphate precursor, and through uniform mixing and sintering, the heat shrinkage properties of the metal powder are used to cause the lithium iron phosphate particles to shrink tightly and increase the compaction density.

Benefits of technology

The compacted density of lithium iron phosphate material is increased to 2.7g/cm3, which simplifies the preparation process and avoids the need to increase the particle size or reduce the amount of carbon coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118771333A_ABST
    Figure CN118771333A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a lithium iron phosphate material, which comprises the following steps: metal powder is added into a lithium iron phosphate precursor, the metal powder comprises at least one of antimony powder or bismuth powder, and after uniform mixing, a sintered precursor is obtained; sintering the sintering precursor; and naturally cooling the sintered precursor to room temperature, and crushing to obtain the powdery lithium iron phosphate material. The preparation method provided by the invention is simple in process, and the compaction density of the lithium iron phosphate can be improved. The invention also provides a positive plate comprising the lithium iron phosphate and a battery comprising the positive plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of lithium iron phosphate materials, and specifically to a preparation method of lithium iron phosphate materials, a positive electrode sheet and a battery. Background Art

[0002] Compared with other lithium-ion battery cathode materials, lithium iron phosphate batteries have more advantages in comprehensive indicators such as safety, cycle life, and production cost. At present, lithium iron phosphate batteries have been widely used in many fields including electric vehicles, automobiles, ships, and energy storage, becoming one of the most developed power batteries at this stage. However, the low volume energy density limits the application of lithium iron phosphate cathode materials, and the key to volume energy density lies in increasing the compaction density.

[0003] In the prior art, the methods for increasing the compaction density of lithium iron phosphate materials include: increasing the particle size of lithium iron phosphate materials and reducing the amount of carbon coating on the surface of lithium iron phosphate. However, increasing the particle size of the material will cause its capacity to decrease and its rate performance to deteriorate; reducing the amount of carbon coating on the particle surface will cause the material to easily agglomerate. Moreover, the above method is cumbersome. Summary of the invention

[0004] In view of this, the present application provides a preparation method capable of improving the compaction density of lithium iron phosphate material, and the method has a simple process.

[0005] The present application provides a method for preparing a lithium iron phosphate material, comprising the following steps:

[0006] Adding metal powder to a lithium iron phosphate precursor, wherein the metal powder includes at least one of antimony powder and bismuth powder, and mixing them uniformly to obtain a sintered precursor;

[0007] sintering the sintering precursor;

[0008] The sintered precursor is naturally cooled to room temperature and crushed to obtain a powdery lithium iron phosphate material.

[0009] Optionally, the sintering comprises the following steps:

[0010] The process is sintered at 250-650°C for 2-4 hours, and then heated to 750-800°C for 8-12 hours, with a heating rate of 2-5°C / min. The sintering is carried out under vacuum conditions or in a protective atmosphere with a flow rate of 10-40 L / min, wherein the oxygen content in the protective atmosphere is below 50 ppm.

[0011] Optionally, the mass of the metal powder is 3-10% of the mass of the lithium iron phosphate precursor.

[0012] Optionally, the particle size of the lithium iron phosphate precursor is 0.3-2 μm.

[0013] Optionally, the particle size of the metal powder is less than 20 μm.

[0014] Optionally, the lithium iron phosphate precursor includes a lithium source, an iron source and a carbon source, the molar ratio of the lithium source to the iron source is 0.96-1.04, the mass of the carbon source is 5-15% of the total mass of the lithium source and the iron source, and the iron source or the lithium source includes phosphate.

[0015] Optionally, the preparation of the lithium iron phosphate precursor includes:

[0016] Mixing the lithium source, the iron source and the carbon source according to a stoichiometric ratio, and adding deionized water to obtain a mixture;

[0017] The mixture was wet ball milled and dried.

[0018] The present application also provides a positive electrode sheet, comprising a positive electrode material, wherein the positive electrode material comprises the lithium iron phosphate material obtained by the preparation method of the lithium iron phosphate material.

[0019] The present application also provides a battery, which includes the positive electrode sheet.

