Preparation method and application of organic silicon-phenoxy phosphazene-acrylate graft copolymer
Through the preparation method of silicone-phenoxyphosphazene-acrylate graft copolymer, the problem of difficult to balance flame retardancy and toughness enhancement in plastics is solved, and the low-temperature impact resistance and flame retardancy properties are significantly improved, with good Application prospects and market value.
Patent Information
- Application Number
- CN202410781354.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-15
AI Technical Summary
It is difficult to achieve both flame retardancy and toughness-enhancing properties in plastics using existing technology. At the same time, the low-temperature toughness of plastics is insufficient, which limits their wide application.
Using the preparation method of silicone-phenoxyphosphazene-acrylate graft copolymer, nano silicone rubber particles with flame retardant and toughness-enhancing properties are prepared through emulsification and grafting reactions, and are used in plastics to improve low-temperature impact performance.
It significantly improves the low-temperature impact resistance and flame retardant properties of plastics, reduces the amount of flame retardants, reduces production costs, and provides an environmentally friendly solution.
Smart Images

Figure CN118772341A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and specifically relates to a preparation method and application of an organosilicon-phenoxyphosphazene-acrylate graft copolymer. Background Art
[0002] With the development of science and technology, the requirements for the comprehensive performance of materials are getting higher and higher. As we all know, the toughening and flame retardancy of plastics have always been a difficult problem to balance. Toughening agents will reduce the flame retardancy of plastics while toughening them. The addition of flame retardants often sacrifices a lot of toughness. At the same time, as the use temperature decreases, the low-temperature toughness of plastics will be greatly reduced, which seriously restricts its further widespread application.
[0003] Therefore, developing a polymer that has flame retardant and toughening properties while greatly improving the low-temperature toughness of plastic products has become an important issue that needs to be urgently addressed in the industry.
[0004] CN113307916A discloses a method for preparing a silsesquioxane-modified acrylate flame retardant toughening agent. The flame retardant toughening agent contains a plurality of propylene-based silsesquioxane methacrylates as emulsion polymerization centers, which are firstly subjected to emulsion polymerization with butyl acrylate and diallyl diethyl ammonium chloride as core materials of a core-shell structure, and then subjected to a second step of emulsion polymerization with methyl methacrylate as a shell, thereby preparing a silsesquioxane-modified acrylate material with a core-shell structure. The plastic material to which the product of the invention is added can not only obviously achieve a toughening effect, but also the addition of the organosilicon material can also provide a good flame retardant effect for the material.
[0005] CN111393576A discloses a toughening agent with flame retardant effect, a synthesis method and application, which solves the problem of large amount of flame retardant and high production cost in the preparation process of modified plastics in the prior art. The synthesis method of the invention uses borate and silane coupling agent containing acrylate group as raw materials to synthesize seeds with acrylate group, then coats them with acrylate rubber, and finally grafts styrene-acrylonitrile. The toughening agent prepared by the synthesis method of the invention is used in the preparation of modified plastics. The invention creatively grafts hybrid Si-O-Si, B-O-Si, BOB structural units on the ASA graft copolymer skeleton to make them synergistic with the benzene ring and N of the ASA graft copolymer shell, effectively improving the flame retardant performance of the toughening agent. Applying it in the field of modified plastics can reduce the relative amount of flame retardant and reduce costs. The toughening agent of the invention does not contain halogen and phosphorus elements and is environmentally friendly.
[0006] The flame retardant toughening agents synthesized by the above two schemes do not mention the low-temperature impact performance of the products. Therefore, further research and development is needed. Summary of the invention
[0007] One of the purposes of the present invention is to propose a method for preparing an organosilicon-phenoxyphosphazene-acrylate graft copolymer; in the method, organosilicon and phosphazene rubber have good toughening effect and both have a certain flame retardant effect, so that the prepared graft copolymer has flame retardant and toughening properties, and the low-temperature toughness of plastic products is particularly improved.
[0008] In order to achieve the above invention object, the technical solution of the present invention is as follows:
[0009] A method for preparing an organosilicon-phenoxyphosphazene-acrylate graft copolymer, wherein the graft copolymer has good low-temperature flame retardant and toughening effects. The specific preparation method comprises the following steps:
[0010] 1) dissolving an organosilicon-phenoxyphosphazene high molecular copolymer in a solvent, then adding deionized water and an emulsifier, stirring, and then strongly emulsifying in an emulsifier to obtain an organosilicon-phenoxyphosphazene high molecular copolymer emulsion; in this step, the organosilicon-phenoxyphosphazene high molecular copolymer is a prior art, and can be specifically prepared by the method in CN 112142985A, which is not described in detail here.
