Method for synthesizing 4, 4 '-diaminodiphenyl ether through continuous catalytic hydrogenation
By using nanomagnetic Fe3O4@SiO2@Salent-Ni(II) composite catalyst in a tubular reactor for continuous catalytic hydrogenation reaction, the problems of low catalyst efficiency and environmental pollution in the existing technology are solved, and high-efficiency, low-cost The cost-effective production of 4,4'-diaminodiphenyl ether is suitable for industrial production.
Patent Information
- Application Number
- CN202410851435.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-15
AI Technical Summary
The existing technology has the problems of low catalyst efficiency, high cost and environmental pollution in the production of 4,4'-diaminodiphenyl ether, and the intermittent hydrogenation process is cumbersome and has low production efficiency.
The nanomagnetic Fe3O4@SiO2@Salent-Ni(II) composite catalyst is used to carry out continuous catalytic hydrogenation reaction in a tubular reactor. The power frequency magnetic field is used to promote catalytic efficiency, achieve continuous production of products, and reduce catalyst separation steps and three wastes. produce.
It improves catalytic efficiency, reduces production costs, simplifies the process flow, is suitable for industrial production, significantly reduces environmental pollution, and improves product yield and purity.
Smart Images

Figure CN118771992A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of organic synthesis, and specifically relates to a method for synthesizing 4,4'-diaminodiphenyl ether by continuous catalytic hydrogenation. Background Art
[0002] 4,4'-diaminodiphenyl ether (abbreviated as 4,4'-ODA or ODA) is an important chemical intermediate, which is mainly used to prepare resins such as polyimide, or to synthesize 3,3',4,4'-tetraaminodiphenyl aldehyde, and then to prepare high temperature resistant heterocyclic polymers such as polybenzimidazole. In addition, 4,4'-diaminodiphenyl ether can also be used as a curing agent for heat-resistant epoxy resins and polyurethanes. 4,4'-diaminodiphenyl ether is widely used in chemical fields such as dyes, polyethers, polyamides, polyether esters and flame retardants, and is also used to synthesize fluorescent dyes, photosensitive substances and high-performance polymers.
[0003] Industrially, 4,4'-diaminodiphenyl ether is mainly prepared by reducing 4,4'-dinitrodiphenyl ether. There are two main methods: one is the non-catalytic hydrogenation reduction method, which uses chemical substances other than hydrogen as reducing agents, which can be further divided into iron powder reduction method, stannous chloride-hydrochloric acid reduction method, alkali sulfide reduction method and hydration reduction method. The iron powder reduction method uses iron as an electron donor, water or alcohol as a proton donor, electrolytes such as NH4C1, FeCl2, etc. can promote the reaction, and the addition of surfactants can increase the reaction contact area. The stannous chloride (SnCl2)-hydrochloric acid reduction method uses hydrochloric acid as a medium, SnCl2 as a reducing agent, or SnCl2 produced by the in-situ reaction of tin flowers with concentrated hydrochloric acid as a reducing agent. The alkali sulfide reduction method uses alkali sulfide as an electron donor and water as a proton. Commonly used alkali sulfides include Na2S, NaHHS, and Na2S2. The hydrazine hydrate reduction method uses hydrazine hydrate as a reducing agent and hydrogen donor, and the catalyst includes Pd / C or FeC13·6H20. The first three methods are classic methods for reducing nitro compounds to amines. The process is relatively mature, but the yield is low, and a large amount of solid waste is generated, which pollutes the environment and is an obsolete process. The hydrazine hydrate reduction method uses highly corrosive hydrazine hydrate, has a high production cost, and is not suitable for large-scale production.
[0004] The second is the catalytic hydrogenation reduction method, which is to pass hydrogen gas in the presence of a catalyst for reduction. This method has a high yield and less process pollution, and is a green synthesis process. The catalyst used in the catalytic hydrogenation of 4,4'-dinitrodiphenyl ether to prepare 4,4'-diaminodiphenyl ether is mainly skeleton nickel (Ni), Pd / C or Pt / C, and the hydrogenation yield is about 90%, but the manufacture of skeleton Ni catalyst will cause environmental pollution, and the price of Pd and Pt precious metals is high, and the production cost is high.
[0005] Supported Ni-based catalysts exhibit excellent hydrogenation activity and selectivity and have broad application prospects.
[0006] In addition, intermittent hydrogenation requires high-pressure equipment, cumbersome operation, low single-time utilization of hydrogen, long production cycle, and low production efficiency. Continuous hydrogenation is the development direction. The use of microchannel reactors to achieve continuous hydrogenation can simplify the process, improve product yield and purity, and is of great significance to the green manufacturing of 4,4'-diaminodiphenyl ether.
