A water-swellable acrylic acid-based gel material and preparation method thereof
By modifying graphene oxide and using acrylic, acrylamide monomers and octavinyl POSS, water-swelling acrylic-based gel material was prepared, which solved the problem of insufficient adsorption capacity and mechanical properties of existing hydrogel materials, and achieved high efficiency The effect of removing dyes.
Patent Information
- Application Number
- CN202411262655.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-10
Smart Images

Figure 8UEUUMZMKKWPZSEKIX9H7OBL0MKGEAFZEPTRWUED
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of gel materials, and in particular to a water-swellable acrylic acid-based gel material and a preparation method thereof. Background Art
[0002] In today's world, the shortage of water resources restricts the survival and development of mankind, and water pollution, especially the pollution of toxic and harmful organic chemicals, not only poses a serious threat to the human living environment, but also further aggravates the shortage of water resources. Since dyes are widely used in printing and dyeing, textiles, papermaking, leather processing and other industrial fields, the discharge of a large amount of dye wastewater has caused serious environmental pollution. Dye wastewater has a high content of organic pollutants, complex structure and deep chroma, and most water-soluble dyes are toxic and chemically stable. Bacteria in conventional activated sludge cannot devour and destroy it and are difficult to degrade. Therefore, it is recognized as one of the difficult-to-treat wastewaters at home and abroad. Therefore, it is urgent to actively explore new technologies, methods and materials for wastewater treatment, and to deeply treat dye-containing wastewater to alleviate the pollution and shortage of water resources.
[0003] In recent years, new methods for dye wastewater treatment have been continuously proposed, such as electrolytic coagulation, chemical oxidation, electrochemical method, photocatalytic method, flotation, membrane separation, biodegradation, etc. Although these methods have good treatment effects, they have strict process conditions, poor stability, and high treatment costs. Therefore, these methods cannot be well applied to the treatment of dye wastewater. The adsorption method for treating dye wastewater consumes less energy, can effectively enrich and separate organic pollutants from wastewater, and will not introduce new pollutants. It is considered to be a relatively economical and efficient method.
[0004] Commonly used adsorbents include activated carbon, resin, etc. Although these adsorbents have good adsorption capacity, they are expensive and difficult to regenerate, which greatly limits their practical application. Therefore, adsorbents that are efficient, cheap, and environmentally friendly have attracted widespread attention from domestic and foreign companies. At present, in the research of dye wastewater treatment materials, hydrogels are considered to be a new type of adsorbent that can quickly remove dyes because they have hydrophilic groups and three-dimensional network structures, can store a large amount of water but are insoluble in water, and can produce specific interactions between the functional groups in the gel network and the dye molecules. However, the hydrogels prepared by the prior art have defects such as low adsorption capacity and poor mechanical properties, which make it difficult to simultaneously meet the dual requirements of super hygroscopicity of adsorbent materials and dye adsorption capacity. Summary of the invention
[0005] In view of this, the purpose of the present invention is to provide a water-swellable acrylic acid-based gel material and a preparation method thereof, and the technical problem to be solved is to prepare a hydrogel material with low preparation cost, green environmental protection, high mechanical properties and high adsorption performance.
[0006] The purpose of the present invention and the technical problem to be solved are achieved by adopting the following technical solutions. A method for preparing a water-swellable acrylic acid-based gel material according to the present invention comprises the following steps:
[0007] (1) Modifying graphene oxide with amino-containing POSS to prepare a modified graphene oxide dispersion; the mass ratio of graphene oxide to amino-containing POSS is 1:(0.05-0.50);
[0008] (2) Adding acrylic acid, acrylamide monomer and cross-linking agent to the modified graphene oxide dispersion in sequence, stirring evenly, then adding initiator, and reacting for a certain time to obtain a pre-reaction liquid; the mass ratio of acrylic acid, acrylamide monomer and graphene oxide is 500: (100-200): (5-10);
[0009] (3) Add octavinyl POSS to the pre-reaction solution, and continue the reaction at 60-75°C for 1-3 hours to obtain a gel mixed solution; the mass ratio of acrylic acid to octavinyl POSS is 500:(1-2);
[0010] (4) freeze-drying the gel mixture solution to obtain a water-swellable acrylic acid-based gel material.