[0011] 2) heating the organosilicon-phenoxyphosphazene high molecular copolymer emulsion, adding dropwise a methyl methacrylate mixed liquid containing an initiator, and continuing to keep the temperature for reaction after the addition is complete, to obtain an organosilicon-phenoxyphosphazene-acrylate graft copolymer emulsion;
[0012] 3) adding the organosilicon-phenoxyphosphazene-acrylate graft copolymer emulsion into an aqueous solution containing a demulsifier, performing a temperature-raising reaction, and then filtering, washing, and drying to obtain an organosilicon-phenoxyphosphazene-acrylate graft copolymer powder.
[0013] As a better embodiment of the present application, in step 1) of the preparation method, the mass ratio of the organosilicon-phenoxyphosphazene polymer copolymer, the solvent, the deionized water, and the emulsifier is 0.5-1:1-2:10-20:0.01-0.05; the speed in the emulsifier is 2000-5000 r / min, and the emulsification time is 5-10 min.
[0014] As a better embodiment of the present application, in step 1) of the preparation method, the solvent is selected from any one of toluene, xylene, acetone, butanone or a mixture of several thereof; the emulsifier is selected from any one of sodium dodecyl sulfate and sodium dodecylbenzene sulfonate or a mixture of two thereof.
[0015] As a preferred embodiment of the present application, in step 2) of the preparation method, when the organosilicon-phenoxyphosphazene high molecular copolymer emulsion is heated to 60-80°C, a mixed liquid consisting of an initiator and methyl methacrylate is added dropwise; the mixed monomer is added dropwise within 2-3 hours, and the reaction is continued at a temperature of 2-3 hours. The mass ratio of the organosilicon-phenoxyphosphazene high molecular copolymer emulsion to the mixed liquid is 5-10:5.
[0016] As a better embodiment of the present application, in step 2) of the preparation method, the initiator is selected from any one of potassium persulfate and sodium persulfate or a mixture of the two; wherein the weight ratio of the initiator to methyl methacrylate is 0.1% to 0.5%:1.
[0017] As a better implementation of the present application, in step 3) of the preparation method, the content of demulsifier in the demulsifier aqueous solution is 1-2wt%; the mass ratio of the organosilicon-phenoxyphosphazene-acrylate graft copolymer emulsion to the demulsifier aqueous solution is 1:1-2.
[0018] As a preferred embodiment of the present application, in step 3) of the preparation method, the temperature of the organosilicon-phenoxyphosphazene-acrylate graft copolymer emulsion and the demulsifier aqueous solution is raised to 60-80° C. and the reaction is maintained for 1-2 hours.
[0019] As a better embodiment of the present application, in step 3) of the preparation method, the demulsifier is selected from any one of magnesium persulfate and calcium chloride or a mixture of the two.
[0020] The second object of the present invention is to protect the organosilicon-phenoxyphosphazene-acrylate graft copolymer prepared by the above method or any combination of the method steps, and the graft copolymer has flame retardant and low-temperature toughening effects.
[0021] The third object of the present invention is to protect the application method of the above-mentioned organosilicon-phenoxyphosphazene-acrylate graft copolymer.
[0022] Furthermore, the invention provides an application of the organosilicon-phenoxyphosphazene-acrylate graft copolymer in modified plastics.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The graft copolymer prepared by the synthesis method of the present invention is applied to plastics, and the nano silicone rubber particles in the graft copolymer can effectively improve the impact resistance of plastic products. The glass transition temperature of the organic silicone rubber is below -110°C, and the impact resistance of the products in low temperature environments is particularly improved. At the same time, the graft copolymer prepared by the present invention can effectively improve the flame retardant properties of plastics through silicon-phosphorus synergistic flame retardancy, and has good application prospects and market value. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the DSC spectrum of the organosilicon-phenoxyphosphazene-acrylate graft copolymer synthesized in Example 1. DETAILED DESCRIPTION
[0026] A method for preparing an organosilicon-phenoxyphosphazene-acrylate graft copolymer comprises the following steps:
[0027] Step 1:
[0028] Step 1: dissolving the organosilicon-phenoxyphosphazene high molecular copolymer in a solvent, then adding deionized water and an emulsifier, stirring, and then strongly emulsifying in an emulsifier at a rate of 2000-5000 r / min for 5-10 minutes to obtain an organosilicon-phenoxyphosphazene high molecular copolymer emulsion;
[0029] Step 2: heating the above-mentioned organosilicon-phenoxyphosphazene high molecular copolymer emulsion to 60-80° C., and dripping a mixed liquid containing methyl methacrylate and an initiator, wherein the mixed liquid is dripped within 2-3 hours, and the reaction is continued at the temperature for 2-3 hours to obtain an organosilicon-phenoxyphosphazene-acrylate graft copolymer emulsion;
[0030] Step 3: Add the organosilicon-phenoxyphosphazene-acrylate graft copolymer emulsion to a 1-2 wt% concentration of a demulsifier aqueous solution, wherein the weight ratio of the organosilicon-phenoxyphosphazene-acrylate graft copolymer emulsion to the demulsifier aqueous solution is 1:1-2, heat to 60-80°C and maintain the reaction for 1 hour, then filter, wash and dry to obtain the organosilicon-phenoxyphosphazene-acrylate graft copolymer powder.