[0007] Therefore, it is necessary to provide a method for preparing 4,4'-diaminodiphenyl ether with high catalytic efficiency, low cost and environmental friendliness. Summary of the invention
[0008] The technical problem to be solved by the present invention is: in view of the shortcomings of the prior art, a method for synthesizing 4,4'-diaminodiphenyl ether by continuous catalytic hydrogenation is provided, the method has stable reaction conditions, high catalyst efficiency, no separation is required, and continuous production of the product can be achieved.
[0009] In order to solve the above technical problems, the technical solution of the present invention is:
[0010] A method for synthesizing 4,4'-diaminodiphenyl ether by continuous catalytic hydrogenation comprises the following steps:
[0011] S1: mixing 4,4'-dinitrodiphenyl ether represented by formula (I) with a protic solvent to prepare a feed solution;
[0012] S2: Nano-magnetic Fe 3 O 4 @SiO 2 The @Salent-Ni(II) composite catalyst is loaded into the tubular reactor 6, and after nitrogen is introduced to completely replace the air, nitrogen is passed for protection, the tubular reactor 6 is preheated, the industrial frequency magnetic field generator 4 is turned on, and then hydrogen is continuously introduced;
[0013] S3: After the feed liquid prepared in step S1 and hydrogen are mixed in a gas-liquid mixer 3 in a continuous feeding manner, a continuous catalytic hydrogenation reaction is carried out through a shell-and-tube reactor 6, and the reaction liquid is condensed through a condenser, the gas and liquid are separated, the separated liquid is collected, the separated liquid is cooled, crystallized, filtered, and dried to obtain the target product 4,4'-diaminodiphenyl ether represented by formula (II);
[0014] The reaction equation is as follows:
[0015]
[0016] Furthermore, in step S1, the inner diameter of the reaction tube 7 of the shell-and-tube reactor 6 is 3 mm to 5 mm, the tube length is 1 m, and the catalyst fixed bed filling length is 60 to 80 cm; the shell-and-tube reactor 6 is composed of 4 to 10 reaction tubes 7 arranged in parallel.
[0017] Furthermore, in step S1, the protic solvent is one or a mixture of two or more of DMF, DMAC, ethylene glycol, n-butanol or glycerol; the mass amount of the protic solvent is 5 to 6 times the mass of 4,4'-dinitrodiphenyl ether represented by the raw material formula (I).
[0018] Furthermore, in step S2, the preheating temperature of the shell-and-tube reactor is 90-130°C, the magnetic field strength is 500A / m-1200A / m, and after hydrogen is passed, the pressure in the shell-and-tube reactor 6 is 6.0MPa-8.0MPa.
[0019] Furthermore, in step S2, the nanomagnetic Fe 3 O 4 @SiO 2 The preparation method of @Salent-Ni(II) composite catalyst comprises the following steps:
[0020] (i) dissolving nickel acetate in anhydrous ethanol to prepare a nickel acetate-ethanol solution, placing a Salen ligand in anhydrous ethanol to prepare a Salen ligand solution, heating, and ultrasonically treating until the mixture is uniformly mixed, then dropping the nickel acetate-ethanol solution into the Salen ligand solution, and after ultrasonic treatment, stopping the reaction, cooling in an ice bath to crystallize, filtering, washing the filter cake with ethanol for 3 times, and vacuum drying to obtain a Salen-Ni(II) complex;
[0021] (ii) Take magnetic nanoparticles Fe 3 O 4 @SiO 2 The aqueous solution was soaked with Salen-Ni(II) complex, and then passed into a magnetic separator to separate magnetic particles. The magnetic particles were then washed with distilled water for 3 times and vacuum dried to obtain magnetic Fe 3 O 4 @SiO 2 @Salen-Ni(II).
[0022] Furthermore, in step (i), the Salen ligand is N,N′-bis(2-hydroxyphenyl)ethylenediamine, N,N′-disalicylicylaldehyde-1,2-phenylenediamine or 1,2-cyclohexylamine bis(3,5-butyl sulfate).
[0023] Furthermore, in step (i), the molar ratio of Salen ligand to nickel acetate is 1:1, the concentration of Salen ligand solution is 10-20wt%, the concentration of nickel acetate-ethanol solution is 4-5wt%, the heating temperature is 40-50°C, the power of ultrasonic treatment is 800-1200W, and the time of ultrasonic treatment is 60-90min.
[0024] Furthermore, in step (ii), the magnetic nanoparticles Fe3 O 4 @SiO 2 The mass concentration of the aqueous solution is 1 mg / mL;
[0025] Nanoparticle Fe 3 O 4 @SiO 2 The mass ratio of the mixture to the Salen-Ni(II) complex is 1:(0.05-0.1), and the soaking time is 5-6 hours.
[0026] Furthermore, in step S3, the molar ratio of hydrogen to 4,4'-dinitrodiphenyl ether represented by formula (I) is 8 to 10:1.
[0027] Furthermore, in step S3, the residence time is 120s to 600s, and the crystallization temperature of the separated liquid is -5 to 0°C.
