AlN ceramic substrate and preparation method and application thereof

CN118771891APending Publication Date: 2024-10-15KONFOONG MATERIALS INTERNATIONAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410846732.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

When preparing AlN ceramic substrates in the existing technology, substrates with a thickness greater than 0.5 mm need to go through complex intermediate processes such as lamination and warm isostatic pressing, resulting in complex processes and high additional costs, and there is a lack of simplified preparation methods.

Method used

Using a combined organic solvent system of ethanol, butanone and n-butanol, the plasticizer, binder and AlN powder are mixed by heating and stirring, and ball milling and tape casting are performed to directly prepare a blank with a thickness of 1.5-3mm, and pass After degreasing and sintering, a 0.6-1.5mm AlN ceramic substrate is obtained, which avoids lamination and warm isostatic pressing processes.

Benefits of technology

It significantly simplifies the process flow, reduces additional costs, improves production efficiency, and is suitable for large-scale applications.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides an AlN ceramic substrate and a preparation method and application thereof, and the preparation method comprises the steps: mixing a plasticizer, a binder and an organic solvent, and heating and stirring to obtain a mixed solvent; performing first-stage powder mixing on the mixed dispersing agent, the sintering aid and part of the mixed solvent to obtain a first mixed material; mixing AlN powder and the first mixed material for second-stage powder mixing to obtain a second mixed material; mixing the residual mixed solvent and the second mixed material, and performing ball milling to obtain AlN slurry; sequentially carrying out vacuum defoaming, tape casting and drying on the AlN slurry to obtain an AlN biscuit; sequentially slitting and degreasing the AlN biscuit to obtain an AlN green body; and sintering the AlN green body to obtain the AlN ceramic substrate. According to the preparation method provided by the invention, the thick ceramic green body can be obtained without intermediate processes such as lamination and warm isostatic pressing, so that the process flow is simplified, the additional cost is reduced, the production efficiency is improved, and large-scale popularization and application are facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of ceramic substrates, and relates to an AlN ceramic substrate, and in particular to an AlN ceramic substrate and a preparation method and application thereof. Background Art

[0002] AlN is a covalently bonded compound with a hexagonal wurtzite crystal structure. Its thermal conductivity is phonon conduction, which satisfies the characteristics of high thermal conductivity. Its theoretical thermal conductivity is 320W / (m·K) and its theoretical density is 3.26g / cm 3 , Mohs hardness is 7-8, decomposition temperature is 2200-2250℃, has low dielectric constant, linear expansion coefficient matching silicon (Si), excellent electrical insulation, high specific strength, high temperature resistance, non-toxicity and other characteristics. The comprehensive performance of AlN ceramics is better than A1 2 O 3 And BeO ceramics are the first choice for the new generation of semiconductor substrates and electronic component packaging materials, and have very broad application prospects in the electronics industry.

[0003] Ceramic molding is an important process in the preparation of ceramic materials. Specifically, it refers to making ceramic raw powder into a green body with a specified size and shape and a certain mechanical strength. There are many molding processes in the preparation of ceramic materials. Commonly used AlN ceramic preparation molding processes include dry pressing, isostatic pressing, powder injection molding and tape casting.

[0004] Among them, the shape of the green body formed by dry pressing and isostatic pressing is limited by the mold and is not suitable for manufacturing green bodies with complex structures. In addition, the mold production cost is high, the friction between the powder and the mold is large during the pressing process, and the axial compressive stress is easily lost, resulting in uneven stress distribution and inconsistent density of the internal structure of the green body. Injection molding is suitable for preparing ceramic parts with complex shapes, and for thin plate-type ceramic parts, it is suitable to be prepared by tape casting. This process has the advantages of simplicity, high efficiency, short production cycle, and easy mass production. It is the preferred method for preparing AlN ceramic substrates.

[0005] CN102557646A discloses a method for preparing an AlN ceramic substrate. The method comprises the following steps: firstly preparing a substrate main body green sheet and a surface layer green sheet respectively by a tape casting method, then attaching the surface layer green sheet to the upper and lower surfaces of the substrate main body green sheet, and then pressing the green sheet into a complete green body. After debinding and sintering, the AlN ceramic substrate is obtained.

[0006] CN106187201A discloses a method for preparing aluminum nitride ceramics by benzene-free tape casting. The method comprises the following steps: firstly, a mixed solvent is prepared by using a plurality of alcohol solvents, and the mixed solvent, a dispersant, AlN ceramic powder and a sintering aid are mixed and subjected to primary ball milling. Then, a plasticizer and a binder are added and subjected to secondary ball milling. The AlN slurry after the secondary ball milling is subjected to vacuum stirring and degassing, and then a tape casting operation is performed and the mixture is dried and peeled off to obtain an AlN green sheet with uniform structure and high density.