[0031] The solvent in step 1 of the present invention is selected from any one or a mixture of toluene, xylene, acetone, butanone, etc.; the emulsifier is selected from any one or a mixture of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, etc.;
[0032] The initiator in step 2 of the present invention is selected from any one or a mixture of potassium persulfate, sodium persulfate, etc.;
[0033] The demulsifier in step 3 of the present invention is selected from any one or a mixture of magnesium persulfate, calcium chloride, etc.
[0034] All features disclosed in this specification, or steps in all methods or processes disclosed, except mutually exclusive features and / or steps, can be combined in any manner.
[0035] Any feature disclosed in this specification (including claims and abstract), unless otherwise stated, may be replaced by other alternative features that are equivalent or have similar purposes. That is, unless otherwise stated, each feature is only an example of a series of equivalent or similar features.
[0036] The features and properties of the present invention are further described in detail below in conjunction with the examples. Where specific conditions are not specified in the examples, the conditions are carried out under conventional conditions or those recommended by the manufacturer. Where the manufacturers of reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0037] In the present application, the preparation method of the organosilicon-phenoxyphosphazene high molecular copolymer is a prior art, and reference may be made to the preparation method of the organosilicon / phenoxyphosphazene high molecular copolymer of CN112142985 A.
[0038] Embodiment 1:
[0039] Preparation of organosilicon-phenoxyphosphazene polymer copolymer (the method is the same as Example 1 in CN 112142985 A, the only difference is that 10g of methyltrichlorosilane in step ③ is replaced with 10g of 3-acryloxypropylmethyldichlorosilane, 50g of dimethyldichlorosilane, and 10g of methyltrichlorosilane):
[0040] 40g of hexachlorocyclotriphosphazene is ring-opened at 250°C to prepare a linear chlorine-containing polyphosphazene. After the reaction is detected to be complete, heating is stopped and the product is set aside. At 160°C, 200g of a 5wt% aqueous solution of NaOH is introduced into 100g of xylene containing 10g of bisphenol A and water is immediately separated. When bisphenol A disodium salt is formed and precipitated, it is dissolved in isopropanol. Finally, all the solvents are evaporated to obtain dry bisphenol A disodium salt. Finally, the prepared bisphenol A disodium salt is dissolved in xylene to prepare a 10% bisphenol A disodium salt-xylene solution.
[0041] The obtained linear chlorine-containing polyphosphazene, 10g 3-acryloxypropylmethyldichlorosilane, 50g dimethyldichlorosilane, 10g methyltrichlorosilane, and 80g 10wt% bisphenol A disodium phenol-xylene solution were reacted at 80°C for 2h, and after solvent removal, washing and purification, an organosilicon-phenoxyphosphazene high molecular copolymer was obtained.
[0042] Preparation of organosilicon-phenoxyphosphazene-acrylate graft copolymer:
[0043] The organosilicon-phenoxyphosphazene high molecular copolymer prepared above was completely dissolved in 140 g of acetone, and then 700 g of deionized water and 0.3 g of sodium dodecylbenzene sulfonate were added, stirred, and then strongly emulsified at a rate of 5000 r / min for 5 min in an emulsifier to obtain an organosilicon-phenoxyphosphazene high molecular copolymer emulsion (the solid content of the organosilicon-phosphazene was 20 wt %);
[0044] The organosilicon-phenoxyphosphazene high molecular copolymer emulsion was heated to 60°C, 40g of a mixed liquid of methyl methacrylate containing 5wt‰ potassium persulfate was added dropwise, and the addition was completed within 3 hours, and the reaction was continued at the temperature for 2 hours to obtain an organosilicon-phenoxyphosphazene-acrylate graft copolymer emulsion;
[0045] The organosilicon-phenoxyphosphazene-acrylate graft copolymer emulsion is added to a 2wt% magnesium sulfate aqueous solution (demulsifier), wherein the weight ratio of the copolymer emulsion to the demulsifier solution is 1:1, the temperature is raised to 60°C and the reaction is maintained for 1 hour, followed by filtration, washing and drying to obtain an organosilicon-phenoxyphosphazene-acrylate graft copolymer powder (moisture content ≤ 0.5wt%), which is also used as a flame retardant toughening agent.