[0011] Acrylic acid-based hydrogel has a unique three-dimensional network structure, which enables it to have the unique property of swelling but not dissolving in water. Its three-dimensional network pore structure has high adsorption to pollutants in water. Acrylic acid-based hydrogel can not only utilize the porous structure for physical adsorption; but also utilize the functional groups such as amide, carboxyl, amino, hydroxyl in the hydrogel structure to remove some pollutants such as organic dyes and heavy metal ions in the water body through electrostatic attraction, ion exchange, coordination chelation and the like. However, pure polyacrylic acid hydrogel has poor mechanical properties and low adsorption capacity. In order to improve the adsorption capacity and mechanical properties of acrylic acid, the present invention adds a certain amount of POSS-modified graphene oxide, and uses octavinyl POSS as a cross-linking agent to prepare acrylic acid-based hydrogel.
[0012] Graphene oxide can not only be used as an acrylic hydrogel reinforcement material, but also has a huge π-electron conjugated structure, a large specific surface area, and oxygen-containing functional groups such as hydroxyl, carboxyl, epoxy, and carbonyl on the surface, which provide abundant binding sites for the adsorption of heavy metals and dyes on GO. However, as a nanofiller, graphene oxide is prone to uneven dispersion during the polymerization process. Modification of graphene oxide with amino-containing POSS can improve the dispersion performance of graphene oxide in gel. Among them, the active amino groups on amino-containing POSS can react or form hydrogen bonds with oxygen-containing functional groups such as hydroxyl, carboxyl, epoxy, and carbonyl on graphene oxide, thereby improving the adhesion ability of POSS; and the introduction of large-volume POSS structure can effectively isolate graphene oxide and prevent secondary aggregation of graphene oxide during the polymerization process.
[0013] Octavinyl POSS is one of many siloxane molecules with a small diameter of only 1-3nm. Its structure contains an inorganic skeleton composed of silicon and oxygen elements, which makes the material have good mechanical properties and heat resistance. The skeleton connects eight reactive groups, which can not only improve the interaction between POSS and the polyacrylic acid matrix, but also has the same structure as the modified groups on the modified graphene oxide, further improving the dispersion of graphene oxide in the gel material. Compared with common cross-linking agents, octavinyl POSS has more active groups, which can effectively increase the degree of cross-linking. Moreover, as a rigid nanoparticle, it can play a reinforcing role similar to inorganic nanoparticles, greatly improving the mechanical properties of the gel. However, since POSS has a certain hydrophobicity and high rigidity, its dosage should not be too much, otherwise it will affect the water absorption and mechanical properties of the gel.
[0014] In one embodiment, the amino-containing POSS in step (1) is at least one of aminoethylaminopropylisobutylPOSS, aminopropylheptaphenylPOSS, and aminopropylheptaisobutylPOSS.
[0015] In one embodiment, the specific process of modifying graphene oxide with amino-containing POSS in step (1) is: dispersing graphene oxide and amino-containing POSS in deionized water; and then reacting at 60-90° C. for 3-6 hours to obtain a modified graphene oxide dispersion.
[0016] In one embodiment, the concentration of graphene oxide in deionized water is 0.1-0.5 g / L.
[0017] In one embodiment, the cross-linking agent in step (2) is N,N'-methylenebisacrylamide.
[0018] In one embodiment, the initiator in step (2) is at least one of ammonium persulfate, potassium persulfate and sodium persulfate.
[0019] In one embodiment, the mass ratio of acrylic acid, crosslinking agent and initiator in step (2) is 500:(1-5):(3-5). In order to improve the dispersibility of the reaction components, each component is added in the form of an aqueous solution.
[0020] In one embodiment, the stirring time in step (2) is 0.5-1 h.
[0021] In one embodiment, the reaction in step (2) is carried out at 45-55° C. for 0.5-1 h.
[0022] The present invention also provides a water-swellable acrylic acid-based gel material, which is filled with pore structures and has stability and excellent water absorption and swelling properties.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1. The preparation method of the water-swellable acrylic acid-based gel material is simple, the reaction conditions are mild, the operability is strong, and the cationic dye can be effectively and quickly removed.