[0007] However, the existing technology for preparing AlN ceramic substrates with a thickness greater than 0.5 mm is all made by stacking and firing multiple layers of thin green blanks. In the middle, multiple steps such as lamination and warm isostatic pressing are required to obtain ceramic green blanks, and finally sintering is performed to prepare the AlN ceramic substrate. The intermediate process is complicated and the additional cost is high.

[0008] It can be seen that how to provide an AlN ceramic substrate and a preparation method thereof to avoid obtaining thick ceramic green bodies through intermediate processes such as lamination and warm isostatic pressing, simplify the process flow, reduce additional costs, and improve production efficiency has become an urgent problem that technical personnel in this field need to solve. Summary of the invention

[0009] In view of the shortcomings of the prior art, the purpose of the present invention is to provide an AlN ceramic substrate and a preparation method and application thereof. The preparation method does not require intermediate processes such as lamination and warm isostatic pressing to obtain a thick ceramic green body, simplifies the process flow, reduces additional costs, improves production efficiency, and is conducive to large-scale promotion and application.

[0010] To achieve this object, the present invention adopts the following technical solutions:

[0011] In a first aspect, the present invention provides a method for preparing an AlN ceramic substrate, the preparation method comprising the following steps:

[0012] (1) mixing a plasticizer, a binder and an organic solvent, heating and stirring the mixture to obtain a mixed solvent; the organic solvent is a combination of ethanol, butanone and n-butanol;

[0013] (2) mixing a dispersant, a sintering aid and a portion of the mixed solvent obtained in step (1) to perform a first stage powder mixing to obtain a first mixed material;

[0014] (3) mixing AlN powder and the first mixed material obtained in step (2) to perform second-stage powder mixing to obtain a second mixed material;

[0015] (4) mixing the remaining mixed solvent obtained in step (1) and the second mixed material obtained in step (3) and performing ball milling to obtain AlN slurry;

[0016] (5) subjecting the AlN slurry obtained in step (4) to vacuum degassing, tape casting and drying in sequence to obtain an AlN blank;

[0017] (6) cutting and degreasing the AlN blank obtained in step (5) to obtain an AlN green blank;

[0018] (7) Sintering the AlN green body obtained in step (6) to obtain an AlN ceramic substrate.

[0019] The preparation method provided by the present invention adopts a ternary solvent system of a combination of ethanol, butanone and n-butanol to prepare an AlN ceramic substrate, and can directly realize the casting of a thick film. First, AlN powder, a plasticizer, a binder, a dispersant and a sintering aid are uniformly mixed to prepare an AlN slurry, and then a tape casting molding process is adopted to cast a green blank with a thickness of 1.5-3 mm through the synergistic effect of various solvents, and then through processes such as degreasing and sintering, finally, an AlN ceramic substrate with a thickness of 0.6-1.5 mm is directly obtained, without the need for intermediate processes such as lamination and warm isostatic pressing, thereby significantly simplifying the process flow, reducing additional costs, improving production efficiency, and being conducive to large-scale promotion and application.

[0020] Preferably, the plasticizer in step (1) comprises dibutyl phthalate and / or butyl benzyl phthalate.

[0021] Preferably, the binder in step (1) comprises polyvinyl butyral.

[0022] Preferably, taking the total mass of the mixed solvent as the calculation basis, the content of the binder is 6-15wt%, for example, it can be 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt% or 15wt%, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0023] Preferably, the mass ratio R of the plasticizer to the binder in step (1) is (0.2-1):1, for example, it can be 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1 or 1:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0024] Preferably, taking the total mass of the organic solvent in step (1) as a calculation basis, the content of the ethanol is 5-15wt%, for example, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt% or 15wt%, the content of the butanone is 10-20wt%, for example, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt% or 20wt%, and the content of the n-butanol is 65-85wt%, for example, 65wt%, 66wt%, 68wt%, 70wt%, 72wt%, 74wt%, 76wt%, 78wt%, 80wt%, 82wt%, 84wt% or 85wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are equally applicable.

[0025] Preferably, the heating and stirring in step (1) is carried out in a constant temperature magnetic stirrer, and the heating temperature is 40-80°C, for example, it can be 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] Preferably, the dispersant in step (2) comprises any one of herring oil, castor oil or triolein, or a combination of at least two of them. Typical but non-limiting combinations include a combination of herring oil and castor oil, a combination of castor oil and triolein, a combination of herring oil and triolein, or a combination of herring oil, castor oil and triolein.

