Super-hydrophobic thermal insulation composite material as well as preparation method and application thereof

The super-hydrophobic thermal insulation composite material prepared through high inward emulsion in-situ polymerization technology solves the problems of poor mechanical strength and high production cost of traditional airgel materials. It achieves a combination of low thermal conductivity, super-hydrophobicity and high mechanical properties and is suitable for many applications. kind of application fields.

CN118772322AActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310372392.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-15
Estimated Expiration
2043-04-10

AI Technical Summary

Technical Problem

Traditional airgel insulation materials have problems such as poor mechanical strength, easy powdering, low hydrophobicity and easy hydrolysis, and the preparation requires a complex supercritical carbon dioxide drying process, resulting in high production costs.

Method used

Using raw materials such as styrene, divinylbenzene, functionalized styrene, silane coupling agent modified hollow glass beads and inorganic fillers, superhydrophobic thermal insulation composite materials are prepared through high inward emulsion in-situ polymerization, with a thermal conductivity ≤0.03W/ m.K, water contact angle >150°, and use conventional drying methods during the drying process to reduce production costs.

Benefits of technology

A superhydrophobic thermal insulation composite material with low thermal conductivity, large water contact angle and high mechanical properties has been obtained, which overcomes the shortcomings of traditional aerogel materials and is suitable for thermal insulation, thermal insulation, waterproofing and other fields. It also simplifies the preparation process and reduces the cost of production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772322A_ABST
    Figure CN118772322A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of chemical materials, and discloses a super-hydrophobic thermal insulation composite material and a preparation method and application thereof. The super-hydrophobic thermal insulation composite material is prepared from the following raw materials: styrene, divinyl benzene, functionalized styrene, silane coupling agent modified hollow glass beads, an inorganic filler, an initiator, an emulsifier and water. The heat conductivity coefficient of the super-hydrophobic thermal insulation composite material is smaller than or equal to 0.03 W / m.K, and the water contact angle is larger than 150 degrees. The composite material has excellent thermal insulation performance and super-hydrophobicity; meanwhile, the composite material has the characteristics of relatively high mechanical property and uniform pore size distribution, and has a very good application prospect in the fields of heat insulation, heat preservation, water prevention and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of chemical materials, and in particular to a super-hydrophobic thermal insulation composite material and a preparation method and application thereof. Background Art

[0002] At present, reducing heat loss in high-temperature pipelines is an important part of the general trend of carbon emission reduction. The outside of high-temperature pipelines in refining and chemical enterprises is usually covered with thicker insulation materials. Insulating the pipelines can effectively reduce the company's energy consumption and reduce carbon emissions. However, after a long period of operation, the insulation performance of pipelines using conventional insulation materials such as calcium silicate, composite silicates, rock wool, and slag wool decreases, which increases heat loss and leads to increased energy consumption of the device. On the other hand, the decrease in insulation performance increases the temperature of the outer surface of the pipeline, increasing the possibility of scalding accidents. In addition, materials such as rock wool and aluminum silicate easily absorb water, causing insulation failure, affecting the normal operation of the device.

[0003] Aerogel is a new generation of highly efficient and energy-saving thermal insulation material, which has demonstrated excellent performance in multiple fields such as thermal, acoustic, optical, electrical, and mechanical. Currently, the commercial application of aerogel is mainly based on its high thermal insulation ability, and is used downstream in multiple fields such as petrochemical, thermal pipe network, lithium battery, construction materials, outdoor clothing, aerospace, and military industry.

[0004] For example, patent application CN114100534A discloses a method for preparing a silicon-aluminum binary aerogel composite material, which uses a short-chain alcohol and a long-chain alcohol to mix and reduce the phase separation of the gel material, and then prepares the aerogel material by supercritical drying. Patent CN110282947B discloses a high-strength composite aerogel thermal insulation material and a preparation method thereof, which uses nitrided carbon fibers to be evenly distributed on the surface or inside of the aerogel, effectively improving the mechanical properties of the silica aerogel. In addition, the softness and thermal insulation properties of the aluminum silicate fibers are used to modify the silica aerogel, thereby enhancing its flexibility and reducing its thermal conductivity. Patent application CN113416028A discloses a production process for a water-resistant aerogel thermal insulation material, which uses silica sol, modified graphene, and chitosan as a matrix, and uses modified graphene to modify the aerogel surface with a hydrophobic modifier prepared to obtain a hydrophobic surface, and the hydrophobicity of the material can reach 99%.

[0005] However, the preparation of aerogel materials requires a supercritical carbon dioxide drying process. The wet gel needs to withstand a drying stress of up to 100MPa-200MPa during the drying process. This stress will cause the gel structure to continue to shrink and crack, and easily lead to structural collapse. Therefore, the aerogel material is very easy to powderize and fall off, affecting the service life of the aerogel material. Summary of the invention

[0006] The purpose of the present invention is to overcome the problems of poor mechanical strength, easy pulverization and slagging, low hydrophobicity and easy hydrolysis of traditional aerogel insulation materials in the prior art, and the need for a complex supercritical carbon dioxide drying process and high production cost, and to provide a super-hydrophobic thermal insulation composite material and its preparation method and application.

[0007] In order to achieve the above object, the present invention provides a super hydrophobic thermal insulation composite material on the one hand, wherein the raw materials for preparing the super hydrophobic thermal insulation composite material contain styrene, divinylbenzene, functionalized styrene, silane coupling agent modified hollow glass microspheres, inorganic filler, initiator, emulsifier and water;

[0008] The thermal conductivity of the super-hydrophobic thermal insulation composite material is ≤0.03 W / mK, and the water contact angle is >150°.

[0009] Preferably, the compressive strength of the super-hydrophobic thermal insulation composite material is ≥1 MPa.

[0010] Preferably, the most probable pore size of the super hydrophobic thermal insulation composite material is 10-200 nm.

[0011] Preferably, the inorganic filler is selected from one or more of silicon carbide, titanium nitride, titanium dioxide, worm graphite, graphene and carbon black.

[0012] Preferably, the silane coupling agent is selected from one or more of tetraethoxysilane, vinyltriethoxysilane, aminopropyltrimethoxysilane, glycidyloxypropyltrimethoxysilane, vinyltrimethoxysilane and γ-methacryloxypropyltrimethoxysilane.

