Bio-based degradable nylon and preparation method thereof

By using degradable diamines and bio-based dibasic acids for specific processing, bio-based degradable nylon with excellent mechanical and heat-resistant properties is prepared, which solves the problem of poor material performance in the existing technology and achieves efficient Bio-based nylon preparation.

CN118772399AActive Publication Date: 2024-10-15CHUANHUA GRP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411260236.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-10-15
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

The existing preparation method of biodegradable nylon has complicated steps, and the resulting material has poor mechanical properties and heat resistance, and has a high water absorption rate.

Method used

Using degradable diamines and bio-based dibasic acids as raw materials, through specific mixing, heating, pressurization and condensation reactions in a vacuum environment, bio-based biodegradable products with excellent degradation properties, good mechanical properties and heat resistance are prepared. Degraded nylon.

Benefits of technology

It achieves the high degradation performance, low water absorption, excellent mechanical and heat resistance properties of biodegradable nylon, and increases the yield and molecular weight, making it suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772399A_ABST
    Figure CN118772399A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of high polymer materials, and relates to bio-based degradable nylon and a preparation method thereof, and the preparation raw materials comprise degradable diamine and bio-based binary acid; the degradable diamine is selected from at least one of 4, 4 '-dithio diphenylamine, 2, 2'-dimethoxy-4, 4 '-dithio diphenylamine, and 3, 3'-dithio dipropylamine; the bio-based binary acid is selected from at least one of 2, 5-furandicarboxylic acid, 2-hydroxysuccinic acid, itaconic acid, malonic acid, succinic acid, glutaric acid, adipic acid and sebacic acid. The prepared bio-based degradable nylon is high in degradation rate, excellent in mechanical property and heat resistance, low in water absorption rate, high in yield and molecular weight and capable of achieving large-scale production, and has the advantages of being environmentally friendly in preparation method, high in economic benefit, easy and convenient to operate, good in application prospect and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials and relates to a bio-based degradable nylon and a preparation method thereof. Background Art

[0002] Nylon (PA) is a general term for polymers with amide groups (-CO-NH-), which can be formed by self-polymerization of lactam molecules or by polycondensation of diamines and dibasic acids. Its molecular structure is mainly composed of amide groups and methine or other cycloalkyl and aromatic groups. Nylon has good mechanical properties, heat resistance, wear resistance and self-lubricating properties, and is widely used in electronic appliances, automobiles, aerospace and other fields.

[0003] However, the polymerization monomers of nylon are generally derived from fossil fuels, which consume a large amount of oil resources. At present, the growth rate of proven oil reserves has slowed down significantly, the remaining production capacity is limited, and the extraction, refining, storage, transportation and use of oil are prone to damage the ecological environment. As the concept of sustainable development has become popular, the conversion and utilization of biomass raw materials has become a new research hotspot. Therefore, bio-based degradable nylon has received more and more attention from academia and industry in recent years.

[0004] However, the existing preparation methods of bio-based degradable nylon have the problems of complicated preparation steps, and the prepared degradable nylon has poor mechanical properties and poor heat resistance. Summary of the invention

[0005] In order to solve the defects in the prior art, the present invention provides a bio-based degradable nylon and a preparation method thereof. The obtained bio-based degradable nylon has excellent degradation performance, good mechanical properties and heat resistance, as well as low water absorption, high yield and molecular weight.

[0006] To achieve the above object, the present invention adopts the following technical solutions: In a first aspect, the present invention provides a bio-based degradable nylon, the raw materials for preparing the nylon include a degradable diamine and a bio-based dibasic acid; The degradable diamine is selected from at least one of 4,4'-dithiodiphenylamine, 2,2'-dimethoxy-4,4'-dithiodiphenylamine, and 3,3'-dithiobispropylamine; The bio-based dibasic acid is selected from at least one of 2,5-furandicarboxylic acid, 2-hydroxysuccinic acid, itaconic acid, malonic acid, succinic acid, glutaric acid, adipic acid, and sebacic acid.

[0007] Preferably, the molar ratio of the degradable diamine to the bio-based dibasic acid is 1:(0.6-1.2). More preferably, the molar ratio of the degradable diamine to the bio-based dibasic acid is 1:1.

[0008] Preferably, the degradable diamine is 4,4'-dithiodiphenylamine.

[0009] Preferably, the bio-based dibasic acid is 2,5-furandicarboxylic acid.

[0010] Preferably, the structural formula of the bio-based degradable nylon is as shown in Formula I below:

[0011] Formula I.

[0012] Preferably, the number average molecular weight of the bio-based degradable nylon is 55,000-61,000.

[0013] In a second aspect, the present invention provides a method for preparing bio-based degradable nylon, comprising the following steps: S1. Mixing a degradable diamine, a bio-based dibasic acid and a solvent in a protective atmosphere to obtain a mixture; the degradable diamine is selected from at least one of 4,4'-dithiodiphenylamine, 2,2'-dimethoxy-4,4'-dithiodiphenylamine and 3,3'-dithiobispropylamine; the bio-based dibasic acid is selected from at least one of 2,5-furandicarboxylic acid, 2-hydroxysuccinic acid, itaconic acid, malonic acid, succinic acid, glutaric acid, adipic acid and sebacic acid; S2, stirring the mixture under elevated temperature, stopping the temperature increase after reaching the target temperature and pressurizing to carry out condensation reaction to obtain reactant 1; S3, subjecting the reactant 1 to a reaction after gradually increasing the temperature under a pressurized environment to obtain a reactant 2; S4, releasing the pressure of the reactant 2, raising the temperature, and reacting in a vacuum environment to obtain bio-based degradable nylon.