[0027] Preferably, taking the total mass of the first mixture as the calculation basis, the content of the dispersant is 0.5-3wt%, for example, it can be 0.5wt%, 0.6wt%, 0.8wt%, 1wt%, 1.2wt%, 1.4wt%, 1.6wt%, 1.8wt%, 2wt%, 2.2wt%, 2.4wt%, 2.6wt%, 2.8wt% or 3wt%, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] Preferably, the sintering aid in step (2) includes Y 2 O 3 , CaF 2 , HfO 2 or LaF 3 Any one or a combination of at least two of the following, typical but non-limiting combinations include Y 2 O 3 With CaF 2 Combination of CaF2 With HfO 2 Combination of HfO 2 With LaF 3 Combination of Y 2 O 3 , CaF 2 With HfO 2 Combination of CaF 2 , HfO 2 With LaF 3 A combination of, or Y 2 O 3 , CaF 2 , HfO 2 With LaF 3 combination.

[0029] Preferably, taking the total mass of the first mixture as the calculation basis, the content of the sintering aid is 1-7wt%, for example, it can be 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, 5.5wt%, 6wt%, 6.5wt% or 7wt%, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] Preferably, the mass ratio of the mixed solvent in step (2) to the mixed solvent in step (1) is 10-50%, for example, it can be 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45% or 50%, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0031] Preferably, the time for mixing the powder in the first stage of step (2) is 0.5-3 h, for example, it can be 0.5 h, 0.6 h, 0.8 h, 1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h, 2 h, 2.2 h, 2.4 h, 2.6 h, 2.8 h or 3 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0032] Preferably, the mixing mass ratio of the AlN powder to the first mixed material in step (3) is 1:(0.5-2), for example, it can be 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9 or 1:2, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0033] Preferably, the time for the second stage powder mixing in step (3) is 6-24 hours, for example, it can be 6 hours, 8 hours, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours or 24 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] Preferably, the ball milling time in step (4) is 6-24 h, for example, 6 h, 8 h, 10 h, 12 h, 14 h, 16 h, 18 h, 20 h, 22 h or 24 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] Preferably, the viscosity of the AlN slurry after vacuum degassing in step (5) is 15-30 Pa·s, for example, it can be 15 Pa·s, 16 Pa·s, 17 Pa·s, 18 Pa·s, 19 Pa·s, 20 Pa·s, 21 Pa·s, 22 Pa·s, 23 Pa·s, 24 Pa·s, 25 Pa·s, 26 Pa·s, 27 Pa·s, 28 Pa·s, 29 Pa·s or 30 Pa·s, but is not limited to the listed values, and other unlisted values ​​within the numerical range are equally applicable.

[0036] Preferably, the tape casting in step (5) is carried out in a tape casting machine, and the height of the scraper is adjusted to 1.5-3.5 mm, for example, it can be 1.5 mm, 1.6 mm, 1.8 mm, 2 mm, 2.2 mm, 2.4 mm, 2.6 mm, 2.8 mm, 3 mm, 3.2 mm, 3.4 mm or 3.5 mm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] Preferably, the casting speed of the tape casting in step (5) is 0.05-0.2 m / min, for example, it can be 0.05 m / min, 0.06 m / min, 0.08 m / min, 0.1 m / min, 0.12 m / min, 0.14 m / min, 0.16 m / min, 0.18 m / min or 0.2 m / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] Preferably, the thickness of the AlN blank in step (5) is 1.5-3 mm, for example, 1.5 mm, 1.6 mm, 1.7 mm, 1.8 mm, 1.9 mm, 2 mm, 2.1 mm, 2.2 mm, 2.3 mm, 2.4 mm, 2.5 mm, 2.6 mm, 2.7 mm, 2.8 mm, 2.9 mm or 3 mm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0039] Preferably, the degreasing in step (6) is carried out in a degreasing furnace, and the degreasing temperature is 500-600°C, for example, it can be 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 590°C or 600°C, and the insulation time is 1-5h, for example, it can be 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h or 5h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are equally applicable.

[0040] Preferably, the sintering treatment in step (7) is carried out in a vacuum sintering furnace in a protective gas atmosphere, and the protective gas includes nitrogen, helium or argon, more preferably nitrogen.