[0020] Compared with the prior art, the present application uniformly mixes antimony powder or bismuth powder in the lithium iron phosphate precursor, so that the antimony powder or bismuth powder is evenly dispersed in the particle gaps of the lithium iron phosphate precursor. Since antimony powder or bismuth powder has the special property of thermal shrinkage, as the temperature rises, the crystal structure and atomic arrangement will change, and the atomic arrangement will be tighter, resulting in a reduction in volume. In the step of sintering to form lithium iron phosphate, the antimony powder or bismuth powder will drive the lithium iron phosphate precursor particles to shrink tightly together, reducing the distance between the particles of the lithium iron phosphate precursor, thereby being able to at least increase the compaction density of the lithium iron phosphate material to 2.7g / cm 3 In addition, the present application only shrinks the lithium iron phosphate precursor, and there is no need to increase the size of the lithium iron phosphate particles or reduce the amount of carbon coating on the particle surface, which is conducive to simplifying the process of preparing lithium iron phosphate. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 A flow chart for preparing lithium iron phosphate provided in this application;

[0022] Figure 2 This is a SEM image of the lithium iron phosphate material provided in Example 1 of the present application. DETAILED DESCRIPTION

[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0025] Some embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0026] Reference Figure 1 The present application provides a method for preparing lithium iron phosphate, the preparation method comprising the following steps:

[0027] Step S101, adding metal powder to lithium iron phosphate precursor particles, wherein the metal powder includes at least one of antimony powder and bismuth powder, and mixing them evenly to obtain a sintered precursor. A high-speed mixer can be used to mix the metal powder to obtain the sintered precursor.

[0028] In some embodiments, the lithium iron phosphate precursor particles include a lithium source, an iron source and a carbon source, the molar ratio of the lithium source to the iron source is 0.96-1.04, and the mass of the carbon source is 5-15% of the total mass of the lithium source and the iron source. The lithium source or the iron source includes a phosphate radical. The lithium source may include at least one of lithium carbonate, lithium hydroxide, lithium chloride, lithium sulfate, lithium acetate, lithium phosphate and lithium nitrate. The iron source may include at least one of ferric phosphate, ferric nitrate and ferrous sulfate. The carbon source may include at least one of glucose, sucrose, polyethylene glycol and lactose.

[0029] In some embodiments, the preparation of the lithium iron phosphate precursor may include the following steps:

[0030] The lithium source, the iron source, and the carbon source are mixed in a stoichiometric ratio, and deionized water is added to obtain a mixture. Optionally, the mass of the deionized water is 30-60% of the total mass of the lithium source, the iron source, and the carbon source. The proportion of the deionized water is selected to ensure uniform mixing between the lithium source, the iron source, and the carbon source, while also reducing energy consumption in subsequent steps.

[0031] The mixture is wet ball-milled and dried. The ball-milled mixture can be dried by spray granulation to obtain the lithium iron phosphate precursor. Optionally, the particle size of the lithium iron phosphate precursor can be 0.3-2 μm.

[0032] In another embodiment, the particle size of the lithium iron phosphate precursor may be less than 0.3 μm or greater than 2 μm.

[0033] In another embodiment, the lithium iron oxide precursor can be obtained by dry grinding.

[0034] In some embodiments, the mass of the metal powder is 3-10% of the mass of the lithium iron phosphate precursor. The particle size of the metal powder is less than 20 μm.

[0035] In other embodiments, the mass ratio of the metal powder to the lithium iron phosphate precursor particles may be less than 0.03 or greater than 0.1.

[0036] Step S102, sintering the sintering precursor. The sintering includes the following steps:

[0037] Sintering at 250-650°C for 2-4 hours, then heating to 750-800°C for 8-12 hours. The heating rate is 2-5°C / min, and the sintering is carried out under vacuum conditions or in a protective atmosphere with a flow rate of 10-40L / min, and the oxygen content in the protective atmosphere is below 50ppm. The protective gas includes but is not limited to nitrogen.

[0038] During the sintering process, the iron source, the lithium source and the carbon source react to generate lithium iron phosphate.

[0039] Step S103, naturally cooling the sintered precursor to room temperature and crushing it to obtain a powdery lithium iron phosphate material. The sintered precursor can be crushed by grinding or air flow crushing.

[0040] The present application uniformly mixes antimony powder or bismuth powder in the lithium iron phosphate precursor so that the antimony powder or bismuth powder is evenly dispersed in the particle gaps of the lithium iron phosphate precursor. Since antimony powder or bismuth powder has the special property of thermal shrinkage, as the temperature rises, the crystal structure and atomic arrangement will change, and the atomic arrangement will be tighter, resulting in a reduction in volume. In the step of sintering to form lithium iron phosphate, the antimony powder or bismuth powder will drive the lithium iron phosphate precursor particles to shrink tightly together, reducing the spacing between the particles of the lithium iron phosphate precursor, thereby being able to at least increase the compaction density of the lithium iron phosphate material to 2.7g / cm3. In addition, the present application only shrinks the lithium iron phosphate precursor, and there is no need to increase the size of the lithium iron phosphate particles or reduce the amount of carbon coating on the surface of the particles, which is conducive to simplifying the process of preparing lithium iron phosphate.

[0041] The present application also provides a positive electrode sheet, comprising a positive electrode material, wherein the positive electrode material comprises the lithium iron phosphate material obtained by the preparation method of the lithium iron phosphate material.