[0013] Preferably, the functionalized styrene is selected from one or more of N,N-dimethylstyrene, N,N-diethylstyrene, N,N-diphenylstyrene, methoxystyrene, methylthiostyrene, p-chlorostyrene and p-bromostyrene.

[0014] Preferably, the weight ratio of styrene, divinylbenzene, functionalized styrene, emulsifier, silane coupling agent modified hollow glass microspheres, inorganic filler and initiator is 1:0.5-6:0.1-3:0.5-3:0.01-0.5:0.01-0.1:0.2-1, and the weight ratio of water to styrene is 20-100:1.

[0015] A second aspect of the present invention provides a method for preparing a super-hydrophobic thermal insulation composite material, the method comprising the following steps:

[0016] (1) mixing styrene, divinylbenzene, functionalized styrene, an emulsifier and water to obtain a mixture A;

[0017] (2) mixing mixed material A, hollow glass microspheres modified by silane coupling agent and inorganic filler to obtain mixed material B;

[0018] (3) Mixed material B is mixed with an initiator solution containing an initiator and water, followed by reaction, and then washing and drying.

[0019] Preferably, the inorganic filler is selected from one or more of silicon carbide, titanium nitride, titanium dioxide, worm graphite, graphene and carbon black.

[0020] Preferably, the silane coupling agent is selected from one or more of tetraethoxysilane, vinyltriethoxysilane, aminopropyltrimethoxysilane, glycidyloxypropyltrimethoxysilane, vinyltrimethoxysilane and γ-methacryloxypropyltrimethoxysilane.

[0021] Preferably, the functionalized styrene is selected from one or more of N,N-dimethylstyrene, N,N-diethylstyrene, N,N-diphenylstyrene, methoxystyrene, methylthiostyrene, p-chlorostyrene and p-bromostyrene.

[0022] Preferably, the weight ratio of styrene, divinylbenzene, functionalized styrene, emulsifier, silane coupling agent modified hollow glass microspheres, inorganic filler and initiator is 1:0.5-6:0.1-3:0.5-3:0.01-0.5:0.01-0.1:0.2-1.

[0023] Preferably, the weight ratio of the sum of the amounts of water used in step (1) and step (3) to styrene is 20-100:1;

[0024] Preferably, in step (1), the weight ratio of water to styrene is 20-80:1.

[0025] Preferably, the emulsifier is selected from one or more of Tween 80, sodium dodecylbenzene sulfonate and polyvinyl alcohol.

[0026] Preferably, the initiator is selected from potassium persulfate, ammonium persulfate or hydrogen peroxide.

[0027] Preferably, in step (3), the reaction conditions include: temperature of 65-85° C. and reaction time of 3-6 h.

[0028] Preferably, in step (3), the drying is vacuum drying.

[0029] The third aspect of the present invention provides a super-hydrophobic thermal insulation composite material prepared by the method described above.

[0030] A fourth aspect of the present invention provides use of the super-hydrophobic thermal insulation composite material as described above or the super-hydrophobic thermal insulation composite material prepared by the method as described above in the field of heat insulation, thermal insulation, sound insulation or waterproofing.

[0031] Compared with the prior art, the present invention has the following advantages:

[0032] 1. The present invention provides a super-hydrophobic thermal insulation composite material, the thermal conductivity of the composite material is ≤0.03W / mK, and the water contact angle is >150°, indicating that the composite material has excellent thermal insulation performance and super-hydrophobicity; at the same time, it has high mechanical properties and uniform pore size distribution, and has good application prospects in the fields of heat insulation, thermal insulation, waterproofing, etc.

[0033] 2. In the method described in the present invention, styrene, divinylbenzene and functionalized styrene are used as monomers, and silane coupling agent is added to modify hollow glass microspheres and inorganic fillers. The prepared composite material has excellent thermal insulation performance and super hydrophobicity through the mutual coordination between the raw materials; it has high mechanical properties and uniform pore size distribution. At the same time, based on the selection of raw materials, various conventional drying methods in the field can be used to complete drying during the preparation process, overcoming the high production cost and harsh conditions caused by the need to use a complex supercritical carbon dioxide drying process for traditional aerogel materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 is a photograph of the product prepared in Example 1;

[0035] Figure 2 This is a SEM characterization result diagram of the product prepared in Example 2;

[0036] Figure 3 This is a water contact angle test photograph of the product prepared in Example 1;

[0037] Figure 4 It is the BET pore size distribution diagram of the products prepared in Examples 1-3. DETAILED DESCRIPTION

[0038] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0039] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0040] On one hand, the present invention provides a super-hydrophobic thermal insulation composite material, wherein the raw materials for preparing the super-hydrophobic thermal insulation composite material include styrene, divinylbenzene, functionalized styrene, silane coupling agent modified hollow glass microspheres, inorganic filler, initiator, emulsifier and water;

[0041] The thermal conductivity of the super-hydrophobic thermal insulation composite material is ≤0.03 W / mK, and the water contact angle is >150°.

[0042] The super-hydrophobic thermal insulation composite material of the present invention has excellent thermal insulation performance and super-hydrophobic performance, and also has the characteristics of high mechanical properties and uniform pore size distribution, and has good application prospects in the fields of heat insulation, thermal insulation, waterproofing, etc.

[0043] In a preferred embodiment, the compressive strength of the super-hydrophobic thermal insulation composite material is ≥1 MPa.

[0044] In a preferred embodiment, the maximum pore size of the super hydrophobic thermal insulation composite material is 10-200 nm.

[0045] In the present invention, the most probable pore size refers to the pore size value of the pore with the highest probability in a series of pores in the material. In the test process, the pore size corresponding to the peak value appearing on the differential distribution curve of the pore size obtained by BET test is usually the most probable pore size.

[0046] In a preferred embodiment, the inorganic filler is selected from one or more of silicon carbide, titanium nitride, titanium dioxide, worm graphite, graphene and carbon black.

[0047] In order to further improve the thermal insulation performance, mechanical properties and hydrophobicity of the super-hydrophobic thermal insulation composite material, in a preferred embodiment, the silane coupling agent is selected from one or more of tetraethoxysilane, vinyl triethoxysilane, aminopropyl trimethoxysilane, glycidyloxypropyl trimethoxysilane, vinyl trimethoxysilane and γ-methacryloxypropyl trimethoxysilane.

[0048] In a specific embodiment, the silane coupling agent is γ-methacryloxypropyltrimethoxysilane (KH570).

