Optimization method of barium carbonate powder preparation process based on microwave calcination and hydrothermal method
By combining microwave calcination and hydrothermal methods in the preparation process of barium carbonate, using La+ ion doping and optimizing calcination conditions, the problems of high impurity content and large particle size of barium carbonate products in the existing technology were solved, and small particle size, Spherical barium carbonate particles with good uniformity meet the high-quality needs of the microelectronics industry.
Patent Information
- Application Number
- CN202410972165.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-15
AI Technical Summary
The products generated by existing barium carbonate preparation methods have high impurity content, uncontrollable particle morphology, large particle size, and long production time, making it difficult to meet the application needs of high-quality barium carbonate in the field of microelectronic devices.
A process optimization method based on microwave calcination and hydrothermal method was adopted. Barium carbonate slurry was prepared by hydrothermal method and then calcined in a constant-temperature microwave calciner. Combined with La+ ion doping, the calcining conditions were adjusted to obtain small particle size and high tetragonality. Spherical barium carbonate particles.
The preparation of barium carbonate particles with small particle size and good uniformity has been achieved, the impurity content has been reduced, the crystallinity and dispersion of the particles have been improved, and the demand for high-quality barium carbonate in the electronics industry has been met.
Smart Images

Figure CN118771433A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of barium carbonate production, and in particular relates to a method for optimizing the preparation process of barium carbonate powder based on microwave calcination and hydrothermal method. Background Art
[0002] Barium carbonate is an important inorganic chemical raw material, widely used in glass, ceramics, microelectronic devices and other fields. With the development of science and technology, the quality requirements for barium carbonate are getting higher and higher, and different fields have different requirements for its particle morphology. For example, rod-shaped barium carbonate is suitable for general ceramic fields, needle-shaped barium carbonate is suitable for coating fields, and spherical barium carbonate is the first choice for microelectronic devices. In addition, barium carbonate isotopes as tracer substances also have broad application prospects in the biomedical field.
[0003] At present, most methods for preparing barium carbonate adopt a hydrothermal method. For example, Chinese patent application No. 202011089098.4 discloses a method for preparing spherical barium carbonate particles by a hydrothermal method, comprising: preparing a weakly acidic aqueous solution and deoxygenating it; mixing the deoxygenated weakly acidic aqueous solution with an organic solvent, adding BaCl2·2H2O and an anionic surfactant to dissolve, and obtaining a barium chloride solution; taking the deoxygenated weakly acidic aqueous solution, adding urea to dissolve, and obtaining a urea solution; mixing the urea solution and the barium chloride solution, transferring them into a reactor, and reacting them at 100-120°C to obtain spherical barium carbonate particles; the mass ratio of BaCl2·2H2O to urea is (7-14):(1-7). The method adds a surfactant to make the barium carbonate spherical during the growth process, and the sphericity is good; the hydrothermal method sets the temperature at 100° to 120°, and the pH is 6.0 to 6.5, and then only centrifugal separation, washing and drying are performed, resulting in the prepared spherical barium carbonate particles with large particle size, high distortion rate and serious agglomeration. Summary of the invention
[0004] In order to solve the problems existing in the background technology, the present invention provides a method for optimizing the preparation process of barium carbonate powder based on microwave calcination and hydrothermal method, comprising:
[0005] S1: preparing barium carbonate slurry by hydrothermal method;
[0006] S2: The barium carbonate slurry obtained after hydrothermal synthesis is put into a constant temperature microwave calcining furnace and calcined at a constant temperature T1 for 0.5 h to obtain spherical barium carbonate particles.
[0007] Preferably, the constant temperature microwave calcining furnace uses air atmosphere as the reaction atmosphere.
[0008] Preferably, after the constant temperature microwave calcination furnace calcines the nano-barium carbonate particles at a constant temperature T1 for 0.5 hours, the temperature is reduced at a cooling rate of 7 to 10° C. / min.
[0009] Preferably, the T1 is between 650°C and 750°C.
[0010] Preferably, when the barium carbonate slurry is calcined in a constant temperature microwave calcining furnace, La is doped into the barium carbonate slurry. + particle.