[0025] 2. The water-swellable acrylic-based gel material is supplied in solid form. The product does not contain water and organic solvents, thus avoiding environmental pollution and energy consumption problems in the production, storage, transportation and use.
[0026] 3. The water-swellable acrylic acid-based gel material has a wide range of applicable reaction conditions, high mechanical strength, and high adsorption activity, and has good application prospects in the treatment of cationic dye wastewater. DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Example 1
[0029] A method for preparing a water-swellable acrylic acid-based gel material comprises the following steps:
[0030] (1) Graphene oxide was modified by amino-containing POSS to prepare a modified graphene oxide dispersion; the mass ratio of graphene oxide to amino-containing POSS was 1:0.10; the amino-containing POSS was aminoethylaminopropylisobutyl POSS; the specific process of modifying graphene oxide by amino-containing POSS was as follows: graphene oxide and amino-containing POSS were dispersed in deionized water; then reacted at 60°C for 6h to obtain a modified graphene oxide dispersion; the concentration of graphene oxide in deionized water was 0.1g / L;
[0031] (2) Add acrylic acid, acrylamide monomer and cross-linking agent to the modified graphene oxide dispersion in sequence, stir evenly, then add initiator, and react for a certain time to obtain a pre-reaction solution; the mass ratio of acrylic acid, acrylamide monomer and graphene oxide is 500:100:5; the cross-linking agent is N,N'-methylenebisacrylamide; the initiator is ammonium persulfate; the mass ratio of acrylic acid, cross-linking agent and initiator is 500:1:3; the stirring time is 0.5h; the reaction is reacted at 45°C for 1h;
[0032] (3) Add octavinyl POSS to the pre-reaction solution and continue the reaction at 60°C for 3 hours to obtain a gel mixed solution; the mass ratio of acrylic acid to octavinyl POSS is 500:1;
[0033] (4) freeze-drying the gel mixture solution to obtain a water-swellable acrylic acid-based gel material.
[0034] Example 2
[0035] A method for preparing a water-swellable acrylic acid-based gel material comprises the following steps:
[0036] (1) Graphene oxide was modified by amino-containing POSS to prepare a modified graphene oxide dispersion; the mass ratio of graphene oxide to amino-containing POSS was 1:0.20; the amino-containing POSS was aminopropyl heptadiphenyl POSS; the specific process of modifying graphene oxide by amino-containing POSS was as follows: graphene oxide and amino-containing POSS were dispersed in deionized water; then reacted at 90°C for 3h to obtain a modified graphene oxide dispersion; the concentration of graphene oxide in deionized water was 0.5g / L;
[0037] (2) Add acrylic acid, acrylamide monomer and cross-linking agent to the modified graphene oxide dispersion in sequence, stir evenly, then add initiator, and react for a certain time to obtain a pre-reaction solution; the mass ratio of acrylic acid, acrylamide monomer and graphene oxide is 500:200:10; the cross-linking agent is N,N'-methylenebisacrylamide; the initiator is potassium persulfate; the mass ratio of acrylic acid, cross-linking agent and initiator is 500:5:5; the stirring time is 1 hour; the reaction is reacted at 55°C for 0.5 hour;
[0038] (3) Add octavinyl POSS to the pre-reaction solution and continue the reaction at 75°C for 1 hour to obtain a gel mixed solution; the mass ratio of acrylic acid to octavinyl POSS is 500:2;
[0039] (4) freeze-drying the gel mixture solution to obtain a water-swellable acrylic acid-based gel material.