[0049] In the present invention, the silane coupling agent modified hollow glass microspheres are obtained by modifying hollow glass microspheres with a silane coupling agent.

[0050] In a preferred embodiment, in the raw materials for preparing the silane coupling agent-modified hollow glass microspheres, the weight ratio of the silane coupling agent to the hollow glass microspheres is 0.01-0.03:1; specifically, it can be 0.01:1, 0.0.2:1 or 0.03:1.

[0051] In the present invention, the method for preparing the silane coupling agent modified hollow glass microspheres comprises the following steps: mixing the hollow glass microspheres with a solvent, then mixing with a silane coupling agent, then reacting, then filtering and drying.

[0052] Preferably, the solvent is ethanol or ethyl acetate.

[0053] Preferably, the reaction conditions include: temperature of 40-60°C, time of 0.5-2h; specifically, the reaction temperature may be 40°C, 45°C, 50°C, 55°C or 60°C; the reaction time may be 0.5h, 1h, 1.5h or 2h.

[0054] In order to further improve the thermal insulation performance, mechanical properties and hydrophobicity of the super-hydrophobic thermal insulation composite material, in a preferred embodiment, the functionalized styrene is selected from one or more of N,N-dimethylstyrene, N,N-diethylstyrene, N,N-diphenylstyrene, methoxystyrene, methylthiostyrene, p-chlorostyrene and p-bromostyrene.

[0055] In order to further improve the thermal insulation performance, mechanical properties and hydrophobicity of the super-hydrophobic thermal insulation composite material, the ratio of each component in the raw material can be reasonably controlled. In a preferred embodiment, the weight ratio of styrene, divinylbenzene, functionalized styrene, emulsifier, silane coupling agent modified hollow glass microspheres, inorganic filler and initiator in the raw material is 1: 0.5-6: 0.1-3: 0.5-3: 0.01-0.5: 0.01-0.1: 0.2-1; the weight ratio of water to styrene is 20-100: 1.

[0056] In a specific embodiment, the weight ratio of styrene to divinylbenzene can be 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5 or 1:6.

[0057] In a specific embodiment, the weight ratio of styrene to functionalized styrene can be 1:0.1, 1:0.2, 1:0.3, 1:0.5, 1:0.6, 1:0.8, 1:1, 1:1.2, 1:1.4, 1:1.5, 1:1.8, 1:2, 1:2.5 or 1:3.

[0058] In a specific embodiment, the weight ratio of styrene to emulsifier can be 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2, 1:1.5, 1:2, 1:2.5 or 1:3.

[0059] In a specific embodiment, the weight ratio of styrene to silane coupling agent modified hollow glass microspheres can be 1:0.01, 1:0.02, 1:0.03, 1:0.04, 1:0.05, 1:0.08, 1:0.1, 1:0.15, 1:0.2, 1:0.25, 1:0.31:, 0.36, 1:0.4, 1:0.45 or 1:0.5.

[0060] In a specific embodiment, the weight ratio of styrene to the inorganic filler can be 1:0.01, 1:0.02, 1:0.03, 1:0.04, 1:0.05, 1:0.06, 1:0.07, 1:0.08, 1:0.09 or 1:0.1.

[0061] In a specific embodiment, the weight ratio of styrene to initiator can be 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9 or 1:1.

[0062] In a specific embodiment, the weight ratio of water to styrene can be 20:1, 25:1, 30:1, 35:1, 40:1, 45:1, 50:1, 55:1, 60:1, 65:1, 70:1, 75:1, 80:1, 85:1, 90:1, 95:1 or 100:1.

[0063] A second aspect of the present invention provides a method for preparing a super-hydrophobic thermal insulation composite material, the method comprising the following steps:

[0064] (1) mixing styrene, divinylbenzene, functionalized styrene, an emulsifier and water to obtain a mixture A;

[0065] (2) Mixing a mixture A, hollow glass microspheres modified by a silane coupling agent, and an inorganic filler to obtain a mixture B;

[0066] (3) Mixed material B is mixed with an initiator solution containing an initiator and water, followed by reaction, and then washing and drying.

[0067] In the method described in the present invention, styrene, divinylbenzene and functionalized styrene are used as monomers, hollow glass microspheres and inorganic fillers are modified by silane coupling agents, and then a super-hydrophobic thermal insulation composite aerogel material is obtained by high inward emulsion in-situ polymerization. The material has high mechanical properties and thermal insulation properties, a thermal conductivity of ≤0.03W / mK, a compressive strength of ≥1MPa, and a super-hydrophobic surface, a water contact angle of >150°, a material with a maximum pore size of 10-200nm, and a uniform pore size distribution.

[0068] In order to further improve the thermal insulation performance, mechanical properties and hydrophobicity of the super-hydrophobic thermal insulation composite material, in a preferred embodiment, the inorganic filler is selected from one or more of silicon carbide, titanium nitride, titanium dioxide, worm graphite, graphene and carbon black.

[0069] In order to further improve the thermal insulation performance, mechanical properties and hydrophobicity of the super-hydrophobic thermal insulation composite material, in a preferred embodiment, the silane coupling agent is selected from one or more of tetraethoxysilane, vinyl triethoxysilane, aminopropyl trimethoxysilane, glycidyl ether oxypropyl trimethoxysilane, vinyl trimethoxysilane and γ-methacryloxypropyl trimethoxysilane.

[0070] In a preferred embodiment, in the raw materials for preparing the silane coupling agent-modified hollow glass microspheres, the weight ratio of the silane coupling agent to the hollow glass microspheres is 0.01-0.03:1; specifically, it can be 0.01:1, 0.0.2:1 or 0.03:1.

[0071] In the present invention, the method for preparing the silane coupling agent modified hollow glass microspheres comprises the following steps: mixing the hollow glass microspheres with a solvent, then mixing with a silane coupling agent, then reacting, then filtering and drying.

[0072] Preferably, the solvent is ethanol or ethyl acetate.

[0073] Preferably, the hollow glass microspheres and the solvent are mixed by ultrasonic mixing; more preferably, the ultrasonic mixing time is 1 hour.

[0074] Preferably, the reaction conditions include: temperature of 40-60°C, time of 0.5-2h; specifically, the reaction temperature may be 40°C, 45°C, 50°C, 55°C or 60°C; the reaction time may be 0.5h, 1h, 1.5h or 2h.

[0075] In a specific embodiment, the silane coupling agent is γ-methacryloxypropyltrimethoxysilane (KH570).