[0046] Embodiment 2:
[0047] The preparation method of the organosilicon-phenoxyphosphazene high molecular copolymer is the same as that of Example 2 in CN 112142985 A, except that 13 g of ethyltrichlorosilane in step ③ of Example 2 is replaced with 10 g of 3-acryloxypropylmethyldichlorosilane, 50 g of dimethyldichlorosilane, and 10 g of methyltrichlorosilane to obtain the organosilicon-phenoxyphosphazene high molecular copolymer;
[0048] The organosilicon-phenoxyphosphazene high molecular copolymer prepared above was completely dissolved in 120 g of acetone, and then 600 g of deionized water and 0.2 g of sodium dodecylbenzene sulfonate were added, stirred, and then strongly emulsified in an emulsifier at a rate of 5000 r / min for 5 min to obtain an organosilicon-phenoxyphosphazene high molecular copolymer emulsion (the solid content of the organosilicon-phosphazene was 20 wt %);
[0049] The organosilicon-phenoxyphosphazene high molecular copolymer emulsion was heated to 60°C, 35 g of a mixed liquid of methyl methacrylate containing 5 wt‰ potassium persulfate was added dropwise, and the addition was completed within 3 hours, and the reaction was continued at the temperature for 2 hours to obtain an organosilicon-phenoxyphosphazene-acrylate graft copolymer emulsion;
[0050] The organosilicon-phenoxyphosphazene-acrylate graft copolymer emulsion is added to a 2wt% concentration of magnesium sulfate (demulsifier) aqueous solution, wherein the weight ratio of the copolymer emulsion to the demulsifier aqueous solution is 1:1, the temperature is raised to 60°C and the reaction is maintained for 1 hour, followed by filtration, washing and drying to obtain an organosilicon-phenoxyphosphazene-acrylate graft copolymer powder (moisture content ≤ 0.5wt%), which is also used as a flame retardant toughening agent.
[0051] Embodiment 3:
[0052] The preparation method of the organosilicon-phenoxyphosphazene polymer copolymer is the same as that of Example 3 in CN 112142985 A, except that 15 g of diethyldichlorosilane in step ③ of Example 3 is replaced with 10 g of 3-acryloxypropylmethyldichlorosilane, 50 g of dimethyldichlorosilane, and 10 g of methyltrichlorosilane to obtain the organosilicon-phosphazene copolymer;
[0053] The organosilicon-phenoxyphosphazene high molecular copolymer prepared above was completely dissolved in 125 g of acetone, and then 650 g of deionized water and 0.25 g of sodium dodecylbenzene sulfonate were added, stirred, and then strongly emulsified in an emulsifier at a rate of 5000 r / min for 5 min to obtain an organosilicon-phenoxyphosphazene high molecular copolymer emulsion (organosilicon-phosphazene solid content was 20 wt %);
[0054] The temperature of the organosilicon-phenoxyphosphazene high molecular copolymer emulsion was raised to 60°C, and 35 g of a mixed liquid of methyl methacrylate containing 5 wt‰ potassium persulfate (i.e., 5 wt‰ potassium persulfate and the rest being methyl methacrylate) was added dropwise, and the addition was completed within 3 hours, and the reaction was continued at the temperature for 2 hours to obtain an organosilicon-phenoxyphosphazene-acrylate graft copolymer emulsion;
[0055] The organosilicon-phenoxyphosphazene-acrylate graft copolymer emulsion is added to a 2wt% magnesium sulfate aqueous solution, wherein the weight ratio of the copolymer emulsion to the demulsifier solution is 1:1, the temperature is raised to 60°C and the reaction is maintained for 1 hour, followed by filtration, washing and drying to obtain an organosilicon-phenoxyphosphazene-acrylate graft copolymer powder (moisture content ≤ 0.5wt%), which is also used as a flame retardant toughening agent.
[0056] Test 1:
[0057] The organosilicon-phenoxyphosphazene-acrylate graft copolymer powder prepared in Examples 1-3 was mixed with polycarbonate (PC) and additives (antioxidant and anti-drip agent) according to the formula in the table, and then granulated and injection molded into strips by twin-screw extruder for testing. The flame retardant and impact performance comparison data are as follows:
[0058]
[0059]
[0060] Test 2:
[0061] Performance of the flame retardant toughening agent synthesized in Test Example 1 with different amounts of PC and additives
[0062] Note: Notched impact test is determined according to the method recorded in GB / T 1843.