[0028] Due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0029] 1. The present invention adopts a novel Ni-based catalyst loaded with magnetic nanoparticles, which has high catalytic efficiency and adopts a fixed bed reactor, which does not require catalyst separation, is simple in post-processing, greatly reduces the generation of three wastes, and is environmentally friendly.
[0030] 2. The present invention effectively promotes the catalytic efficiency of the catalyst by setting the industrial frequency magnetic field strength, ensures the smooth progress of the reaction, and effectively controls the occurrence of side reactions.
[0031] 3. The present invention adopts tubular continuous flow to replace the traditional kettle intermittent reaction, which effectively improves the safety of the reaction. At the same time, the continuous hydrogenation process is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a schematic diagram of the structure of the synthesis device used in the reaction of the present invention.
[0033] Description of the numbers in the figure:
[0034] 1 hydrogen cylinder, 2 liquid storage tank, 3 gas-liquid mixer, 4 power frequency magnetic field generator, 5 tubular reactor jacket, A cavity, 6 tubular reactor, 7 reaction tube, 8 back pressure valve, 9 condenser, 10 gas-liquid separator, 11 receiving tank. DETAILED DESCRIPTION
[0035] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0036] Unless otherwise specified, all chemical reagents and materials in the following examples are commercially available products.
[0037] Example 1
[0038] Nano-magnetic Fe 3 O 4 @SiO 2 The preparation method of @Salent-Ni(II) composite catalyst comprises the following steps:
[0039] Step 1: The starting material is Salen ligand N,N'-bis(2-hydroxyphenyl)ethylenediamine, and the molar ratio of Salen ligand N,N'-bis(2-hydroxyphenyl)ethylenediamine ligand to nickel acetate is 1:1;
[0040] Nickel acetate is dissolved in anhydrous ethanol to prepare a nickel acetate-ethanol solution with a concentration of 4wt%; N, N'-bis(2-hydroxyphenyl)ethylenediamine is placed in anhydrous ethanol to prepare a Salen ligand N, N'-bis(2-hydroxyphenyl)ethylenediamine solution with a concentration of 10wt%, which is heated to 50°C and subjected to 800W ultrasonic treatment until the mixture is uniformly mixed; under 800W ultrasonic treatment, the nickel acetate-ethanol solution is added dropwise to the Salen ligand N, N'-bis(2-hydroxyphenyl)ethylenediamine solution, followed by ultrasonic treatment for 90 minutes, stopping the reaction, cooling in an ice bath for crystallization, filtering, washing the filter cake with ethanol for 3 times, and vacuum drying to obtain the N, N'-bis(2-hydroxyphenyl)ethylenediamine-Ni(II) complex.
[0041] Step 2: Nanoparticle Fe 3 O 4 @SiO 2 The mass ratio of the complex to N,N'-bis(2-hydroxyphenyl)ethylenediamine-Ni(II) is 1:0.1.
[0042] The magnetic nanoparticles Fe with a mass concentration of 1 mg / mL 3 O 4 @SiO 2 The aqueous solution was added to the N,N'-bis(2-hydroxyphenyl)ethylenediamine-Ni(ID) complex and immersed for 5 h. The magnetic particles were separated by a magnetic separator. The separated magnetic particles were washed with distilled water for 3 times and vacuum dried to obtain magnetic Fe 3 O 4 @SiO 2 @N,N′-Bis(2-hydroxyphenyl)ethylenediamine-Ni(II).
[0043] Example 2
[0044] Nano-magnetic Fe 3 O 4 @SiO 2 The preparation method of @Salent-Ni(II) composite catalyst comprises the following steps:
[0045] Step 1: The starting material is Salen ligand N, N'-disalicylic aldehyde-1, 2-phenylenediamine; the molar ratio of Salen ligand N, N'-disalicylic aldehyde-1, 2-phenylenediamine ligand to nickel acetate is 1:1;
[0046] Nickel acetate is dissolved in anhydrous ethanol to prepare a nickel acetate-ethanol solution with a concentration of 5wt%; N, N'-disalicylicaldehyde-1, 2-phenylenediamine is placed in anhydrous ethanol to prepare a Salen ligand N, N'-bis(2-hydroxyphenyl)ethylenediamine solution with a concentration of 20wt%, which is heated to 40°C and subjected to 1200W ultrasonic treatment until the mixture is uniformly mixed; under 1200W ultrasonic treatment, the nickel acetate-ethanol solution is added dropwise to the Salen ligand N, N'-bis(2-hydroxyphenyl)ethylenediamine solution, followed by ultrasonic treatment for 60 minutes, stopping the reaction, cooling in an ice bath for crystallization, filtering, washing the filter cake with ethanol for 3 times, and vacuum drying to obtain the N, N'-disalicylicaldehyde-1, 2-phenylenediamine-Ni(II) complex.