[0076] In the method described in the present invention, by using styrene, divinylbenzene and functionalized styrene as monomers, it is beneficial to increase the dispersibility of hollow microspheres and inorganic fillers in the polymer matrix, and improve the thermal insulation performance and infrared radiation barrier properties of the material.

[0077] In a preferred embodiment, the functionalized styrene is selected from one or more of N,N-dimethylstyrene, N,N-diethylstyrene, N,N-diphenylstyrene, methoxystyrene, methylthiostyrene, p-chlorostyrene and p-bromostyrene.

[0078] In order to further improve the thermal insulation performance, mechanical properties and hydrophobicity of the super-hydrophobic thermal insulation composite material, the ratio of the raw materials used in the preparation process can be reasonably controlled. In a preferred embodiment, the weight ratio of styrene, divinylbenzene, functionalized styrene, emulsifier, silane coupling agent modified hollow glass microspheres, inorganic filler and initiator is 1:0.5-6:0.1-3:0.5-3:0.01-0.5:0.01-0.1:0.2-1.

[0079] In a specific embodiment, the weight ratio of styrene to divinylbenzene can be 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5 or 1:6.

[0080] In a specific embodiment, the weight ratio of styrene to functionalized styrene can be 1:0.1, 1:0.2, 1:0.3, 1:0.5, 1:0.6, 1:0.8, 1:1, 1:1.2, 1:1.4, 1:1.5, 1:1.8, 1:2, 1:2.5 or 1:3.

[0081] In a specific embodiment, the weight ratio of styrene to emulsifier can be 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2, 1:1.5, 1:2, 1:2.5 or 1:3.

[0082] In a specific embodiment, the weight ratio of styrene to silane coupling agent modified hollow glass microspheres can be 1:0.01, 1:0.02, 1:0.03, 1:0.04, 1:0.05, 1:0.08, 1:0.1, 1:0.15, 1:0.2, 1:0.25, 1:0.31:, 0.36, 1:0.4, 1:0.45 or 1:0.5.

[0083] In a specific embodiment, the weight ratio of styrene to the inorganic filler can be 1:0.01, 1:0.02, 1:0.03, 1:0.04, 1:0.05, 1:0.06, 1:0.07, 1:0.08, 1:0.09 or 1:0.1.

[0084] In a specific embodiment, the weight ratio of styrene to initiator can be 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9 or 1:1.

[0085] In a preferred embodiment, the weight ratio of the sum of the amounts of water used in step (1) and step (3) to styrene is 20-100:1; wherein the amount of water used in step (3) refers to the weight of water contained in the initiator solution in step (3).

[0086] More preferably, in step (1), the weight ratio of water to styrene is 20-80:1; specifically, it can be 20:1, 25:1, 30:1, 35:1, 40:1, 45:1, 50:1, 55:1, 60:1, 65:1, 70:1, 75:1 or 80:1.

[0087] More preferably, in step (3), the weight ratio of water to styrene is 1-10:1.

[0088] In the method of the present invention, there is no special requirement for the selection of emulsifier, and it can be any emulsifier conventionally used in emulsion polymerization in the art. In a preferred embodiment, the emulsifier is selected from one or more of Tween 80, sodium dodecylbenzene sulfonate and polyvinyl alcohol.

[0089] In a preferred embodiment, the initiator is selected from potassium persulfate, ammonium persulfate or hydrogen peroxide.

[0090] In a preferred embodiment, in step (1), the mixing may be stirring mixing.

[0091] In a preferred embodiment, in step (2), the mixing method is stirring and mixing. Further preferably, the stirring and mixing temperature is 25-35° C., and the stirring and mixing time is 30-60 min.

[0092] In a preferred embodiment, in step (3), the specific process of mixing the mixed material B with the initiator solution includes: adding the initiator solution dropwise to the mixed material B under stirring; more preferably, the adding time is 20-40 min.

[0093] In a specific embodiment, the initiator solution is added dropwise using a constant pressure low liquid funnel.

[0094] In a preferred embodiment, in step (3), the initiator solution further contains calcium chloride, and the presence of calcium chloride is conducive to the dissolution of the initiator. There is no special requirement for the amount of calcium chloride used, and it can be a conventional amount in the art. Further preferably, in the initiator solution, the ratio of the weight of calcium chloride to the sum of the weight of calcium chloride and water is 1-3%.

[0095] In a specific embodiment, the initiator solution is prepared by mixing water and calcium chloride, and then adding the initiator.

[0096] In a preferred embodiment, in step (3), the reaction conditions include: temperature of 65-85°C and reaction time of 3-6h. Specifically, the temperature may be 65°C, 70°C, 75°C, 80°C or 85°C; and the reaction time may be 3h, 3.5h, 4h, 4.5h, 5h, 5.5h or 6h.

[0097] In a preferred embodiment, the washing agent used in the washing is ethanol, which can remove water and residual monomers.

[0098] In the method described in the present invention, in step (3), the washed material can be dried by any conventional drying method in the art, thus overcoming the problem of high production cost caused by the need to use a complex supercritical carbon dioxide drying process for traditional aerogel materials, and having the characteristics of simple process and low cost.

[0099] In a preferred embodiment, in step (3), the drying is vacuum drying.

[0100] In a specific embodiment, the process of preparing the super hydrophobic thermal insulation composite material comprises the following steps:

[0101] (1) stirring and mixing styrene, divinylbenzene, functionalized styrene, an emulsifier and water to obtain a mixture A;

[0102] (2) mixing the mixed material A, the silane coupling agent-modified hollow glass microspheres and the inorganic filler to obtain a mixed material B;

[0103] (3) Under stirring, an initiator solution is added dropwise to the mixed material B, followed by reaction, and then washing and vacuum drying. The initiator solution contains an initiator, water and calcium chloride.

[0104] The third aspect of the present invention provides a super-hydrophobic thermal insulation composite material prepared by the method described above.

[0105] A fourth aspect of the present invention provides use of the super-hydrophobic thermal insulation composite material as described above or the super-hydrophobic thermal insulation composite material prepared by the method as described above in the field of heat insulation, thermal insulation, sound insulation or waterproofing.

[0106] For example, the insulation layer structure between power batteries, the waterproof insulation layer of low-temperature cooling pipes, etc.

[0107] The present invention will be described in detail below through examples, but the protection scope of the present invention is not limited thereto.

[0108] Unless otherwise specified, the reagents used in the following examples and comparative examples are all commercially available products.