[0011] Preferably, the preparation of spherical nano-barium carbonate particles by hydrothermal method comprises:
[0012] S11: soaking and slurrying the barium carbonate ore to select a mixed ore of barium sulfate, barium carbonate and calcium carbonate;
[0013] S12: pouring the selected mixed ore into a glass fiber reinforced plastic hydrochloric acid tank for acid hydrolysis, adjusting the solution pH to 3.00 to separate the barite;
[0014] S13: The mixed solution of calcium chloride and barium chloride after the heavy metal stone is separated in step S12 is initially concentrated by an MVR evaporator to salt out crude barium chloride;
[0015] S14: Recrystallizing the crude barium chloride salted out in step S13 with deionized water to prepare high-purity barium chloride;
[0016] S15: reacting the high-purity barium chloride prepared in step S14 with membrane caustic soda to produce primary barium hydroxide, and purifying the primary barium hydroxide by an LGZ centrifuge to obtain high-purity barium hydroxide;
[0017] S16: Pass carbon dioxide gas through the reactor to remove impurities, then add sodium hydroxide aqueous solution and mix with carbon dioxide, then add the high-purity barium hydroxide obtained in step S15, stir and dissolve, and keep warm at a temperature of 150-210° C. and a pressure of 3 MPa for 12-24 hours to obtain barium carbonate slurry.
[0018] Preferably, the pH value of the solution is maintained at 3 during the stirring process of step S16.
[0019] The present invention has at least the following beneficial effects
[0020] Compared with the existing barium carbonate preparation methods, which have the defects of high impurity content, uncontrollable particle morphology, large particle size and long production time, the present invention improves the hydrothermal method and creates a microwave calcination method, fully considering factors such as raw material purity, good calcination atmosphere and uniform synthesis, ensuring that the product can be obtained by calcining at 700 degrees Celsius for 0.5 hours. In addition, while ensuring a small particle size, the tetragonality of the barium carbonate particles is greatly improved, which is more in line with the application requirements of the electronics industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a schematic diagram of the method flow of the present invention;
[0022] Figure 2 This is an experimental simulation diagram of spherical barium carbonate particles prepared by traditional hydrothermal method;
[0023] Figure 3 This is an experimental simulation diagram of the spherical barium carbonate particles prepared by the present invention;
[0024] Figure 4 Graph showing the effect of pH value on the purity of barium carbonate slurry in an embodiment of the present invention. DETAILED DESCRIPTION
[0025] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the illustrations provided in the following embodiments only illustrate the basic concept of the present invention in a schematic manner, and the following embodiments and features in the embodiments can be combined with each other without conflict.
[0026] Among them, the drawings are only used for illustrative explanations, and they only represent schematic diagrams rather than actual pictures, and should not be understood as limitations on the present invention. In order to better illustrate the embodiments of the present invention, some parts of the drawings may be omitted, enlarged or reduced, and do not represent the size of actual products. For those skilled in the art, it is understandable that some well-known structures and their descriptions in the drawings may be omitted.
[0027] The same or similar numbers in the drawings of the embodiments of the present invention correspond to the same or similar parts; in the description of the present invention, it should be understood that if the terms "upper", "lower", "left", "right", "front", "rear", etc. indicate the orientation or position relationship, they are based on the orientation or position relationship shown in the drawings, which is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation. Therefore, the terms describing the position relationship in the drawings are only used for illustrative purposes and cannot be understood as limiting the present invention. For ordinary technicians in this field, the specific meanings of the above terms can be understood according to specific circumstances.
[0028] See also Figure 1 The present invention provides a method for optimizing the preparation process of barium carbonate powder based on microwave calcination and hydrothermal method, comprising:
[0029] S1: preparing barium carbonate slurry by hydrothermal method;
[0030] S2: The barium carbonate slurry obtained after hydrothermal synthesis is put into a constant temperature microwave calcining furnace and calcined at a constant temperature T1 for 0.5 h to obtain spherical barium carbonate particles.
[0031] Preferably, the constant temperature microwave calcining furnace uses air atmosphere as the reaction atmosphere.
[0032] Preferably, after the constant temperature microwave calcination furnace calcines the nano-barium carbonate particles at a constant temperature T1 for 0.5 hours, the temperature is reduced at a cooling rate of 7 to 10° C. / min.
[0033] Preferably, the T1 is between 650°C and 750°C.
[0034] Preferably, when the barium carbonate slurry is calcined in a constant temperature microwave calcining furnace, La3 + Particles, doping concentration ratio 100:8, La + Ion doping can adjust the grain size of barium carbonate crystals, making them have better crystal structure and performance; La + Ion doping may help improve the thermal stability of barium carbonate materials, enabling them to better withstand high-temperature calcination processes.