[0047] Step 2: Nanoparticle Fe 3 O 4 @SiO 2 The mass ratio of the raw materials to N, N′-disalicylicylaldehyde-1, 2-phenylenediamine-Ni (II) complex is 1:0.05.
[0048] The magnetic nanoparticles Fe with a mass concentration of 1 mg / mL 3 O 4 @SiO 2 The aqueous solution was added to the N,N'-disalicylicaldehyde-1,2-phenylenediamine-Ni(II) complex and immersed for 6 h. The magnetic particles were separated by a magnetic separator. The magnetic particles were washed with distilled water for 3 times and vacuum dried to obtain magnetic Fe 3 O 4 @SiO 2 @N, N′-disalicylicylaldehyde-1,2-phenylenediamine-Ni(ID.
[0049] Example 3
[0050] Nano-magnetic Fe 3 O 4 @SiO 2 The preparation method of @Salent-Ni(II) composite catalyst comprises the following steps:
[0051] Step 1: The starting material is Salen ligand 1,2-cyclohexylamine bis(3,5-sulfate butyl), and the molar ratio of Salen ligand 1,2-cyclohexylamine bis(3,5-sulfate butyl) ligand to nickel acetate is 1:1;
[0052] Nickel acetate is dissolved in anhydrous ethanol to prepare a nickel acetate-ethanol solution with a concentration of 5wt%; Salen ligand 1,2-cyclohexylamine bis(3,5-butyl sulfate) is placed in anhydrous ethanol to prepare a Salen ligand 1,2-cyclohexylamine bis(3,5-butyl sulfate) solution with a concentration of 15wt%, heated to 45°C, and ultrasonically treated at 1000W until mixed uniformly; under 1000W ultrasound, the nickel acetate-ethanol solution is added dropwise to the Salen ligand 1,2-cyclohexylamine bis(3,5-butyl sulfate) solution, followed by ultrasonic treatment for 80min, stopping the reaction, cooling in an ice bath for crystallization, filtering, washing the filter cake with ethanol for 3 times, and vacuum drying to obtain a 1,2-cyclohexylamine bis(3,5-butyl sulfate)-Ni(II) complex.
[0053] Nanoparticle Fe 3 O 4 @SiO 2 , 1,2-cyclohexylamine bis(3,5-sulfate butyl)-Ni(II) complex was added in a mass ratio of 1:0.08, and magnetic nanoparticles Fe with a mass concentration of 1 mg / mL were added. 3 O 4 @SiO 2 The aqueous solution was added to the 1,2-cyclohexylamine bis(3,5-sulfate butyl)-Ni(II) complex and immersed for 6 h. The magnetic particles were separated by a magnetic separator. The magnetic particles were washed with distilled water for 3 times and vacuum dried to obtain magnetic Fe 3 O 4 @SiO 2 @1,2-Cyclohexylamine bis(3,5-butylsulfate)-Ni(II).
[0054] Example 4
[0055] A method for continuously catalytic hydrogenation to synthesize 4,4'-diaminodiphenyl ether, the reaction device is shown in the attached Figure 1 .
[0056] The inner diameter of the reaction tube 7 is 3 mm, the tube length is 1 m, and the catalyst fixed bed filling length is 60 cm; the shell-and-tube reactor 6 is composed of 10 reaction tubes 7 arranged in parallel.
[0057] The protic solvent is DMF, and the mass amount of the protic solvent is 5 times the mass of the raw material 4,4'-dinitrodiphenyl ether. 3 O 4 @SiO 2 @Salent-Ni(II) composite catalyst is the magnetic Fe prepared in Example 1 3 O 4 @SiO 2 @N,N'-Bis(2-hydroxyphenyl)ethylenediamine-Ni(II).
[0058] The specific synthesis steps are as follows:
[0059] S1: 4,4'-dinitrodiphenyl ether and a protic solvent are mixed to prepare a feed liquid, which is placed in a feed liquid storage tank 2 for standby use.
[0060] S2: Nano-magnetic Fe 3 O 4 @SiO 2 @Salent-Ni(II) composite catalyst is loaded into the reaction tube 7 in the shell-and-tube reactor 6, and nitrogen is introduced to completely replace the air, and then nitrogen is passed for protection. The shell-and-tube reactor 6 is placed in the cavity A in the shell-and-tube reactor jacket 5, preheated to 90°C, the industrial frequency magnetic field generator 4 is turned on, the magnetic field strength is set to 800A / m, the back pressure valve 8 is opened, and then hydrogen is continuously introduced to make the pressure in the shell-and-tube reactor 6 reach 6.0MPa.