[0042] Specifically, in some embodiments, the lithium iron phosphate material can be prepared into a positive electrode sheet by the following steps:

[0043] A binder slurry is prepared, a conductive additive is added to the binder slurry to prepare a first slurry, and then lithium iron phosphate is added to the first slurry to prepare a second slurry, the second slurry is coated on an aluminum foil, and then baked to obtain a positive electrode sheet.

[0044] The present application also provides a battery (not shown), the battery comprising the positive electrode sheet. Specifically, the battery may also comprise a negative electrode sheet and a separator.

[0045] Specifically:

[0046] Embodiment 1:

[0047] 36.64 g lithium carbonate, 150.82 g iron phosphate, 11.31 g glucose and 281.20 g deionized water were weighed and added to a stirring tank for wet ball milling to obtain a slurry with a particle size D50 of 0.3 μm. The slurry was dried by spray drying to obtain a granular lithium iron phosphate precursor.

[0048] Antimony powder is added to the lithium iron phosphate precursor, wherein the mass of the antimony powder is 3% of the lithium iron phosphate precursor and the particle size of the antimony powder is 15 μm. The lithium iron phosphate precursor and the antimony powder can be evenly mixed by a high-speed mixer to obtain a sintered precursor.

[0049] The sintering precursor was placed in a box furnace for sintering in a nitrogen atmosphere with a flow rate of 25 L / min and an oxygen content of less than 50 ppm. The sintering was first performed at 630° C. for 2 hours, then heated to 780° C. at a heating rate of 5° C. / min and sintered for another 11 hours.

[0050] The sintered precursor is naturally cooled to room temperature and subjected to air flow crushing to obtain a powdery lithium iron phosphate product. The SEM image of the lithium iron phosphate product is as follows: Figure 2 shown.

[0051] Embodiment 2:

[0052] The difference from Example 1 is that the mass of the antimony powder is 5% of the lithium iron phosphate precursor, the particle size of the antimony powder is 10 μm, and the sintered precursor is first sintered at 640° C. for 3 hours and then heated to 790° C. for 12 hours.

[0053] Embodiment 3:

[0054] The difference from Example 1 is that the mass of the antimony powder is 7% of the lithium iron phosphate precursor, the particle size of the antimony powder is 8 μm, and the sintered precursor is first sintered at 650° C. for 4 hours and then heated to 800° C. for 12 hours.

[0055] Embodiment 4:

[0056] 36.64 g lithium carbonate, 150.82 g iron phosphate, 11.31 g glucose and 281.20 g deionized water were weighed and added to a stirring tank for wet ball milling to obtain a slurry with a particle size D50 of 0.3 μm. The slurry was dried by spray drying to obtain a granular lithium iron phosphate precursor.

[0057] Bismuth powder is added to the lithium iron phosphate precursor, wherein the mass of the bismuth powder is 3% of the lithium iron phosphate precursor and the particle size of the bismuth powder is 15 μm. The lithium iron phosphate precursor and the bismuth powder can be uniformly mixed by a high-speed mixer to obtain a sintered precursor.

[0058] The sintering precursor was placed in a box furnace for sintering. The sintering was carried out in a nitrogen atmosphere with a flow rate of 25 L / min and an oxygen content of less than 50 ppm. The sintering was first carried out at 270°C for 2 hours, and then the temperature was increased to 780°C at a heating rate of 5°C / min and sintered for another 11 hours.

[0059] The sintered precursor is naturally cooled to room temperature and subjected to air flow crushing to obtain a powdery lithium iron phosphate product.

[0060] Embodiment 5:

[0061] The difference from Example 4 is that the mass of the bismuth powder is 5% of the lithium iron phosphate precursor, and the particle size of the bismuth powder is 10 μm. The sintered precursor is first sintered at 280° C. for 4 hours, and then heated to 790° C. for 12 hours.

[0062] Embodiment 6:

[0063] The difference from Example 4 is that the mass of the bismuth powder is 7% of the lithium iron phosphate precursor, and the particle size of the bismuth powder is 8 μm. The sintered precursor is first sintered at 290° C. for 4 hours, and then heated to 800° C. for 12 hours.

[0064] Embodiment 7:

[0065] The difference from Example 1 is that antimony powder and bismuth powder are added to the lithium iron phosphate precursor. The particle size of the antimony powder is 10 μm. The mass of the bismuth powder is 3% of the lithium iron phosphate precursor, and the particle size of the bismuth powder is 8 μm. The lithium iron phosphate precursor and the antimony powder and bismuth powder can be uniformly mixed by a high-speed mixer to obtain a sintered precursor.