[0041] Preferably, the temperature of the sintering treatment in step (7) is 1750-1850°C, for example, it can be 1750°C, 1760°C, 1770°C, 1780°C, 1790°C, 1800°C, 1810°C, 1820°C, 1830°C, 1840°C or 1850°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0042] Preferably, the sintering time in step (7) is 1-5 h, for example, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h or 5 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0043] Preferably, the thickness of the AlN ceramic substrate in step (7) is 0.6-1.5 mm, for example, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm or 1.5 mm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0044] As a preferred technical solution of the first aspect of the present invention, the preparation method comprises the following steps:

[0045] (1) mixing ethanol, butanone and n-butanol to obtain an organic solvent, wherein the total mass of the organic solvent is used as a calculation basis, the content of the ethanol is 5-15wt%, the content of the butanone is 10-20wt%, and the content of the n-butanol is 65-85wt%;

[0046] (2) mixing a plasticizer, a binder and the organic solvent obtained in step (1), heating and stirring in a constant temperature magnetic stirrer, and the heating temperature is 40-80° C. to obtain a mixed solvent; the plasticizer comprises dibutyl phthalate and / or butyl benzyl phthalate, the binder comprises polyvinyl butyral, and the total mass of the mixed solvent is used as a calculation basis, the content of the binder is 6-15wt%, and the mass ratio R of the plasticizer to the binder is (0.2-1):1;

[0047] (3) mixing a dispersant, a sintering aid and a portion of the mixed solvent obtained in step (2) for a first stage of mixing for 0.5-3 hours to obtain a first mixed material; the dispersant comprises any one of herring oil, castor oil or triolein or a combination of at least two thereof; the sintering aid comprises Y 2 O 3 , CaF 2 , HfO 2 or LaF 3 Any one or a combination of at least two of the above, and taking the total mass of the first mixed material as the calculation basis, the content of the dispersant is 0.5-3wt%, and the content of the sintering aid is 1-7wt%; the mass ratio of the mixed solvent to the mixed solvent in step (2) is 10-50%;

[0048] (4) mixing AlN powder and the first mixed material obtained in step (3) in a mass ratio of 1:(0.5-2) for 6-24 hours to obtain a second mixed material;

[0049] (5) mixing the remaining mixed solvent obtained in step (2) and the second mixed material obtained in step (4) and ball milling for 6-24 hours to obtain AlN slurry;

[0050] (6) vacuum degassing the AlN slurry obtained in step (4), adjusting the slurry viscosity to 15-30 Pa·s, and then injecting it into a tape casting machine for tape casting, and adjusting the height of the scraper to 1.5-3.5 mm and the tape casting speed to 0.05-0.2 m / min. After drying, an AlN blank with a thickness of 1.5-3 mm is obtained;

[0051] (7) cutting the AlN blank obtained in step (5) and then placing it in a degreasing furnace for degreasing, and controlling the degreasing temperature to be 500-600° C. and the holding time to be 1-5 h to obtain an AlN green blank;

[0052] (8) The AlN green body obtained in step (6) is placed in a vacuum sintering furnace in a nitrogen atmosphere for sintering, and the sintering temperature is controlled to be 1750-1850° C. and the holding time is 1-5 h to obtain an AlN ceramic substrate with a thickness of 0.6-1.5 mm.

[0053] In a second aspect, the present invention provides an AlN ceramic substrate, wherein the AlN ceramic substrate is prepared by the preparation method described in the first aspect.

[0054] In a third aspect, the present invention provides an application of the AlN ceramic substrate as described in the second aspect, wherein the AlN ceramic substrate is used as a packaging material for integrated circuits, semiconductor module circuits, and high-power devices.

[0055] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0056] Compared with the prior art, the present invention has the following beneficial effects:

[0057] The preparation method provided by the present invention adopts a ternary solvent system of a combination of ethanol, butanone and n-butanol to prepare an AlN ceramic substrate, and can directly realize the casting of a thick film. First, AlN powder, a plasticizer, a binder, a dispersant and a sintering aid are uniformly mixed to prepare an AlN slurry, and then a tape casting molding process is adopted to cast a green blank with a thickness of 1.5-3 mm through the synergistic effect of various solvents, and then through processes such as degreasing and sintering, finally, an AlN ceramic substrate with a thickness of 0.6-1.5 mm is directly obtained, without the need for intermediate processes such as lamination and warm isostatic pressing, thereby significantly simplifying the process flow, reducing additional costs, improving production efficiency, and being conducive to large-scale promotion and application. DETAILED DESCRIPTION