[0061] S3: The liquid in the liquid storage tank 2 and the hydrogen in the hydrogen cylinder 1 are mixed in a gas-liquid mixer 3 by continuous feeding in a molar ratio of 8:1, and then the mixed liquid is subjected to continuous catalytic hydrogenation reaction through a tubular reactor 6; after a stay of 450 seconds, the reaction liquid is passed into a condenser 9 for condensation, and then the condensate is passed into a gas-liquid separator 10 for gas-liquid separation, and the separated liquid is stored in a receiving tank 11. After the collected separated liquid is cooled to -5 to 0°C, it is crystallized, filtered, and dried to obtain the target product 4,4'-diaminodiphenyl ether shown in formula (II). The calculated product yield is 90.21%, and the product purity (HPLC) is 98.9%.
[0062] Example 5
[0063] A method for continuously catalytic hydrogenation to synthesize 4,4'-diaminodiphenyl ether, the reaction device is shown in the attached Figure 1 .
[0064] The inner diameter of the reaction tube 7 is 4 mm, the tube length is 1 m, and the catalyst fixed bed filling length is 70 cm; the shell-and-tube reactor is composed of 8 reaction tubes arranged in parallel.
[0065] The protic solvent is DMAC, and the mass amount of the protic solvent is 6 times the mass of the raw material 4,4'-dinitrodiphenyl ether. 3 O 4 @SiO 2 @Salent-Ni(II) composite catalyst is the magnetic Fe prepared in Example 2 3 O 4 @SiO 2 @N, N'-disalicylicylaldehyde-1,2-phenylenediamine-Ni(II).
[0066] The specific synthesis steps are as follows:
[0067] S1: 4,4'-dinitrodiphenyl ether and a protic solvent are mixed to prepare a feed liquid, which is placed in a feed liquid storage tank 2 for standby use.
[0068] S2: Nano-magnetic Fe 3 O 4 @SiO 2 @Salent-Ni(II) composite catalyst is loaded into the reaction tube 7 in the shell-and-tube reactor 6, and nitrogen is introduced to completely replace the air, and then nitrogen is passed for protection. The shell-and-tube reactor 6 is placed in the cavity A in the shell-and-tube reactor jacket 5, preheated to 110°C, the industrial frequency magnetic field generator is turned on, the magnetic field strength is set to 500A / m, the back pressure valve 8 is opened, and then hydrogen is continuously introduced to make the pressure in the shell-and-tube reactor 6 reach 8.0MPa.
[0069] S3: The liquid in the liquid storage tank 2 and the hydrogen in the hydrogen cylinder 1 are mixed in a gas-liquid mixer 3 in a molar ratio of 10:1 by continuous feeding, and then the mixed liquid is subjected to continuous catalytic hydrogenation reaction through a shell-and-tube reactor 6. After 600s of residence, the reaction liquid is passed into a condenser 9 for condensation, and then the condensate is passed into a gas-liquid separator 10 for gas-liquid separation, and the separated liquid is stored in a receiving tank 11. After the collected separated liquid is cooled to -5 to 0°C, it is crystallized, filtered, and dried to obtain the target product 4,4'-diaminodiphenyl ether shown in formula (II). The calculated product yield is 89.63%, and the product purity (HPLC) is 99.10%.
[0070] Example 6
[0071] A method for continuously catalytic hydrogenation to synthesize 4,4'-diaminodiphenyl ether, the reaction device is shown in the attached Figure 1 .
[0072] The inner diameter of the tubular reactor is 5 mm, the tube length is 1 m, and the catalyst fixed bed filling length is 80 cm; the tubular reactor is composed of 4 reaction tubes arranged in parallel.
[0073] The protic solvent is ethylene glycol, and the mass amount of the protic solvent is 5 times the mass of the raw material 4,4'-dinitrodiphenyl ether. 3 O 4 @SiO 2 @Salent-Ni(II) composite catalyst is the magnetic Fe prepared in Example 3 3 O 4 @SiO 2 @1,2-Cyclohexylamine bis(3,5-butylsulfate)-Ni(II).
[0074] The specific synthesis steps are as follows:
[0075] S1: 4,4'-dinitrodiphenyl ether and a protic solvent are mixed to prepare a feed liquid, which is placed in a feed liquid storage tank 2 for standby use.
[0076] S2: Nano-magnetic Fe 3 O 4 @SiO 2 @Salent-Ni(II) composite catalyst is loaded into the reaction tube 7 in the shell-and-tube reactor 6, and nitrogen is introduced to completely replace the air, and then nitrogen is passed for protection. The shell-and-tube reactor 6 is placed in the cavity A in the shell-and-tube reactor jacket 5, preheated to 130°C, the industrial frequency magnetic field generator 4 is turned on, the magnetic field strength is set to 1000A / m, the back pressure valve 8 is opened, and then hydrogen is continuously introduced to make the pressure in the shell-and-tube reactor 6 reach 8.0MPa.