[0040] Example 3
[0041] A method for preparing a water-swellable acrylic acid-based gel material comprises the following steps:
[0042] (1) Graphene oxide was modified by amino-containing POSS to prepare a modified graphene oxide dispersion; the mass ratio of graphene oxide to amino-containing POSS was 1:0.12; the amino-containing POSS was aminopropyl heptaisobutyl POSS; the specific process of modifying graphene oxide by amino-containing POSS was as follows: graphene oxide and amino-containing POSS were dispersed in deionized water; then reacted at 70°C for 5h to obtain a modified graphene oxide dispersion; the concentration of graphene oxide in deionized water was 0.2g / L;
[0043] (2) Add acrylic acid, acrylamide monomer and cross-linking agent to the modified graphene oxide dispersion in sequence, stir evenly, then add initiator, and react for a certain time to obtain a pre-reaction solution; the mass ratio of acrylic acid, acrylamide monomer and graphene oxide is 500:100:10; the cross-linking agent is N,N'-methylenebisacrylamide; the initiator is ammonium persulfate; the mass ratio of acrylic acid, cross-linking agent and initiator is 500:2:3; the stirring time is 0.6h; the reaction is reacted at 48°C for 0.8h;
[0044] (3) Add octavinyl POSS to the pre-reaction solution and continue the reaction at 65°C for 2 hours to obtain a gel mixed solution; the mass ratio of acrylic acid to octavinyl POSS is 500:1.2;
[0045] (4) freeze-drying the gel mixture solution to obtain a water-swellable acrylic acid-based gel material.
[0046] Example 4
[0047] A method for preparing a water-swellable acrylic acid-based gel material comprises the following steps:
[0048] (1) Graphene oxide was modified by amino-containing POSS to prepare a modified graphene oxide dispersion; the mass ratio of graphene oxide to amino-containing POSS was 1:0.18; the amino-containing POSS was aminoethylaminopropylisobutyl POSS; the specific process of modifying graphene oxide by amino-containing POSS was as follows: graphene oxide and amino-containing POSS were dispersed in deionized water; then reacted at 80°C for 3.5h to obtain a modified graphene oxide dispersion; the concentration of graphene oxide in deionized water was 0.4g / L;
[0049] (2) Add acrylic acid, acrylamide monomer and cross-linking agent to the modified graphene oxide dispersion in sequence, stir evenly, then add initiator, and react for a certain time to obtain a pre-reaction liquid; the mass ratio of acrylic acid, acrylamide monomer and graphene oxide is 500:200:5; the cross-linking agent is N,N'-methylenebisacrylamide; the initiator is potassium persulfate; the mass ratio of acrylic acid, cross-linking agent and initiator is 500:5:4; the stirring time is 0.8h; the reaction is reacted at 50°C for 0.6h;
[0050] (3) Add octavinyl POSS to the pre-reaction solution and continue the reaction at 72°C for 1.3 hours to obtain a gel mixed solution; the mass ratio of acrylic acid to octavinyl POSS is 500:1.8;
[0051] (4) freeze-drying the gel mixture solution to obtain a water-swellable acrylic acid-based gel material.
[0052] Example 5
[0053] A method for preparing a water-swellable acrylic acid-based gel material comprises the following steps:
[0054] (1) Graphene oxide was modified by amino-containing POSS to prepare a modified graphene oxide dispersion; the mass ratio of graphene oxide to amino-containing POSS was 1:0.15; the amino-containing POSS was aminoethylaminopropylisobutyl POSS; the specific process of modifying graphene oxide by amino-containing POSS was as follows: graphene oxide and amino-containing POSS were dispersed in deionized water; then reacted at 80°C for 3h to obtain a modified graphene oxide dispersion; the concentration of graphene oxide in deionized water was 0.3g / L;
[0055] (2) Add acrylic acid, acrylamide monomer and cross-linking agent to the modified graphene oxide dispersion in sequence, stir evenly, then add initiator, and react for a certain time to obtain a pre-reaction solution; the mass ratio of acrylic acid, acrylamide monomer and graphene oxide is 500:150:7; the cross-linking agent is N,N'-methylenebisacrylamide; the initiator is ammonium persulfate; the mass ratio of acrylic acid, cross-linking agent and initiator is 500:3:4; the stirring time is 0.7h; the reaction is reacted at 50°C for 0.8h;
[0056] (3) Add octavinyl POSS to the pre-reaction solution and continue the reaction at 68°C for 2 hours to obtain a gel mixed solution; the mass ratio of acrylic acid to octavinyl POSS is 500:1.5;
[0057] (4) freeze-drying the gel mixture solution to obtain a water-swellable acrylic acid-based gel material.