[0066] Comparative Example 1:

[0067] 36.64 g lithium carbonate, 150.82 g iron phosphate, 11.31 g glucose and 281.20 g deionized water were weighed and added to a stirring tank for wet ball milling to obtain a slurry with a particle size D50 of 0.3 μm. The slurry was dried by spray drying to obtain a granular lithium iron phosphate precursor.

[0068] The sintering precursor was sintered in a box furnace under a 25 L / min nitrogen atmosphere with the oxygen content controlled below 50 ppm. It was first sintered at a low temperature of 270° C. for 2 h, then heated to 780° C. for 12 h, with a heating rate of 5° C. / min.

[0069] The sintered precursor is cooled to room temperature and then the cooled sintered precursor is subjected to air flow crushing to obtain a powdered lithium iron phosphate product.

[0070] The present application tests the compaction density of powdered lithium iron phosphate by the following method.

[0071]

[0072]

[0073] Lithium iron phosphate is prepared into pole pieces, and the pole pieces, negative electrode shells, metal lithium sheets, diaphragms, gaskets, spring sheets, positive electrode shells and electrolytes are assembled into button batteries, and the batteries are tested for charge and discharge. The specific battery test method is:

[0074]

[0075]

[0076] The test results of the compaction density of the lithium iron phosphate powder obtained in the above Examples 1-7 and Comparative Example 1 are as follows.

[0077]

[0078] The above test results show that the compacted density of the lithium iron phosphate without adding antimony powder or bismuth powder in Comparative Example 1 is 2.4 g / cm 3In Examples 1-7, when different proportions of antimony powder or bismuth powder are added to the lithium iron phosphate precursor, the compaction density of the lithium iron phosphate can be increased to at least 2.7 g / cm 3 .

[0079] The above description is only a preferred embodiment of the present application, and does not limit the patent scope of the present application. All equivalent structural changes made under the concept of the present application using the contents of the present application specification and drawings, or directly / indirectly used in other related technical fields are included in the patent protection scope of the present application.

Claims

1. A method for preparing a lithium iron phosphate material, characterized in that: The steps include: Adding metal powder to a lithium iron phosphate precursor, wherein the metal powder includes at least one of antimony powder and bismuth powder, and mixing them evenly to obtain a sintered precursor; sintering the sintering precursor; The sintered precursor is naturally cooled to room temperature and crushed to obtain a powdery lithium iron phosphate material.

2. The method for preparing the lithium iron phosphate material according to claim 1, characterized in that: The sintering comprises the following steps: The process is sintered at 250-650°C for 2-4 hours, and then heated to 750-800°C for 8-12 hours, with a heating rate of 2-5°C / min. The sintering is carried out under vacuum conditions or in a protective atmosphere with a flow rate of 10-40 L / min, wherein the oxygen content in the protective atmosphere is below 50 ppm.

3. The method for preparing the lithium iron phosphate material according to claim 1, characterized in that: The mass of the metal powder is 3-10% of the mass of the lithium iron phosphate precursor.

4. The method for preparing the lithium iron phosphate material according to claim 1, characterized in that: The particle size of the lithium iron phosphate precursor is 0.3-2 μm.

5. The method for preparing the lithium iron phosphate material according to claim 4, characterized in that: The particle size of the metal powder is less than 20 μm.

6. The method for preparing the lithium iron phosphate material according to claim 1, characterized in that: The lithium iron phosphate precursor includes a lithium source, an iron source and a carbon source, the molar ratio of the lithium source to the iron source is 0.96-1.04, the mass of the carbon source is 5-15% of the total mass of the lithium source and the iron source, and the iron source or the lithium source includes phosphate.

7. The method for preparing the lithium iron phosphate material according to claim 6, characterized in that: The preparation of the lithium iron phosphate precursor comprises: Mixing the lithium source, the iron source and the carbon source according to a stoichiometric ratio, and adding deionized water to obtain a mixture; The mixture was wet ball milled and dried.

8. A positive electrode sheet, comprising a positive electrode material, characterized in that: The positive electrode material includes a lithium iron phosphate material obtained by the preparation method of the lithium iron phosphate material according to any one of claims 1 to 7.

9. A battery, characterized in that: The battery comprises the positive electrode sheet as claimed in claim 8.

Citation Information

Patent Citations

  • Method for enhancing conductivity of lithium iron phosphate material

    CN102403502A

  • Preparation method for antimony doped lithium ion battery positive electrode material

    CN103050695A

  • Preparation method for improving compaction density of lithium iron phosphate anode material and lithium iron phosphate anode material

    CN109795998A

  • Bismuth tungstate-coated lithium iron phosphate positive electrode material and preparation method thereof

    CN113471420A

  • Preparation method of lithium iron phosphate positive electrode material and lithium ion battery