[0077] S3: The liquid in the liquid storage tank 2 and the hydrogen in the hydrogen cylinder 1 are mixed in a gas-liquid mixer 3 in a molar ratio of 10:1 by continuous feeding, and then the mixed liquid is subjected to continuous catalytic hydrogenation reaction through a shell-and-tube reactor 6. After a residence time of 300 seconds, the reaction liquid is passed into a condenser 9 for condensation, and then the condensate is passed into a gas-liquid separator 10 for gas-liquid separation, and the separated liquid is stored in a receiving tank 11. After the collected separated liquid is cooled to -5 to 0°C, it is crystallized, filtered, and dried to obtain the target product 4,4'-diaminodiphenyl ether shown in formula (II). The calculated product yield is 92.31%, and the product purity (HPLC) is 99.35%.
[0078] Example 7
[0079] A method for continuously catalytic hydrogenation to synthesize 4,4'-diaminodiphenyl ether, the reaction device is shown in the attached Figure 1 .
[0080] The inner diameter of the reaction tube 7 is 3 mm, the tube length is 1 m, and the catalyst fixed bed filling length is 70 cm; the shell-and-tube reactor 6 is composed of 6 reaction tubes 7 arranged in parallel.
[0081] The proton solvent is a mixed solvent of n-butanol and ethylene glycol in a volume ratio of 1:1, and the amount of the proton solvent is 5 times the mass of the raw material 4,4'-dinitrodiphenyl ether. 3 O 4 @SiO 2 @Salent-Ni(II) composite catalyst is the magnetic Fe prepared in Example 1 3 O 4 @SiO 2 @N,N'-Bis(2-hydroxyphenyl)ethylenediamine-Ni(II).
[0082] S1: 4,4'-dinitrodiphenyl ether is mixed with a protic solvent to obtain a feed liquid, which is placed in a feed liquid storage tank 2 for standby use.
[0083] S2: Nano-magnetic Fe 3 O 4 @SiO 2 @Salent-Ni(II) composite catalyst is loaded into the reaction tube 7 in the shell-and-tube reactor 6, and nitrogen is introduced to completely replace the air, and then nitrogen is passed for protection. The shell-and-tube reactor 6 is placed in the cavity A in the shell-and-tube reactor jacket 5, preheated to 100°C, the industrial frequency magnetic field generator 4 is turned on, the magnetic field strength is set to 1200A / m, the back pressure valve 8 is opened, and then hydrogen is continuously introduced to make the pressure in the shell-and-tube reactor 6 reach 6.0MPa.
[0084] S3: The liquid in the liquid storage tank 2 and the hydrogen in the hydrogen cylinder 1 are mixed in a gas-liquid mixer 3 in a molar ratio of 9:1 by continuous feeding, and then the mixed liquid is subjected to continuous catalytic hydrogenation reaction through a shell-and-tube reactor 6. After 120 seconds of residence, the reaction liquid is passed into a condenser 9 for condensation, and then the condensate is passed into a gas-liquid separator 10 for gas-liquid separation, and the separated liquid is stored in a receiving tank 11. After the collected separated liquid is cooled to -5 to 0°C, it is crystallized, filtered, and dried to obtain the target product 4,4'-diaminodiphenyl ether shown in formula (II). The calculated product yield is 93.71%, and the product purity (HPLC) is 99.50%.
[0085] Example 8
[0086] A method for continuously catalytic hydrogenation to synthesize 4,4'-diaminodiphenyl ether, the reaction device is shown in the attached Figure 1 .
[0087] The inner diameter of the reactor 7 is 4 mm, the tube length is 1 m, and the catalyst fixed bed filling length is 80 cm; the shell-and-tube reactor 6 is composed of 8 reaction tubes 7 arranged in parallel.
[0088] The proton solvent is a mixed solvent of glycerol and n-butanol in a volume ratio of 1:1, and the mass amount of the proton solvent is 6 times the mass of the raw material 4,4'-dinitrodiphenyl ether. 3 O 4 @SiO 2 @Salent-Ni(II) composite catalyst is the magnetic Fe prepared in Example 2 3 O 4 @SiO 2 @N,N′-disalicylicylaldehyde-1,2-phenylenediamine-Ni(II).
[0089] The specific synthesis steps are as follows:
[0090] S1: 4,4'-dinitrodiphenyl ether and a protic solvent are mixed to prepare a feed liquid, which is placed in a feed liquid storage tank 2 for standby use.
[0091] S2: Nano-magnetic Fe 3 O 4 @SiO 2 @Salent-Ni(II) composite catalyst is loaded into the reaction tube 7 in the shell-and-tube reactor 6, and nitrogen is introduced to completely replace the air, and then nitrogen is passed for protection. The shell-and-tube reactor 6 is placed in the cavity A in the shell-and-tube reactor jacket 5, preheated to 120°C, the industrial frequency magnetic field generator 4 is turned on, the magnetic field strength is set to 800A / m, the back pressure valve 8 is opened, and then hydrogen is continuously introduced to make the pressure in the shell-and-tube reactor 6 reach 7.0MPa.