[0058] Example 6
[0059] A method for preparing a water-swellable acrylic acid-based gel material comprises the following steps:
[0060] (1) Graphene oxide was modified by amino-containing POSS to prepare a modified graphene oxide dispersion; the mass ratio of graphene oxide to amino-containing POSS was 1:0.05; the amino-containing POSS was aminoethylaminopropylisobutyl POSS; the specific process of modifying graphene oxide by amino-containing POSS was as follows: graphene oxide and amino-containing POSS were dispersed in deionized water; then reacted at 80°C for 3h to obtain a modified graphene oxide dispersion; the concentration of graphene oxide in deionized water was 0.3g / L;
[0061] (2) Add acrylic acid, acrylamide monomer and cross-linking agent to the modified graphene oxide dispersion in sequence, stir evenly, then add initiator, and react for a certain time to obtain a pre-reaction solution; the mass ratio of acrylic acid, acrylamide monomer and graphene oxide is 500:150:7; the cross-linking agent is N,N'-methylenebisacrylamide; the initiator is ammonium persulfate; the mass ratio of acrylic acid, cross-linking agent and initiator is 500:3:4; the stirring time is 0.7h; the reaction is reacted at 50°C for 0.8h;
[0062] (3) Add octavinyl POSS to the pre-reaction solution and continue the reaction at 68°C for 2 hours to obtain a gel mixed solution; the mass ratio of acrylic acid to octavinyl POSS is 500:1.5;
[0063] (4) freeze-drying the gel mixture solution to obtain a water-swellable acrylic acid-based gel material.
[0064] Example 7
[0065] A method for preparing a water-swellable acrylic acid-based gel material comprises the following steps:
[0066] (1) Graphene oxide was modified by amino-containing POSS to prepare a modified graphene oxide dispersion; the mass ratio of graphene oxide to amino-containing POSS was 1:0.5; the amino-containing POSS was aminoethylaminopropylisobutyl POSS; the specific process of modifying graphene oxide by amino-containing POSS was as follows: graphene oxide and amino-containing POSS were dispersed in deionized water; then reacted at 80°C for 3h to obtain a modified graphene oxide dispersion; the concentration of graphene oxide in deionized water was 0.3g / L;
[0067] (2) Add acrylic acid, acrylamide monomer and cross-linking agent to the modified graphene oxide dispersion in sequence, stir evenly, then add initiator, and react for a certain time to obtain a pre-reaction solution; the mass ratio of acrylic acid, acrylamide monomer and graphene oxide is 500:150:7; the cross-linking agent is N,N'-methylenebisacrylamide; the initiator is ammonium persulfate; the mass ratio of acrylic acid, cross-linking agent and initiator is 500:3:4; the stirring time is 0.7h; the reaction is reacted at 50°C for 0.8h;
[0068] (3) Add octavinyl POSS to the pre-reaction solution and continue the reaction at 68°C for 2 hours to obtain a gel mixed solution; the mass ratio of acrylic acid to octavinyl POSS is 500:1.5;
[0069] (4) freeze-drying the gel mixture solution to obtain a water-swellable acrylic acid-based gel material.
[0070] Comparative Example 1
[0071] A method for preparing a water-swellable acrylic acid-based gel material comprises the following steps:
[0072] (1) Graphene oxide was modified by amino-containing POSS to prepare a modified graphene oxide dispersion; the mass ratio of graphene oxide to amino-containing POSS was 1:0.15; the amino-containing POSS was aminoethylaminopropylisobutyl POSS; the specific process of modifying graphene oxide by amino-containing POSS was as follows: graphene oxide and amino-containing POSS were dispersed in deionized water; then reacted at 80°C for 3h to obtain a modified graphene oxide dispersion; the concentration of graphene oxide in deionized water was 0.3g / L;
[0073] (2) Add acrylic acid, acrylamide monomer, crosslinking agent and octavinyl POSS to the modified graphene oxide dispersion in sequence, stir evenly, then add initiator, and react for a certain time to obtain a pre-reaction solution; the mass ratio of acrylic acid, acrylamide monomer and graphene oxide is 500:150:7; the crosslinking agent is N,N'-methylenebisacrylamide; the initiator is ammonium persulfate; the mass ratio of acrylic acid, crosslinking agent and initiator is 500:3:4; the stirring time is 0.7h; the reaction is carried out at 65°C for 2.8h; a gel mixed solution is obtained; the mass ratio of acrylic acid to octavinyl POSS is 500:1.5;
[0074] (3) Freeze-drying the gel mixture solution to obtain a water-swellable acrylic acid-based gel material.