[0109] Example 1

[0110] The preparation of the super-hydrophobic thermal insulation composite material S1 comprises the following steps:

[0111] (1) 2 g of styrene, 6 g of divinylbenzene, functionalized styrene (2 g of N,N-dimethylstyrene), 3 g of emulsifier (Tween 80) and 80 g of water were stirred and mixed to obtain a mixture A;

[0112] (2) Mixture A, 0.3 g of silane coupling agent-modified hollow glass microspheres a1 and 0.1 g of inorganic filler (silicon carbide) were stirred for 30 min at a temperature of 25° C. to obtain mixture B;

[0113] (3) under stirring, using a constant pressure dropping funnel to drop the initiator solution into the mixed material B, the dropping time is 30 minutes, and after sealing, the polymerization reaction is carried out at 80° C. After the reaction for 6 hours, a solid block product is obtained, which is then washed with ethanol and then vacuum dried; the initiator solution is composed of 1g initiator (potassium persulfate), 9.9g water and 0.1g calcium chloride;

[0114] Among them, the weight ratio of styrene, divinylbenzene, functionalized styrene, emulsifier, silane coupling agent modified hollow glass microspheres a1, inorganic filler and initiator is 1:3:1:1.5:0.15:0.05:0.5; the weight ratio of water used in step (1) to styrene is 40:1; and the ratio of the weight of water contained in the initiator solution to the weight of styrene in step (3) is 4.95:1.

[0115] The preparation process of the silane coupling agent modified hollow glass microsphere a1 includes the following steps: ultrasonically mixing the hollow glass microsphere powder with anhydrous ethanol for 1 hour, then mixing with a silane coupling agent (KH570), then reacting at 60°C for 1 hour, then filtering, and then drying the filter residue at 100°C for 24 hours; wherein the weight ratio of the hollow glass microsphere powder, anhydrous ethanol and silane coupling agent is 1:100:0.02.

[0116] Example 2

[0117] The preparation of the super-hydrophobic thermal insulation composite material S2 comprises the following steps:

[0118] (1) 3 g of styrene, 6 g of divinylbenzene, functionalized styrene (1 g of N,N-diethylstyrene), 4 g of an emulsifier (sodium dodecylbenzene sulfonate) and 80 g of water were stirred and mixed to obtain a mixture A;

[0119] (2) Mixture A, 0.1 g of silane coupling agent-modified hollow glass microspheres a1 and 0.1 g of inorganic filler (titanium dioxide) were stirred for 30 min at a temperature of 25° C. to obtain mixture B;

[0120] (3) under stirring, the initiator solution was added dropwise to the mixture B using a constant pressure dropping funnel for 40 min, and the mixture was sealed and polymerized at 70° C. After 8 hours of reaction, a solid block product was obtained, which was then washed with ethanol and then vacuum dried; the initiator solution consisted of 1.5 g initiator (ammonium persulfate), 9.9 g water and 0.1 g calcium chloride;

[0121] Among them, the weight ratio of styrene, divinylbenzene, functionalized styrene, emulsifier, silane coupling agent modified hollow glass microspheres a1, inorganic filler and initiator is 3:6:1:4:0.1:0.1:1.5; the weight ratio of water used in step (1) to styrene is 80:3; and the ratio of the weight of water contained in the initiator solution in step (3) to the weight of styrene is 3.3:1.

[0122] Example 3

[0123] The preparation of the super-hydrophobic thermal insulation composite material S3 comprises the following steps:

[0124] (1) 5 g of styrene, 4 g of divinylbenzene, functionalized styrene (1 g of N,N-diphenylstyrene), 3 g of an emulsifier (polyvinyl alcohol) and 100 g of water were stirred and mixed to obtain a mixture A;

[0125] (2) Mixture A, 0.2 g of silane coupling agent-modified hollow glass microspheres a1 and 0.05 g of inorganic filler (titanium nitride) were stirred for 30 min at a temperature of 25° C. to obtain mixture B;

[0126] (3) under stirring, using a constant pressure dropping funnel to drop the initiator solution into the mixed material B, the dropping time is 40 minutes, and after sealing, the polymerization reaction is carried out at 80° C. After the reaction for 6 hours, a solid block product is obtained, which is then washed with ethanol and then vacuum dried; the initiator solution is composed of 2g initiator (potassium persulfate), 9.9g water and 0.1g calcium chloride;

[0127] Among them, the weight ratio of styrene, divinylbenzene, functionalized styrene, emulsifier, silane coupling agent modified hollow glass microspheres a1, inorganic filler and initiator is 1:0.8:0.2:0.6:0.04:0.01:0.4; the weight ratio of water used in step (1) to styrene is 20:1; the ratio of the weight of water contained in the initiator solution in step (3) to the weight of styrene is 1.98:1.

[0128] Example 4

[0129] The preparation of the super-hydrophobic thermal insulation composite material S4 comprises the following steps:

[0130] (1) 1 g of styrene, 6 g of divinylbenzene, functionalized styrene (3 g of N,N-diethylstyrene), 3 g of an emulsifier (Tween 80) and 80 g of water were stirred and mixed to obtain a mixture A;

[0131] (2) Mixture A, 0.5 g of silane coupling agent-modified hollow glass microspheres a1 and 0.1 g of inorganic filler (titanium nitride) were stirred for 30 min at a temperature of 25° C. to obtain mixture B;

[0132] (3) under stirring, the initiator solution was added dropwise to the mixture B using a constant pressure dropping funnel for 20 min, and the mixture was sealed and polymerized at 80° C. After 6 hours of reaction, a solid block product was obtained, which was then washed with ethanol and then vacuum dried; the initiator solution contained 1 g of initiator (potassium persulfate), 9.9 g of water and 0.1 g of calcium chloride;

[0133] Among them, the weight ratio of styrene, divinylbenzene, functionalized styrene, emulsifier, silane coupling agent modified hollow glass microspheres a1, inorganic filler and initiator is 1:6:3:3:0.5:0.1:1; the weight ratio of the amount of water used in step (1) to the amount of styrene used is 80:1; and the ratio of the weight of water contained in the initiator solution in step (3) to the weight of styrene is 9.9:1.