[0092] S3: The liquid in the liquid storage tank 2 and the hydrogen in the hydrogen cylinder 1 are mixed in a gas-liquid mixer 3 in a molar ratio of 8:1 by continuous feeding, and then the mixed liquid is subjected to continuous catalytic hydrogenation reaction through a shell-and-tube reactor 6. After a residence time of 250 seconds, the reaction liquid is condensed through a condenser 9, and then the condensed liquid is passed into a gas-liquid separator 10 for gas-liquid separation, and the separated liquid is stored in a receiving tank 11. After the collected separated liquid is cooled to -5 to 0°C, it is crystallized, filtered, and dried to obtain the target product 4,4'-diaminodiphenyl ether shown in formula (II). The calculated product yield is 90.15%, and the product purity (HPLC) is 99.37%.
[0093] Example 9
[0094] A method for continuously catalytic hydrogenation to synthesize 4,4'-diaminodiphenyl ether, the reaction device is shown in the attached Figure 1 .
[0095] The inner diameter of the reactor 7 is 5 mm, the tube length is 1 m, and the catalyst fixed bed filling length is 80 cm; the shell-and-tube reactor 6 is composed of 6 reaction tubes 7 arranged in parallel.
[0096] The proton solvent is a mixed solvent of DMF and ethylene glycol in a volume ratio of 1:1, and the mass amount of the proton solvent is 5 times the mass of the raw material 4,4'-dinitrodiphenyl ether. 3 O 4 @SiO 2 @Salent-Ni(II) composite catalyst is the magnetic Fe prepared in Example 3 3 O 4 @SiO 2 @1,2-Cyclohexylamine bis(3,5-butylsulfate)-Ni(II).
[0097] S1: 4,4'-dinitrodiphenyl ether and a protic solvent are mixed to prepare a feed liquid, which is placed in a feed liquid storage tank 2 for standby use.
[0098] S2: Nano-magnetic Fe 3 O4 @SiO 2 @Salent-Ni(II) composite catalyst is loaded in the fixed bed reaction tube 7 in the shell-and-tube reactor 6, and nitrogen is introduced to completely replace the air, and then nitrogen is passed for protection. The shell-and-tube reactor 6 is placed in the cavity A in the shell-and-tube reactor jacket 5, preheated to 110°C, the industrial frequency magnetic field generator 4 is turned on, the magnetic field strength is set to 1000A / m, the back pressure valve 8 is opened, and then hydrogen is continuously introduced to make the pressure in the shell-and-tube reactor 6 reach 8.0MPa.
[0099] S3: The liquid in the liquid storage tank 2 and the hydrogen in the hydrogen cylinder 1 are mixed in a gas-liquid mixer 3 in a molar ratio of 8:1 by continuous feeding, and then the mixed liquid is subjected to continuous catalytic hydrogenation reaction through a shell-and-tube reactor 6. After a stay of 300 seconds, the reaction liquid is passed into a condenser 9 for condensation, and then the condensate is passed into a gas-liquid separator 10 for gas-liquid separation, and the separated liquid is stored in a receiving tank 11. After the collected separated liquid is cooled to -5 to 0°C, it is crystallized, filtered, and dried to obtain the target product 4,4'-diaminodiphenyl ether shown in formula (II). The calculated product yield is 91.23%, and the product purity (HPLC) is 99.18%.
[0100] Comparative Example 1
[0101] 18Kg4,4'-dinitrodiphenyl ether, 90g Pd / c catalyst with 0.5% Pd content, and 36Kg methanol solvent were added to a 100L hydrogenation reactor with a stirring device. The reactor was replaced with nitrogen three times, and then replaced with hydrogen three times. Steam was introduced into the reactor jacket to heat and heat the reactor. The reaction temperature was controlled at 70°C and the reaction pressure was controlled at 0.4MPa to carry out catalytic hydrogenation reduction reaction. After the reaction was completed, the reaction solution was filtered, cooled and crystallized by a crystallization reactor with a stirring device. Crystallization was completed when the reactor temperature was cooled to below 40°C. Solid 4,4'-diaminodiphenyl ether was obtained by filtration. Subsequently, 4,4'-diaminodiphenyl ether was washed twice with a methanol solvent and dried to obtain 11.63kg of the target product 4,4'-diaminodiphenyl ether with a purity of 98.0% (HPLC) and a yield of 84.1%.