[0058] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0059] Example 1

[0060] This embodiment provides an AlN ceramic substrate and a preparation method thereof, the preparation method comprising the following steps:

[0061] (1) mixing ethanol, butanone and n-butanol to obtain an organic solvent, wherein the total mass of the organic solvent is used as a calculation basis, the content of the ethanol is 10wt%, the content of the butanone is 15wt%, and the content of the n-butanol is 75wt%;

[0062] (2) mixing a plasticizer (dibutyl phthalate), a binder (polyvinyl butyral) and the organic solvent obtained in step (1), heating and stirring in a constant temperature magnetic stirrer at a heating temperature of 60° C. to obtain a mixed solvent, wherein the total mass of the mixed solvent is used as a calculation basis, the content of the binder is 10 wt %, and the mass ratio R of the plasticizer to the binder is 0.6:1;

[0063] (3) Mixed dispersant (herring oil), sintering aid (Y 2 O 3 ) and part of the mixed solvent obtained in step (2) are mixed for 2 hours in the first stage to obtain a first mixed material, and the total mass of the first mixed material is used as the calculation basis, the content of the dispersant is 2wt%, and the content of the sintering aid is 4wt%; the mass ratio of the mixed solvent to the mixed solvent in step (2) is 30%;

[0064] (4) mixing AlN powder and the first mixed material obtained in step (3) in a mass ratio of 1:1.2 for 12 hours to obtain a second mixed material;

[0065] (5) mixing the remaining mixed solvent obtained in step (2) and the second mixed material obtained in step (4) and ball milling for 12 hours to obtain AlN slurry;

[0066] (6) vacuum degassing the AlN slurry obtained in step (4), adjusting the slurry viscosity to 20 Pa·s, and then injecting it into a tape casting machine for tape casting, and adjusting the scraper height to 2.5 mm and the tape casting speed to 0.15 m / min. After drying, an AlN blank with a thickness of 2.2 mm was obtained;

[0067] (7) cutting the AlN blank obtained in step (5) and then placing it in a degreasing furnace for degreasing, and controlling the degreasing temperature to be 550° C. and the holding time to be 3 h to obtain an AlN green blank;

[0068] (8) The AlN green body obtained in step (6) is placed in a vacuum sintering furnace in a nitrogen atmosphere for sintering, and the sintering temperature is controlled to be 1800° C. and the holding time is 3 h to obtain an AlN ceramic substrate with a thickness of 1 mm.

[0069] Example 2

[0070] This embodiment provides an AlN ceramic substrate and a preparation method thereof, the preparation method comprising the following steps:

[0071] (1) mixing ethanol, butanone and n-butanol to obtain an organic solvent, wherein the total mass of the organic solvent is used as a calculation basis, the content of the ethanol is 5wt%, the content of the butanone is 10wt%, and the content of the n-butanol is 85wt%;

[0072] (2) mixing a plasticizer (butyl benzyl phthalate), a binder (polyvinyl butyral) and the organic solvent obtained in step (1), heating and stirring in a constant temperature magnetic stirrer at a heating temperature of 40° C. to obtain a mixed solvent, wherein the total mass of the mixed solvent is used as a calculation basis, the content of the binder is 6wt%, and the mass ratio R of the plasticizer to the binder is 1:1;

[0073] (3) Mixed dispersant (castor oil), sintering aid (CaF 2 ) and part of the mixed solvent obtained in step (2) are mixed for 0.5 h in the first stage to obtain a first mixed material, and the total mass of the first mixed material is used as the calculation basis, the content of the dispersant is 0.5wt%, the content of the sintering aid is 1wt%; the mass ratio of the mixed solvent to the mixed solvent in step (2) is 10%;

[0074] (4) mixing AlN powder and the first mixed material obtained in step (3) in a mass ratio of 1:0.5 for 6 hours to obtain a second mixed material;

[0075] (5) mixing the remaining mixed solvent obtained in step (2) and the second mixed material obtained in step (4) and ball milling for 6 hours to obtain AlN slurry;

[0076] (6) vacuum degassing the AlN slurry obtained in step (4), adjusting the slurry viscosity to 15 Pa·s, and then injecting it into a tape casting machine for tape casting, and adjusting the height of the scraper to 1.8 mm and the tape casting speed to 0.05 m / min. After drying, an AlN blank with a thickness of 1.5 mm was obtained;

[0077] (7) cutting the AlN blank obtained in step (5) and then placing it in a degreasing furnace for degreasing, and controlling the degreasing temperature to be 500° C. and the holding time to be 5 h to obtain an AlN green blank;

[0078] (8) The AlN green body obtained in step (6) is placed in a vacuum sintering furnace in a helium atmosphere for sintering, and the sintering temperature is controlled to be 1750° C. and the holding time is 5 h to obtain an AlN ceramic substrate with a thickness of 0.6 mm.