[0134] Example 5

[0135] The preparation of the super-hydrophobic thermal insulation composite material S5 comprises the following steps:

[0136] (1) 4 g of styrene, 4 g of divinylbenzene, functionalized styrene (2 g of methoxystyrene), 3 g of emulsifier (Tween 80) and 80 g of water were stirred and mixed to obtain a mixture A;

[0137] (2) Mixture A, 0.1 g of silane coupling agent-modified hollow glass microspheres a1 and 0.1 g of inorganic filler (graphene) were stirred for 30 min at a temperature of 25° C. to obtain mixture B;

[0138] (3) under stirring, the initiator solution was added dropwise to the mixture B using a constant pressure dropping funnel for 30 min, and the mixture was sealed and polymerized at 80° C. After 6 hours of reaction, a solid block product was obtained, which was then washed with ethanol and then vacuum dried; the initiator solution contained 1 g of initiator (potassium persulfate), 9.9 g of water and 0.1 g of calcium chloride;

[0139] Among them, the weight ratio of styrene, divinylbenzene, functionalized styrene, emulsifier, silane coupling agent modified hollow glass microspheres a1, inorganic filler and initiator is 1:1:0.5:0.75:0.025:0.025:0.25; the weight ratio of water used in step (1) to styrene is 20:1; the ratio of the weight of water contained in the initiator solution to the weight of styrene in step (3) is 2.475:1.

[0140] Example 6

[0141] The preparation of the super hydrophobic thermal insulation composite material S6 comprises the following steps:

[0142] (1) 3 g of styrene, 5 g of divinylbenzene, functionalized styrene (2 g of p-bromostyrene), 3 g of an emulsifier (polyvinyl alcohol) and 60 g of water were stirred and mixed to obtain a mixture A;

[0143] (2) Mixture A, 0.3 g of silane coupling agent-modified hollow glass microspheres a1 and 0.1 g of inorganic filler (carbon black) were stirred for 30 min at a temperature of 25° C. to obtain mixture B;

[0144] (3) under stirring, the initiator solution was added dropwise to the mixture B using a constant pressure dropping funnel for 30 min, and the mixture was sealed and polymerized at 80° C. After 6 hours of reaction, a solid block product was obtained, which was then washed with ethanol and then vacuum dried; the initiator solution contained 1 g of initiator (potassium persulfate), 9.9 g of water and 0.1 g of calcium chloride;

[0145] Among them, the weight ratio of styrene, divinylbenzene, functionalized styrene, emulsifier, silane coupling agent modified hollow glass microspheres a1, inorganic filler and initiator is 3:5:2:3:0.3:0.1:1; the weight ratio of the amount of water used in step (1) to the amount of styrene used is 20:1; and the ratio of the weight of water contained in the initiator solution in step (3) to the weight of styrene is 3.3:1.

[0146] Example 7

[0147] The preparation of the super-hydrophobic thermal insulation composite material S7 comprises the following steps:

[0148] (1) 2 g of styrene, 6 g of divinylbenzene, functionalized styrene (2 g of methylthiostyrene), 3 g of emulsifier (Tween 80) and 80 g of water were stirred and mixed to obtain a mixture A;

[0149] (2) Mixture A, 0.3 g of silane coupling agent-modified hollow glass microspheres a2 and 0.1 g of inorganic filler (silicon carbide) were stirred for 30 min at a temperature of 25° C. to obtain mixture B;

[0150] (3) under stirring, the initiator solution was added dropwise to the mixture B using a constant pressure dropping funnel for 30 min, and the mixture was sealed and polymerized at 80° C. After 6 hours of reaction, a solid block product was obtained, which was then washed with ethanol and then vacuum dried; the initiator solution contained 1 g of initiator (potassium persulfate), 9.9 g of water and 0.1 g of calcium chloride;

[0151] Among them, the weight ratio of styrene, divinylbenzene, functionalized styrene, emulsifier, silane coupling agent modified hollow glass microspheres a2, inorganic filler and initiator is 1:3:1:1.5:0.15:0.05:0.5; the weight ratio of the amount of water used in step (1) to the amount of styrene used is 40:1; the ratio of the weight of water contained in the initiator solution in step (3) to the weight of styrene is 4.95:1.

[0152] The preparation process of the silane coupling agent modified hollow glass microsphere a2 includes the following steps: ultrasonically mixing the hollow glass microsphere powder with anhydrous ethanol for 1 hour, then mixing with the silane coupling agent (vinyl triethoxysilane), then reacting at 60°C for 1 hour, then filtering, and then drying the filter residue at 100°C for 24 hours; wherein the weight ratio of the hollow glass microsphere powder, anhydrous ethanol and silane coupling agent is 1:100:0.02.

[0153] Example 8

[0154] The preparation of the super hydrophobic thermal insulation composite material S8 comprises the following steps:

[0155] (1) 2 g of styrene, 6 g of divinylbenzene, functionalized styrene (1 g of methoxystyrene + 1 g of methylthiostyrene), 3 g of an emulsifier (Tween 80) and 80 g of water were stirred and mixed to obtain a mixture A;

[0156] (2) Mixture A, 0.3 g of silane coupling agent-modified hollow glass microspheres a2 and 0.1 g of inorganic filler (silicon carbide) were stirred for 30 min at a temperature of 25° C. to obtain mixture B;

[0157] (3) under stirring, the initiator solution was added dropwise to the mixture B using a constant pressure dropping funnel for 30 min, and the mixture was sealed and polymerized at 80° C. After 6 hours of reaction, a solid block product was obtained, which was then washed with ethanol and then vacuum dried; the initiator solution contained 1 g of initiator (potassium persulfate), 9.9 g of water and 0.1 g of calcium chloride;

[0158] Among them, the weight ratio of styrene, divinylbenzene, functionalized styrene, emulsifier, silane coupling agent modified hollow glass microspheres a3, inorganic filler and initiator is 1:3:1:1.5:0.15:0.05:0.5; the weight ratio of the amount of water used in step (1) to the amount of styrene used is 40:1; and the ratio of the weight of water contained in the initiator solution in step (3) to the weight of styrene is 4.95:1.

[0159] The preparation process of the silane coupling agent modified hollow glass microsphere a3 comprises the following steps: mixing the hollow glass microsphere powder with anhydrous ethanol, and then mixing with the silane coupling agent (KH570), and then reacting at 60° C. for 1 hour, and then filtering, and then drying the filter residue at 100° C. for 24 hours; wherein the weight ratio of the hollow glass microsphere powder, anhydrous ethanol and silane coupling agent is 1:100:0.03.