Claims
1. A method for synthesizing 4,4'-diaminodiphenyl ether by continuous catalytic hydrogenation, characterized in that it comprises the following steps: S1: mixing 4,4'-dinitrodiphenyl ether represented by formula (I) with a protic solvent to prepare a feed solution; S2: The nano-magnetic Fe304@SiO2@Salent-Ni(II) composite catalyst is loaded into a shell-and-tube reactor (6), and after nitrogen is introduced to completely replace the air, nitrogen is introduced for protection, the shell-and-tube reactor (6) is preheated, the industrial frequency magnetic field generator (4) is turned on, and then hydrogen is continuously introduced; S3: mixing the feed liquid prepared in step S1 and hydrogen in a gas-liquid mixer (3) in a continuous feeding manner, and then performing a continuous catalytic hydrogenation reaction through a tubular reactor (6), stopping, condensing the reaction liquid through a condenser, separating the gas and liquid, collecting the separated liquid, cooling the separated liquid, crystallizing, filtering, and drying to obtain the target product 4,4'-diaminodiphenyl ether represented by formula (II); The reaction equation is as follows:
2. The method for synthesizing 4,4'-diaminodiphenyl ether by continuous catalytic hydrogenation according to claim 1, characterized in that: In step S1, the inner diameter of the reaction tube (7) of the shell-and-tube reactor (6) is 3 mm to 5 mm, the tube length is 1 m, and the catalyst fixed bed filling length is 60 to 80 cm; the shell-and-tube reactor (6) is composed of 4 to 10 reaction tubes (7) arranged in parallel.
3. The method for synthesizing 4,4'-diaminodiphenyl ether by continuous catalytic hydrogenation according to claim 1, characterized in that: In step S1, the protic solvent is one or a mixture of two or more of DMF, DMAC, ethylene glycol, n-butanol or glycerol; the mass amount of the protic solvent is 5 to 6 times the mass of 4,4'-dinitrodiphenyl ether represented by the raw material formula (I).
4. The method for synthesizing 4,4'-diaminodiphenyl ether by continuous catalytic hydrogenation according to claim 1, characterized in that: In step S2, the preheating temperature of the shell-and-tube reactor is 90-130°C, the magnetic field strength is 500A / m-1200A / m, and after hydrogen is passed, the pressure inside the shell-and-tube reactor (6) is 6.0MPa-8.0MPa.
5. The method for synthesizing 4,4'-diaminodiphenyl ether by continuous catalytic hydrogenation according to claim 1, characterized in that: In step S2, the preparation method of the nanomagnetic Fe304@SiO2@Salent-Ni(II) composite catalyst comprises the following steps: (i) dissolving nickel acetate in anhydrous ethanol to prepare a nickel acetate-ethanol solution, placing a Salen ligand in anhydrous ethanol to prepare a Salen ligand solution, heating, and ultrasonically treating until the mixture is uniformly mixed, then dropping the nickel acetate-ethanol solution into the Salen ligand solution, and after ultrasonic treatment, stopping the reaction, cooling in an ice bath to crystallize, filtering, washing the filter cake with ethanol, and vacuum drying to obtain a Salen-Ni(II) complex; (ii) Take an aqueous solution of magnetic nanoparticles Fe304@SiO2, add Salen-Ni(II) complex to soak it, then pass it into a magnetic separator to separate the magnetic particles, then wash the magnetic particles with distilled water and vacuum dry them to obtain magnetic Fe304@SiO2@Salen-Ni(II).
6. The method for synthesizing 4,4'-diaminodiphenyl ether by continuous catalytic hydrogenation according to claim 5, characterized in that: In step (i), the Salen ligand is N,N'-bis(2-hydroxyphenyl)ethylenediamine, N,N'-disalicylicylaldehyde-1,2-phenylenediamine or 1,2-cyclohexylamine bis(3,5-butyl sulfate).
7. The method for synthesizing 4,4'-diaminodiphenyl ether by continuous catalytic hydrogenation according to claim 5, characterized in that: In step (i), the molar ratio of Salen ligand to nickel acetate is 1:1, the concentration of Salen ligand solution is 10-20wt%, the concentration of nickel acetate-ethanol solution is 4-5wt%, the heating temperature is 40-50°C, the power of ultrasonic treatment is 800-1200W, and the time of ultrasonic treatment is 60-90min.
8. The method for synthesizing 4,4'-diaminodiphenyl ether by continuous catalytic hydrogenation according to claim 5, characterized in that: In step (ii), the mass concentration of the magnetic nanoparticle Fe3O4@SiO2 aqueous solution is 1 mg / mL; The mass ratio of nanoparticles Fe304@SiO2 to Salen-Ni(II) complex is 1:(0.05-0.1), and the immersion time is 5-6h.
9. The method for synthesizing 4,4'-diaminodiphenyl ether by continuous catalytic hydrogenation according to claim 1, characterized in that: In step S3, the molar ratio of hydrogen to 4,4'-dinitrodiphenyl ether represented by formula (I) is 8 to 10:
1.
10. The method for synthesizing 4,4'-diaminodiphenyl ether by continuous catalytic hydrogenation according to claim 1, characterized in that: In step S3, the residence time is 120s to 600s, and the crystallization temperature of the separated liquid is -5 to 0°C.
Citation Information
Cited By
Method for preparing 4, 4 '-diaminodiphenyl ether
CN119390589A
High-activity nickel-based catalyst as well as preparation method and application thereof
CN121648927A