[0035] Embodiment 1, the present invention provides a process for preparing barium carbonate slurry by hydrothermal method, comprising:
[0036] S11: soaking and slurrying the barium carbonate ore to select a mixed ore of barium sulfate, barium carbonate and calcium carbonate;
[0037] An implementation method of step S11, in this embodiment, firstly, barium carbonate ore is placed in an aqueous solution for soaking, the reaction temperature is 800-900° C., and the soaking time is 4-6 hours; the barium carbonate ore is crushed by a crusher, and then the slurry is adjusted by a paddle making machine, and then a concentrator is used to select a mixed ore of barium sulfate, barium carbonate and calcium carbonate by gravity separation.
[0038] S12: pouring the selected mixed ore into a glass fiber reinforced plastic hydrochloric acid tank for acid hydrolysis, adjusting the solution pH to 3.00 to separate the barite;
[0039] An implementation method of step S12, in this embodiment, the selected mixed ore is poured into a glass fiber reinforced plastic hydrochloric acid tank and acidified by hydrochloric acid. The acidification time is 4 hours, and the pH value of the solution is adjusted to 3.00. At this time, the barite can be filtered, and then the filtered barite is washed, filtered, dried, packaged, and high-quality drilling materials are produced.
[0040] S13: The mixed solution of calcium chloride and barium chloride after the heavy metal stone is separated in step S12 is initially concentrated by an MVR evaporator for 1 hour to salt out crude barium chloride;
[0041] S14: placing the crude barium chloride salted out in step S13 into a jacketed crystallization tube, and then recrystallizing with deionized water to prepare high-purity barium chloride;
[0042] S15: reacting the high-purity barium chloride prepared in step S14 with membrane caustic soda, with the reaction temperature controlled at 80-100° C. for 0.1-0.5 hours, until no barium chloride particles are visible, to produce primary barium hydroxide, and purifying the primary barium hydroxide by an LGZ centrifuge to obtain high-purity barium hydroxide;
[0043] S16: Pass carbon dioxide gas through the reactor for 2 hours to remove impurities, then add sodium hydroxide aqueous solution and mix with carbon dioxide, then add the high-purity barium hydroxide obtained in step S15, stir and dissolve, and keep warm at a temperature of 150-210° C. and a pressure of 3 MPa for 12-24 hours to obtain barium carbonate slurry.
[0044] In this embodiment, the temperature in the reactor is 43-55°C.
[0045] Preferably, the pH value of the solution is maintained at 3 during the stirring process of step S16. Figure 3 , Figure 3 The effect of different pH values on the concentration of barium carbonate in the barium carbonate slurry is shown. When the pH value is 3, the concentration is above 99.5%.
[0046] Embodiment 2, the present invention provides a process of barium carbonate slurry comprising:
[0047] (1) preparing a weakly acidic aqueous solution with a pH of 6.00 to 6.50, and performing a deoxygenation treatment to obtain a deoxygenated weakly acidic aqueous solution;
[0048] (2) mixing the deoxygenated weakly acidic aqueous solution in step (1) with an organic solvent, and sequentially adding BaCl2·2H2O and an anionic surfactant to dissolve the mixture to obtain a barium chloride solution;
[0049] (3) taking the deoxygenated weakly acidic aqueous solution in step (1), adding urea to dissolve it to obtain a urea solution;
[0050] (4) The urea solution in step (3) and the barium chloride solution in step (2) are mixed, transferred into a reaction kettle, and reacted at 100-120° C. to obtain a barium carbonate slurry, wherein the mass ratio of the BaCl2·2H2O in step 2) to the urea in step 3) is (7-14):(1-7); in step 2), the volume of the deoxygenated weakly acidic aqueous solution, the volume of the organic solvent, the mass of the BaCl2·2H2O, and the mass of the anionic surfactant are (20-60) mL:(80-120) mL:(7-14) g:(0.6-3) g; the anionic surfactant is selected from one or more of sodium polystyrene sulfonate, polyacrylic acid, and polyglutamic acid; in step 4), the reaction time is 5.5-10 hours. Step 2) is carried out in a nitrogen atmosphere, and the organic solvent is selected from one or more of ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, and tetraethylene glycol; in step 2), the barium element in the BaCl2·2H2O is selected from 138 8. 137 8. 136 8. 135 8. 134 8. 132 8. 130 Ba one or more; the carbon element in the urea is selected from 12 C. 13 C. 14 C one or more; step 4), the drying time is 60 ~ 80 ℃, the drying time is 6 to 8 hours; step 1), the weakly acidic aqueous solution is dilute nitric acid, and nitrogen is introduced for the deoxygenation treatment.