[0063] As can be seen from the table above, the low-temperature impact performance and flame retardancy of the PC strips prepared by using the flame retardant toughening agent of the present invention are greatly improved, and the performance is particularly obvious in the low-temperature impact. The organosilicon-phenoxyphosphazene-acrylate graft copolymer is an excellent flame retardant toughening agent with great application prospects.
[0064] The above-mentioned embodiments only express the specific implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the protection scope of the present application. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the technical solution concept of the present application, and these all belong to the protection scope of the present application.
[0065] This background section is provided to generally present the context of the invention, and the work of the presently named inventors, the work to the extent described in this background section, and aspects of this section that did not constitute prior art at the time of application are neither explicitly nor implicitly admitted to be prior art to the present invention.
Claims
1. A method for preparing an organosilicon-phenoxyphosphazene-acrylate graft copolymer, characterized in that The following steps are involved: 1) dissolving an organosilicon-phenoxyphosphazene high molecular copolymer in a solvent, then adding deionized water and an emulsifier, stirring, and then strongly emulsifying in an emulsifier to obtain an organosilicon-phenoxyphosphazene high molecular copolymer emulsion; 2) heating the organosilicon-phenoxyphosphazene high molecular copolymer emulsion, adding a mixed liquid consisting of an initiator and methyl methacrylate dropwise, and continuing to keep the temperature for reaction after the addition is completed, to obtain an organosilicon-phenoxyphosphazene-acrylate graft copolymer emulsion; 3) adding the organosilicon-phenoxyphosphazene-acrylate graft copolymer emulsion into an aqueous solution containing a demulsifier, performing a temperature-raising reaction, and then filtering, washing, and drying to obtain an organosilicon-phenoxyphosphazene-acrylate graft copolymer powder.
2. The preparation method according to claim 1, characterized in that: In step 1), the mass ratio of the organosilicon-phenoxyphosphazene polymer copolymer, the solvent, the deionized water and the emulsifier is 0.5-1:1-2:10-20:0.01-0.05; the speed in the emulsifier is 2000-5000 r / min, and the emulsification time is 5-10 min.
3. The preparation method according to claim 1, characterized in that: In step 1), the solvent is selected from any one or a mixture of toluene, xylene, acetone, and butanone; and the emulsifier is selected from any one or two of sodium dodecyl sulfate and sodium dodecylbenzene sulfonate.
4. The preparation method according to claim 1, characterized in that: In step 2), when the temperature of the organosilicon-phenoxyphosphazene high molecular copolymer emulsion is raised to 60-80° C., the mixed liquid is added dropwise; the addition is completed within 2-3 hours, and the reaction is continued at the temperature for 2-3 hours; the mass ratio of the organosilicon-phenoxyphosphazene-acrylate graft copolymer emulsion to the mixed liquid is 5-10:
5.
5. The preparation method according to claim 1, characterized in that: In step 2), the initiator is selected from any one or both of potassium persulfate and sodium persulfate; in the mixed liquid, the weight ratio of the initiator to methyl methacrylate is 0.1% to 0.5%:
1.
6. The preparation method according to claim 1, characterized in that: In step 3), the content of the demulsifier in the aqueous solution containing the demulsifier is 1-2 wt %; the mass ratio of the organosilicon-phenoxyphosphazene-acrylate graft copolymer emulsion to the demulsifier aqueous solution is 1:1-2.
7. The preparation method according to claim 1, characterized in that: In step 3), the temperature of the organosilicon-phenoxyphosphazene-acrylate graft copolymer emulsion and the demulsifier aqueous solution is raised to 60-80° C. and maintained at this temperature for 1-2 hours.
8. The preparation method according to claim 1, characterized in that: In step 3), the demulsifier is selected from any one or both of magnesium persulfate and calcium chloride.
9. The organosilicon-phenoxyphosphazene-acrylate graft copolymer prepared according to the method of any one of claims 1 to 8, wherein the graft copolymer has good flame retardant and toughening effects.
10. Use of the organosilicon-phenoxyphosphazene-acrylate graft copolymer according to claim 9 in modified plastics.
Citation Information
Patent Citations
Toughening agent with flame-retardant effect as well as synthesis method and application thereof
CN111393576A
Organosilicon / phenoxy phosphazene high-molecular copolymer, and preparation method and application thereof
CN112142985A
Silsesquioxane modified acrylate type flame-retardant toughening agent and preparation method thereof