[0079] Example 3

[0080] This embodiment provides an AlN ceramic substrate and a preparation method thereof, the preparation method comprising the following steps:

[0081] (1) mixing ethanol, butanone and n-butanol to obtain an organic solvent, wherein the total mass of the organic solvent is used as a calculation basis, the content of the ethanol is 15wt%, the content of the butanone is 20wt%, and the content of the n-butanol is 65wt%;

[0082] (2) mixing a plasticizer (equal weights of dibutyl phthalate and butyl benzyl phthalate), a binder (polyvinyl butyral) and the organic solvent obtained in step (1), heating and stirring in a constant temperature magnetic stirrer at a temperature of 80° C. to obtain a mixed solvent, wherein the total weight of the mixed solvent is used as a calculation basis, the content of the binder is 15 wt %, and the mass ratio R of the plasticizer to the binder is 0.2:1;

[0083] (3) Mixed dispersant (triolein), sintering aid (HfO 2 ) and part of the mixed solvent obtained in step (2) are mixed for 3 hours in the first stage to obtain a first mixed material, and the total mass of the first mixed material is used as the calculation basis, the content of the dispersant is 3wt%, and the content of the sintering aid is 7wt%; the mass ratio of the mixed solvent to the mixed solvent in step (2) is 50%;

[0084] (4) mixing AlN powder and the first mixed material obtained in step (3) in a mass ratio of 1:2 for 24 hours to obtain a second mixed material;

[0085] (5) mixing the remaining mixed solvent obtained in step (2) and the second mixed material obtained in step (4) and ball milling for 24 hours to obtain AlN slurry;

[0086] (6) vacuum degassing the AlN slurry obtained in step (4), adjusting the slurry viscosity to 30 Pa·s, and then injecting it into a tape casting machine for tape casting, and adjusting the height of the scraper to 3.5 mm and the tape casting speed to 0.2 m / min. After drying, an AlN blank with a thickness of 3 mm was obtained;

[0087] (7) cutting the AlN blank obtained in step (5) and then placing it in a degreasing furnace for degreasing, and controlling the degreasing temperature to be 600° C. and the holding time to be 1 h to obtain an AlN green blank;

[0088] (8) The AlN green body obtained in step (6) is placed in a vacuum sintering furnace in an argon atmosphere for sintering, and the sintering temperature is controlled to be 1850° C. and the holding time is 1 h to obtain an AlN ceramic substrate with a thickness of 1.5 mm.

[0089] Example 4

[0090] This embodiment provides an AlN ceramic substrate and a preparation method thereof. Except that the mass ratio R of the plasticizer to the binder in step (2) is changed to 0.1:1, the remaining steps and conditions are the same as those in embodiment 1 and are not described in detail here.

[0091] After testing, the thickness of the AlN blank obtained in this embodiment is 2.0 mm, and the thickness of the AlN ceramic substrate is 0.7 mm.

[0092] Example 5

[0093] This embodiment provides an AlN ceramic substrate and a preparation method thereof. Except that the mass ratio R of the plasticizer to the binder in step (2) is changed to 1.2:1, the remaining steps and conditions are the same as those in embodiment 1, and thus are not described in detail here.

[0094] After testing, the thickness of the AlN blank obtained in this embodiment is 2.4 mm, and the thickness of the AlN ceramic substrate is 1.3 mm.

[0095] Comparative Example 1

[0096] This comparative example provides an AlN ceramic substrate and a preparation method thereof, except that step (1) is changed to: mixing ethanol and butanone to obtain an organic solvent, and the total mass of the organic solvent is used as the calculation basis, the content of ethanol is 40wt%, and the content of butanone is 60wt%; the remaining steps and conditions are the same as those in Example 1, and therefore are not described here.

[0097] After testing, the thickness of the AlN blank obtained in this comparative example was 1.2 mm, and the thickness of the AlN ceramic substrate was 0.4 mm.

[0098] Comparative Example 2

[0099] This comparative example provides an AlN ceramic substrate and a preparation method thereof, except that step (1) is changed to: mixing ethanol and n-butanol to obtain an organic solvent, and the total mass of the organic solvent is used as the calculation basis, the content of ethanol is 12wt%, and the content of n-butanol is 88wt%; the remaining steps and conditions are the same as those in Example 1, and therefore are not described here.