[0051] The barium carbonate particles prepared by the method of the present invention have high crystallinity, complete crystal form, a weight loss rate of only 1.1%, an average particle size of 37nm, a specific surface area of 25.975m2 / g, and a barium-carbon ratio of 1.0017. The method of preparing barium carbonate powder by microwave calcination combined with hydrothermal synthesis is conducive to the preparation of small-particle-size, well-dispersed and uniform barium carbonate nanopowders, which can meet the demand of the electronic ceramic industry for high-quality barium carbonate, and can therefore be used in multilayer ceramic capacitors (MLCCs);
[0052] See also Figure 2 and Figure 3 , Figure 2 Spherical barium carbonate particles prepared by traditional hydrothermal method. Figure 3The spherical barium carbonate particles prepared by the present invention are found by comparison that the average particle size of traditional spherical barium carbonate particles is 150-410nm, and the particle size distribution is uneven, while the average particle size of the spherical barium carbonate particles of the present invention is 40-60nm, and the particle size of the spherical barium carbonate particles is smaller and more uniform. Therefore, the method provided by the present invention effectively improves the particle size uniformity of barium titanate powder prepared by the hydrothermal method, and greatly improves the tetragonality of the powder while ensuring a small particle size, which is more in line with the application requirements of the electronics industry.
[0053] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
[0054] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.
Claims
1. A method for optimizing the preparation process of barium carbonate powder based on microwave calcination and hydrothermal method, characterized in that: include: S1: preparing barium carbonate slurry by hydrothermal method; S2: The barium carbonate slurry obtained after hydrothermal synthesis is put into a constant temperature microwave calcining furnace and calcined at a constant temperature T1 for 0.5 h to obtain spherical barium carbonate particles.
2. The method for optimizing the preparation process of barium carbonate powder based on microwave calcination and hydrothermal method according to claim 1, characterized in that: The constant temperature microwave calcining furnace uses air atmosphere as the reaction atmosphere.
3. The method for optimizing the preparation process of barium carbonate powder based on microwave calcination and hydrothermal method according to claim 1, characterized in that: After the nano-barium carbonate particles are calcined for 0.5 hours in a constant temperature microwave calcination furnace at a constant temperature T1, the temperature is lowered at a cooling rate of 7 to 10°C / min.
4. The method for optimizing the preparation process of barium carbonate powder based on microwave calcination and hydrothermal method according to claim 1, characterized in that: The temperature T1 is between 650°C and 750°C.
5. The method for optimizing the preparation process of barium carbonate powder based on microwave calcination and hydrothermal method according to claim 1, characterized in that: When the barium carbonate slurry is calcined in a constant temperature microwave calcination furnace, La is added to the barium carbonate slurry. + particle.
6. The method for optimizing the preparation process of barium carbonate powder based on microwave calcination and hydrothermal method according to claim 1, characterized in that: The method of preparing spherical nano-barium carbonate particles by hydrothermal method comprises: S11: soaking and slurrying the barium carbonate ore to select a mixed ore of barium sulfate, barium carbonate and calcium carbonate; S12: pouring the selected mixed ore into a glass fiber reinforced plastic hydrochloric acid tank for acid hydrolysis, adjusting the solution pH to 3.00 to separate the barite; S13: The mixed solution of calcium chloride and barium chloride after the heavy metal stone is separated in step S12 is initially concentrated by an MVR evaporator to salt out crude barium chloride; S14: Recrystallizing the crude barium chloride salted out in step S13 with deionized water to prepare high-purity barium chloride; S15: reacting the high-purity barium chloride prepared in step S14 with membrane caustic soda to produce primary barium hydroxide, and purifying the primary barium hydroxide by an LGZ centrifuge to obtain high-purity barium hydroxide; S16: Pass carbon dioxide gas through the reactor to remove impurities, then add sodium hydroxide aqueous solution and mix with carbon dioxide, then add the high-purity barium hydroxide obtained in step S15, stir and dissolve, and keep warm at a temperature of 150-210° C. and a pressure of 3 MPa for 12-24 hours to obtain barium carbonate slurry.
7. The method for optimizing the preparation process of barium carbonate powder based on microwave calcination and hydrothermal method according to claim 1, characterized in that: The pH value of the solution was maintained at 3 during the stirring process in step S16.
Citation Information
Patent Citations
Method for preparing spherical barium carbonate particles by hydrothermal method
CN112174182A
Cited By
Process route for preparing high-purity strontium or barium compound
CN120364736A
A process route for preparing high purity strontium or barium compounds
CN120364736B