[0075] Comparative Example 2
[0076] A method for preparing a water-swellable acrylic acid-based gel material comprises the following steps:
[0077] (1) Graphene oxide was modified by amino-containing POSS to prepare a modified graphene oxide dispersion; the mass ratio of graphene oxide to amino-containing POSS was 1:0.15; the amino-containing POSS was aminoethylaminopropylisobutyl POSS; the specific process of modifying graphene oxide by amino-containing POSS was as follows: graphene oxide and amino-containing POSS were dispersed in deionized water; then reacted at 80°C for 3h to obtain a modified graphene oxide dispersion; the concentration of graphene oxide in deionized water was 0.3g / L;
[0078] (2) Add acrylic acid, acrylamide monomer and cross-linking agent to the modified graphene oxide dispersion in sequence, stir evenly, then add initiator, and react for a certain time to obtain a pre-reaction solution; the mass ratio of acrylic acid, acrylamide monomer and graphene oxide is 500:150:7; the cross-linking agent is N,N'-methylenebisacrylamide; the initiator is ammonium persulfate; the mass ratio of acrylic acid, cross-linking agent and initiator is 500:3:4; the stirring time is 0.7h; the reaction is reacted at 50°C for 0.8h;
[0079] (3) Add octavinyl POSS to the pre-reaction solution and continue the reaction at 68°C for 2 hours to obtain a gel mixed solution; the mass ratio of acrylic acid to octavinyl POSS is 500:0.2;
[0080] (4) freeze-drying the gel mixture solution to obtain a water-swellable acrylic acid-based gel material.
[0081] Comparative Example 3
[0082] A method for preparing a water-swellable acrylic acid-based gel material comprises the following steps:
[0083] (1) Graphene oxide was modified by amino-containing POSS to prepare a modified graphene oxide dispersion; the mass ratio of graphene oxide to amino-containing POSS was 1:0.15; the amino-containing POSS was aminoethylaminopropylisobutyl POSS; the specific process of modifying graphene oxide by amino-containing POSS was as follows: graphene oxide and amino-containing POSS were dispersed in deionized water; then reacted at 80°C for 3h to obtain a modified graphene oxide dispersion; the concentration of graphene oxide in deionized water was 0.3g / L;
[0084] (2) Add acrylic acid, acrylamide monomer and cross-linking agent to the modified graphene oxide dispersion in sequence, stir evenly, then add initiator, and react for a certain time to obtain a pre-reaction solution; the mass ratio of acrylic acid, acrylamide monomer and graphene oxide is 500:150:7; the cross-linking agent is N,N'-methylenebisacrylamide; the initiator is ammonium persulfate; the mass ratio of acrylic acid, cross-linking agent and initiator is 500:3:4; the stirring time is 0.7h; the reaction is reacted at 50°C for 0.8h;
[0085] (3) Add octavinyl POSS to the pre-reaction solution and continue the reaction at 68°C for 2 hours to obtain a gel mixed solution; the mass ratio of acrylic acid to octavinyl POSS is 500:5;
[0086] (4) freeze-drying the gel mixture solution to obtain a water-swellable acrylic acid-based gel material.
[0087] Performance Test:
[0088] Tensile properties: The tensile breaking strength of the acrylic-based gel material after water swelling was tested using a universal tensile testing machine.
[0089] Equilibrium swelling ratio: Accurately weigh the water-swellable acrylic gel material with a mass of m0, immerse it in an aqueous solution, take out the gel sample after reaching swelling equilibrium, and use filter paper to absorb the surface water, then weigh the absorbed gel mass m1, and use the formula (m1-m0) / m0 to get the equilibrium swelling ratio of the gel. Equilibrium adsorption capacity: Use distilled water to prepare a methylene blue solution (ρ0) with a mass concentration of 360 mg / L, accurately weigh the water-swellable acrylic gel material with a mass of m0, immerse it in a methylene blue solution with a volume of V, and measure the methylene blue concentration in the solution with a UV-spectrophotometer at regular intervals until the methylene blue concentration (ρ1) remains unchanged, and use the formula (ρ0-ρ1)*V / m0 to get the equilibrium adsorption capacity of the gel.