[0100] After testing, the thickness of the AlN blank obtained in this comparative example was 1.3 mm, and the thickness of the AlN ceramic substrate was 0.5 mm.

[0101] Comparative Example 3

[0102] This comparative example provides an AlN ceramic substrate and a preparation method thereof, except that step (1) is changed to: mixing butanone and n-butanol to obtain an organic solvent, and the total mass of the organic solvent is used as the calculation basis, the content of butanone is 17wt%, and the content of n-butanol is 83wt%; the remaining steps and conditions are the same as those in Example 1, and therefore are not described here.

[0103] After testing, the thickness of the AlN blank obtained in this comparative example was 1.1 mm, and the thickness of the AlN ceramic substrate was 0.3 mm.

[0104] It can be seen that the preparation method provided by the present invention adopts the ternary solvent system of the combination of ethanol, butanone and n-butanol to prepare the AlN ceramic substrate, which can directly realize the casting of thick films. First, the AlN powder, plasticizer, binder, dispersant and sintering aid are uniformly mixed to obtain AlN slurry, and then the tape casting molding process is adopted to cast a green blank with a thickness of 1.5-3mm through the synergistic effect of each solvent, and then through the processes of degreasing and sintering, finally, the AlN ceramic substrate with a thickness of 0.6-1.5mm is directly obtained, without the need for intermediate processes such as lamination and warm isostatic pressing, which significantly simplifies the process flow, reduces the additional cost, improves the production efficiency, and is conducive to large-scale promotion and application.

[0105] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an AlN ceramic substrate, characterized in that: The preparation method comprises the following steps: (1) mixing a plasticizer, a binder, and an organic solvent, heating and stirring the mixture to obtain a mixed solvent; the organic solvent is a combination of ethanol, butanone, and n-butanol; (2) mixing a dispersant, a sintering aid, and a portion of the mixed solvent obtained in step (1) to perform a first-stage powder mixing to obtain a first mixed material; (3) mixing AlN powder and the first mixed material obtained in step (2) to perform a second stage of powder mixing to obtain a second mixed material; (4) mixing the remaining mixed solvent obtained in step (1) and the second mixed material obtained in step (3) and ball milling to obtain AlN slurry; (5) subjecting the AlN slurry obtained in step (4) to vacuum degassing, tape casting, and drying in sequence to obtain an AlN blank; (6) Cutting and degreasing the AlN blank obtained in step (5) to obtain an AlN green blank; (7) Sintering the AlN green body obtained in step (6) to obtain an AlN ceramic substrate.

2. The preparation method according to claim 1, characterized in that The plasticizer in step (1) comprises dibutyl phthalate and / or butyl benzyl phthalate; Preferably, the binder in step (1) comprises polyvinyl butyral; Preferably, the content of the binder is 6-15 wt % based on the total mass of the mixed solvent; Preferably, the mass ratio R of the plasticizer to the binder in step (1) is (0.2-1):

1.

3. The preparation method according to claim 1 or 2, characterized in that Taking the total mass of the organic solvent in step (1) as a calculation basis, the content of the ethanol is 5-15wt%, the content of the butanone is 10-20wt%, and the content of the n-butanol is 65-85wt%; Preferably, the heating and stirring in step (1) is carried out in a constant temperature magnetic stirrer, and the heating temperature is 40-80°C.

4. The preparation method according to any one of claims 1 to 3, characterized in that The dispersant in step (2) comprises any one of herring oil, castor oil or triolein, or a combination of at least two thereof; Preferably, the content of the dispersant is 0.5-3 wt % based on the total mass of the first mixed material; Preferably, the sintering aid in step (2) includes any one of Y2O3, CaF2, HfO2 or LaF3, or a combination of at least two thereof; Preferably, the content of the sintering aid is 1-7 wt % based on the total mass of the first mixed material; Preferably, the mass ratio of the mixed solvent in step (2) to the mixed solvent in step (1) is 10-50%; Preferably, the time for mixing the powder in the first stage of step (2) is 0.5-3 hours.

5. The preparation method according to any one of claims 1 to 4, characterized in that The mixing mass ratio of the AlN powder to the first mixed material in step (3) is 1:(0.5-2); Preferably, the time for mixing the powder in the second stage of step (3) is 6-24 hours; Preferably, the ball milling time in step (4) is 6-24 hours.