[0160] Example 9

[0161] The preparation of the super-hydrophobic thermal insulation composite material S9 comprises the following steps:

[0162] (1) 2 g of styrene, 6 g of divinylbenzene, functionalized styrene (1 g of methoxystyrene + 1 g of N,N-dimethylstyrene), 3 g of an emulsifier (polyvinyl alcohol) and 60 g of water were stirred and mixed to obtain a mixture A;

[0163] (2) Mixture A, 0.3 g of silane coupling agent-modified hollow glass microspheres a1 and 0.1 g of inorganic filler (worm graphite) were stirred for 30 min at a temperature of 25° C. to obtain mixture B;

[0164] (3) under stirring, the initiator solution was added dropwise to the mixture B using a constant pressure dropping funnel for 30 min, and the mixture was sealed and polymerized at 80° C. After 6 hours of reaction, a solid block product was obtained, which was then washed with ethanol and then vacuum dried; the initiator solution contained 1 g of initiator (hydrogen peroxide), 9.7 g of water and 0.3 g of calcium chloride;

[0165] Among them, the weight ratio of styrene, divinylbenzene, functionalized styrene, emulsifier, silane coupling agent modified hollow glass microspheres a1, inorganic filler and initiator is 1:3:1:1.5:0.15:0.05:0.5; the weight ratio of water used in step (1) to styrene is 30:1; and the ratio of the weight of water contained in the initiator solution in step (3) to the weight of styrene is 4.85:1.

[0166] Example 10

[0167] The preparation of the super-hydrophobic thermal insulation composite material S10 comprises the following steps:

[0168] (1) 2 g of styrene, 5 g of divinylbenzene, functionalized styrene (3 g of p-chlorostyrene), 3 g of an emulsifier (polyvinyl alcohol) and 60 g of water were stirred and mixed to obtain a mixture A;

[0169] (2) Mixture A, 0.3 g of silane coupling agent-modified hollow glass microspheres a1 and 0.1 g of inorganic filler (silicon carbide) were stirred for 30 min at a temperature of 25° C. to obtain mixture B;

[0170] (3) under stirring, the initiator solution was added dropwise to the mixture B using a constant pressure dropping funnel for 30 min, and the mixture was sealed and polymerized at 80° C. After 6 hours of reaction, a solid block product was obtained, which was then washed with ethanol and then vacuum dried; the initiator solution contained 1 g of initiator (potassium persulfate), 9.9 g of water and 0.1 g of calcium chloride;

[0171] Among them, the weight ratio of styrene, divinylbenzene, functionalized styrene, emulsifier, silane coupling agent modified hollow glass microspheres a1, inorganic filler and initiator is 1:2.5:1.5:1.5:0.15:0.05:0.5; the weight ratio of water used in step (1) to styrene is 20:1; the ratio of the weight of water contained in the initiator solution in step (3) to the weight of styrene is 4.95:1.

[0172] Comparative Example 1

[0173] The method described in Example 1 is used for implementation, except that the hollow glass microsphere a1 is not modified with a silane coupling agent.

[0174] Comparative Example 2

[0175] The method described in Example 1 was followed, except that no functionalized styrene (N,N-dimethylstyrene) was used.

[0176] Comparative Example 3

[0177] The process was carried out as described in Example 1, except that no divinylbenzene was used.

[0178] Comparative Example 4

[0179] The method described in Example 1 was followed, except that no inorganic filler was used.

[0180] Comparative Example 5

[0181] The method described in Example 1 was used, except that the hollow glass microsphere powder of the same weight was used to replace the silane coupling agent-modified hollow glass microsphere a1.

[0182] Test Example 1

[0183] The product prepared in Example 1 was placed on the pistil and photographed as shown in the following figure. Figure 1 shown.

[0184] Depend on Figure 1 It can be seen that the product prepared in Example 1 is very light and can be placed on the stamens without crushing the stamens.

[0185] The product prepared in Example 2 was characterized by SEM, and the results were as follows: Figure 2 shown.

[0186] Depend on Figure 2 It can be seen that the product prepared in Example 2 is a nanoporous material with low thermal conductivity and is suitable for use as a thermal insulation material.

[0187] Test Example 2

[0188] The compressive strength of the products obtained in the embodiments and comparative examples was tested by the method described in the national standard GB / T 8813-2020. The results are shown in Table 1.

[0189] Table 1

[0190]

[0191]

[0192] It can be seen from Table 1 that, except for Comparative Example 3, the products all have good mechanical properties, and the compressive strength is greater than 1 MPa, indicating that they have strong ability to resist external force damage.

[0193] Test Example 3

[0194] The thermal conductivity of the products obtained in the examples and comparative examples was tested using the method described in the national standard GB / T 10294-2008. The results are shown in Table 2.

[0195] Table 2

[0196] serial number Thermal conductivity W / mK serial number Thermal conductivity W / mK Example 1 0.018 Example 9 0.033 Example 2 0.027 Example 10 0.038 Example 3 0.021 Comparative Example 1 0.058 Example 4 0.022 Comparative Example 2 0.066 Example 5 0.028 Comparative Example 3 0.077 Example 6 0.038 Comparative Example 4 0.047 Example 7 0.035 Comparative Example 5 0.044 Example 8 0.034

[0197] As can be seen from Table 2, the thermal conductivity of the product prepared in the embodiment is relatively low, basically between 0.018-0.028 W / mK, has good thermal insulation performance, and can be applied to various thermal insulation projects.

[0198] Test Example 4

[0199] The infrared reflection properties of the products obtained in the examples and comparative examples were tested using the method described in standard JG / T 235-2014. The results are shown in Table 3.

[0200] Table 3

[0201] serial number Infrared reflectance % serial number Infrared reflectance % Example 1 0.91 Example 9 0.85 Example 2 0.87 Example 10 0.87 Example 3 0.85 Comparative Example 1 0.78 Example 4 0.88 Comparative Example 2 0.88 Example 5 0.85 Comparative Example 3 0.89 Example 6 0.87 Comparative Example 4 0.68 Example 7 0.88 Comparative Example 5 0.85 Example 8 0.87

[0202] It can be seen from Table 3 that the products prepared in the examples have high infrared radiation reflection performance, and the infrared reflectance ratios are all greater than 0.85, which can effectively block the penetration of infrared radiation and prevent heat from diffusing by radiation.

[0203] Test Example 5

[0204] The water contact angles of the products prepared in the examples and comparative examples were measured using a contact angle meter.