[0090]
[0091] As can be seen from Table 1 and Table 2, graphene oxide can not only be used as acrylic acid-based hydrogel reinforcing material, but also provides abundant binding sites for the adsorption of heavy metals and dyes on GO; and the introduction of large-volume POSS structure can effectively isolate graphene oxide, preventing graphene oxide from secondary aggregation during polymerization. Octa-vinyl POSS can effectively increase the degree of crosslinking. And as a kind of rigid nanoparticle, it can play the reinforcing effect of similar inorganic nanoparticles, greatly improving the mechanical properties of gel. Comparative Examples 1-3 can be seen that due to the high degree of crosslinking of octa-vinyl POSS, it can not be added too early, otherwise it causes acrylic acid to be crosslinked too early, and the molecular chain growth is limited, affecting the formation of gel pores and the improvement of mechanical properties. Meanwhile, because POSS has certain hydrophobicity, and rigidity is relatively large, its consumption can not be too much, otherwise it can affect the water absorption and mechanical properties of gel.
[0092] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a water-swellable acrylic acid-based gel material, characterized in that: The following steps are involved: (1) Modifying graphene oxide with amino-containing POSS to prepare a modified graphene oxide dispersion; the mass ratio of graphene oxide to amino-containing POSS is 1:(0.05-0.50); (2) Adding acrylic acid, acrylamide monomer and cross-linking agent to the modified graphene oxide dispersion in sequence, stirring evenly, then adding initiator, and reacting for a certain time to obtain a pre-reaction liquid; the mass ratio of acrylic acid, acrylamide monomer and graphene oxide is 500: (100-200): (5-10); (3) Add octavinyl POSS to the pre-reaction solution, and continue the reaction at 60-75°C for 1-3 hours to obtain a gel mixed solution; the mass ratio of acrylic acid to octavinyl POSS is 500:(1-2); (4) freeze-drying the gel mixture solution to obtain a water-swellable acrylic acid-based gel material.
2. The method for preparing a water-swellable acrylic acid-based gel material according to claim 1, characterized in that: The amino-containing POSS in step (1) is at least one of aminoethylaminopropylisobutylPOSS, aminopropylheptaphenylPOSS, and aminopropylheptaisobutylPOSS.
3. The method for preparing a water-swellable acrylic acid-based gel material according to claim 1, characterized in that: The specific process of modifying graphene oxide with amino-containing POSS in step (1) is as follows: dispersing graphene oxide and amino-containing POSS in deionized water; and then reacting at 60-90° C. for 3-6 hours to obtain a modified graphene oxide dispersion.
4. The method for preparing a water-swellable acrylic acid-based gel material according to claim 3, characterized in that: The concentration of graphene oxide in deionized water is 0.1-0.5 g / L.
5. The method for preparing a water-swellable acrylic acid-based gel material according to claim 1, characterized in that: In step (2), the cross-linking agent is N,N'-methylenebisacrylamide.
6. The method for preparing a water-swellable acrylic acid-based gel material according to claim 1, characterized in that: The initiator in step (2) is at least one of ammonium persulfate, potassium persulfate and sodium persulfate.
7. The method for preparing a water-swellable acrylic acid-based gel material according to claim 1, characterized in that: In step (2), the mass ratio of acrylic acid, crosslinking agent and initiator is 500:(1-5):(3-5).
8. The method for preparing a water-swellable acrylic acid-based gel material according to claim 1, characterized in that: The stirring time in step (2) is 0.5-1h.
9. The method for preparing a water-swellable acrylic acid-based gel material according to claim 1, characterized in that: The reaction in step (2) is carried out at 45-55°C for 0.5-1h.
10. A water-swellable acrylic acid-based gel material, characterized in that: The water-swellable acrylic acid-based gel material is prepared by the preparation method of any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of high-strength stretchable conductive self-healing supramolecular hydrogel
CN109880123A
Graphene oxide / polyacrylic acid composite hydrogel and preparation method thereof
CN110790856A