6. The preparation method according to any one of claims 1 to 5, characterized in that The viscosity of the AlN slurry after vacuum degassing in step (5) is 15-30 Pa·s; Preferably, the tape casting in step (5) is carried out in a tape casting machine, and the height of the scraper is adjusted to 1.5-3.5 mm; Preferably, the casting speed of the tape casting in step (5) is 0.05-0.2 m / min; Preferably, the thickness of the AlN blank in step (5) is 1.5-3 mm.

7. The preparation method according to any one of claims 1 to 6, characterized in that The degreasing in step (6) is carried out in a degreasing furnace, and the degreasing temperature is 500-600° C. and the holding time is 1-5 hours; Preferably, the sintering treatment in step (7) is carried out in a vacuum sintering furnace in a protective gas atmosphere, and the protective gas includes nitrogen, helium or argon, more preferably nitrogen; Preferably, the temperature of the sintering treatment in step (7) is 1750-1850°C; Preferably, the sintering treatment time in step (7) is 1-5 hours; Preferably, the thickness of the AlN ceramic substrate in step (7) is 0.6-1.5 mm.

8. The preparation method according to any one of claims 1 to 7, characterized in that The preparation method comprises the following steps: (1) mixing ethanol, butanone, and n-butanol to obtain an organic solvent, wherein the total mass of the organic solvent is used as a calculation basis, the content of the ethanol is 5-15wt%, the content of the butanone is 10-20wt%, and the content of the n-butanol is 65-85wt%; (2) mixing a plasticizer, a binder, and the organic solvent obtained in step (1), heating and stirring the mixture in a constant temperature magnetic stirrer at a temperature of 40-80° C. to obtain a mixed solvent; wherein the plasticizer comprises dibutyl phthalate and / or butyl benzyl phthalate, the binder comprises polyvinyl butyral, and the total mass of the mixed solvent is used as a calculation basis, the content of the binder is 6-15wt%, and the mass ratio R of the plasticizer to the binder is (0.2-1):1; (3) mixing a dispersant, a sintering aid, and a portion of the mixed solvent obtained in step (2) to perform a first-stage powder mixing for 0.5-3 hours to obtain a first mixed material; the dispersant comprises any one of herring oil, castor oil, or triolein, or a combination of at least two thereof; the sintering aid comprises any one of Y2O3, CaF2, HfO2, or LaF3, or a combination of at least two thereof; and based on the total mass of the first mixed material as a calculation basis, the content of the dispersant is 0.5-3wt%, and the content of the sintering aid is 1-7wt%; the mass ratio of the mixed solvent to the mixed solvent in step (2) is 10-50%; (4) mixing AlN powder and the first mixture obtained in step (3) in a mass ratio of 1:(0.5-2) for a second stage of mixing for 6-24 hours to obtain a second mixture; (5) mixing the remaining mixed solvent obtained in step (2) and the second mixed material obtained in step (4) and ball milling for 6-24 hours to obtain AlN slurry; (6) vacuum degassing the AlN slurry obtained in step (4), adjusting the slurry viscosity to 15-30 Pa·s, and then injecting it into a tape casting machine for tape casting, adjusting the scraper height to 1.5-3.5 mm, and the casting speed to 0.05-0.2 m / min. After drying, an AlN blank with a thickness of 1.5-3 mm is obtained; (7) Cutting the AlN blank obtained in step (5) and then placing it in a degreasing furnace for degreasing, controlling the degreasing temperature to 500-600° C. and the holding time to 1-5 h to obtain an AlN green blank; (8) The AlN green body obtained in step (6) is placed in a vacuum sintering furnace in a nitrogen atmosphere for sintering, and the sintering temperature is controlled to be 1750-1850°C and the holding time is 1-5 hours to obtain an AlN ceramic substrate with a thickness of 0.6-1.5 mm.

9. An AlN ceramic substrate, characterized in that: The AlN ceramic substrate is prepared by the preparation method according to any one of claims 1 to 8.

10. An application of the AlN ceramic substrate according to claim 9, characterized in that: The AlN ceramic substrate is used as a packaging material for integrated circuits, semiconductor module circuits and high-power devices.

Citation Information

Patent Citations

  • Modified aluminum nitride ceramic substrate and production method thereof

    CN106938935A

  • Aluminum nitride ceramic slurry and preparation method thereof

    CN107324812A

  • Sintering aid composite additive for silicon nitride ceramic slurry, silicon nitride ceramic slurry as well as preparation method and application thereof

    CN111484335A

  • Molecular beam epitaxy aluminum nitride ceramic crucible and manufacturing method thereof

    CN116986911A

  • A METHOD FOR PREPARING SPHERICAL AlN GRANULES

    TWI579231B