[0205] The contact angle test photo of the product prepared in Example 1 is as follows: Figure 3 The contact angle test results are shown in Table 4.

[0206] Table 4

[0207]

[0208]

[0209] It can be seen from Table 4 that the products prepared in the examples have high hydrophobicity, and the water contact angles are all greater than 150°, which can effectively prevent water from penetrating into the interior of the material and affecting the thermal insulation performance of the material.

[0210] Test Example 6

[0211] The BET method was used to detect the products prepared in the examples and comparative examples.

[0212] Among them, the pore size distribution of the products prepared in Examples 1-3 is as follows Figure 4 The most probable pore diameter results of the products prepared in the examples and comparative examples are shown in Table 5.

[0213] Table 5

[0214] serial number Most probable pore size (nm) serial number Most probable pore size (nm) Example 1 40 Example 9 200 Example 2 80 Example 10 150 Example 3 90 Comparative Example 1 300 Example 4 100 Comparative Example 2 500 Example 5 60 Comparative Example 3 - Example 6 150 Comparative Example 4 100 Example 7 100 Comparative Example 5 500 Example 8 100

[0215] It can be seen from Table 5 that the most probable pore size of the material is evenly distributed, basically between 40-200 nm. Smaller pore size is conducive to inhibiting air convection, reducing heat loss through air convection, and ensuring better thermal insulation performance.

[0216] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A super-hydrophobic thermal insulation composite material, characterized in that: The raw materials for preparing the super-hydrophobic thermal insulation composite material include styrene, divinylbenzene, functionalized styrene, hollow glass microspheres modified by silane coupling agent, inorganic filler, initiator, emulsifier and water; The thermal conductivity of the super-hydrophobic thermal insulation composite material is ≤0.03 W / mK, and the water contact angle is >150°.

2. The super-hydrophobic thermal insulation composite material according to claim 1, characterized in that: The compressive strength of the super-hydrophobic thermal insulation composite material is ≥1 MPa.

3. The super-hydrophobic thermal insulation composite material according to claim 1 or 2, characterized in that: The most probable pore size of the super hydrophobic thermal insulation composite material is 10-200 nm.

4. The super-hydrophobic thermal insulation composite material according to claim 1 or 2, characterized in that: The inorganic filler is selected from one or more of silicon carbide, titanium nitride, titanium dioxide, worm graphite, graphene and carbon black.

5. The super-hydrophobic thermal insulation composite material according to claim 1, characterized in that: The silane coupling agent is selected from one or more of tetraethoxysilane, vinyl triethoxysilane, aminopropyl trimethoxysilane, glycidyl ether oxypropyl trimethoxysilane, vinyl trimethoxysilane and γ-methacryloxypropyl trimethoxysilane.

6. The super-hydrophobic thermal insulation composite material according to claim 1, characterized in that: The functionalized styrene is selected from one or more of N,N-dimethylstyrene, N,N-diethylstyrene, N,N-diphenylstyrene, methoxystyrene, methylthiostyrene, p-chlorostyrene and p-bromostyrene.

7. The super-hydrophobic thermal insulation composite material according to claim 1, characterized in that: The weight ratio of styrene, divinylbenzene, functionalized styrene, emulsifier, silane coupling agent modified hollow glass microspheres, inorganic filler and initiator is 1:0.5-6:0.1-3:0.5-3:0.01-0.5:0.01-0.1:0.2-1, and the weight ratio of water to styrene is 20-100:

1.

8. A method for preparing a super-hydrophobic thermal insulation composite material, characterized in that: The method comprises the following steps: (1) mixing styrene, divinylbenzene, functionalized styrene, an emulsifier and water to obtain a mixture A; (2) mixing mixed material A, hollow glass microspheres modified by silane coupling agent and inorganic filler to obtain mixed material B; (3) Mixed material B is mixed with an initiator solution containing an initiator and water, followed by reaction, and then washing and drying.

9. The method according to claim 8, characterized in that The inorganic filler is selected from one or more of silicon carbide, titanium nitride, titanium dioxide, worm graphite, graphene and carbon black.

10. The method according to claim 8 or 9, characterized in that: The silane coupling agent is selected from one or more of tetraethoxysilane, vinyl triethoxysilane, aminopropyl trimethoxysilane, glycidyl ether oxypropyl trimethoxysilane, vinyl trimethoxysilane and γ-methacryloxypropyl trimethoxysilane.

11. The method according to claim 8 or 9, characterized in that: The functionalized styrene is selected from one or more of N,N-dimethylstyrene, N,N-diethylstyrene, N,N-diphenylstyrene, methoxystyrene, methylthiostyrene, p-chlorostyrene and p-bromostyrene.

12. The method according to claim 8, characterized in that The weight ratio of styrene, divinylbenzene, functionalized styrene, emulsifier, silane coupling agent modified hollow glass microspheres, inorganic filler and initiator is 1:0.5-6:0.1-3:0.5-3:0.01-0.5:0.01-0.1:0.2-1.

13. The method according to claim 8 or 12, characterized in that: The weight ratio of the sum of the amounts of water used in step (1) and step (3) to styrene is 20-100:1; Preferably, in step (1), the weight ratio of water to styrene is 20-80:

1.

14. The method according to claim 8, characterized in that The emulsifier is selected from one or more of Tween 80, sodium dodecylbenzene sulfonate and polyvinyl alcohol.

15. The method according to claim 8 or 14, characterized in that The initiator is selected from potassium persulfate, ammonium persulfate or hydrogen peroxide.

16. The method according to claim 8, characterized in that In step (3), the reaction conditions include: temperature of 65-85°C and reaction time of 3-6h.

17. The method according to claim 8, characterized in that In step (3), the drying is vacuum drying.

18. A super-hydrophobic thermal insulation composite material prepared by the method according to any one of claims 8 to 17.

19. Use of the super-hydrophobic thermal insulation composite material according to any one of claims 1 to 7 or the super-hydrophobic thermal insulation composite material prepared by the method according to any one of claims 8 to 17 in the fields of heat insulation, thermal insulation, sound insulation or waterproofing.

Citation Information

Patent Citations

  • Titanium dioxide / polystyrene core / shell particle composite material and preparation method thereof

    CN106749790A

  • Thermal-insulation self-cleaning hybrid coating material and preparation method thereof

    CN110776788A

  • Mechanically robust aerogels and preparation method thereof