[0014] Preferably, the molar ratio of the degradable diamine to the bio-based dibasic acid is 1:(0.6-1.2); more preferably, the molar ratio of the degradable diamine to the bio-based dibasic acid is 1:1.

[0015] Preferably, the mass of the solvent accounts for 50-70% of the sum of the mass of the degradable diamine and the bio-based dibasic acid.

[0016] Preferably, the protective atmosphere in S1 is selected from any one of nitrogen, argon, helium and neon.

[0017] Preferably, a catalyst is also added to S1.

[0018] Preferably, the catalyst is selected from at least one of sodium hypophosphite, sodium hypophosphite, potassium hypophosphite, calcium hypophosphite, phosphate ester, propyl titanate, and boric acid.

[0019] Preferably, the mass of the catalyst accounts for 0.15-0.31% of the sum of the mass of the degradable diamine and the bio-based dibasic acid.

[0020] Preferably, the stirring speed in S2 is 300-400 r / min, and the target temperature is 140-170 °C.

[0021] Preferably, the pressurized pressure in S2 is 0.5-0.9 Mpa.

[0022] Preferably, the reaction time of the S2 condensation reaction is 2 to 4 h.

[0023] Preferably, the gradient heating condition in S3 is: heating to 270-310° C. at a heating rate of 20-40° C. / min.

[0024] Preferably, the pressure of the pressurized environment in S3 is 3-4 Mpa.

[0025] Preferably, the reaction time in S3 is 1 to 3 h.

[0026] Preferably, the pressure after decompression in S4 is 0.4-0.8 Mpa.

[0027] Preferably, the temperature in S4 is raised to 320-360 °C. Preferably, the reaction time of S4 is 2 to 4 h.

[0028] The beneficial effects of the present invention are: The bio-based degradable nylon of the invention has good degradation performance, excellent mechanical properties and heat resistance, low water absorption, high yield and molecular weight, excellent comprehensive performance, can be mass-produced, and has good application prospects.

[0029] The bio-based degradable nylon of the invention is prepared by polymerization reaction of biodegradable diamine and dibasic acid as raw materials. The preparation method is green and environmentally friendly, has high economic benefits, is easy to operate, and is conducive to sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a Fourier infrared spectrum characterization diagram of the bio-based degradable nylon prepared in Example 2. DETAILED DESCRIPTION

[0031] In order to enable those skilled in the art to better understand the technical solution of the invention, the present invention is further described in detail below in conjunction with specific implementation methods.

[0032] Example 1 This embodiment provides a method for preparing bio-based degradable nylon, the steps are as follows: S1. Add 248.4 g of 4,4'-dithiodiphenylamine, 93.7 g of 2,5-furandicarboxylic acid (the molar ratio of 4,4'-dithiodiphenylamine to 2,5-furandicarboxylic acid is 1:0.6), 0.7 g of sodium hypophosphite (0.2% of the sum of the mass of 4,4'-dithiodiphenylamine and 2,5-furandicarboxylic acid) and 205.3 g of deionized water (60% of the sum of the mass of 4,4'-dithiodiphenylamine and 2,5-furandicarboxylic acid) into a magnetically driven high-pressure reactor, and introduce a protective atmosphere of N 2 Replace the air in the kettle; S2, start stirring of the magnetically driven high-pressure reactor, set the stirring speed to 360 r / min, heat the reactor to 150 °C and then stop heating, inflate and pressurize to 0.7 MPa, and carry out condensation reaction for 2.5 h to obtain reactant 1; S3, raising the temperature of the magnetically driven high-pressure reactor to 290 °C at a rate of 30 °C / min, and setting the pressure of the reactor to 3 MPa. After reaching the temperature, react for 1 h to obtain reactant 2; S4, release the pressure to 0.5 MPa, increase the temperature to 340 °C, and vacuum the reaction for 2 h, then pressurize and discharge the material to obtain bio-based degradable nylon (PA-SF-1).

[0033] The structural formula of the obtained bio-based degradable nylon is: .

[0034] Example 2 S1. Add 248.4 g of 4,4'-dithiodiphenylamine, 156.1 g of 2,5-furandicarboxylic acid (the molar ratio of 4,4'-dithiodiphenylamine to 2,5-furandicarboxylic acid is 1:1), 0.8 g of sodium hypophosphite (0.2% of the sum of the mass of 4,4'-dithiodiphenylamine and 2,5-furandicarboxylic acid) and 242.7 g of deionized water (60% of the sum of the mass of 4,4'-dithiodiphenylamine and 2,5-furandicarboxylic acid) into a magnetically driven high-pressure reactor, and introduce a protective atmosphere of N 2 Replace the air in the kettle; The steps of S2 to S4 are the same as those in Example 1, and bio-based degradable nylon (PA-SF-2) is obtained.

[0035] The structural formula of the obtained bio-based degradable nylon is the same as that of Example 1.

[0036] Example 3 S1. Add 248.4 g of 4,4'-dithiodiphenylamine, 187.3 g of 2,5-furandicarboxylic acid (the molar ratio of 4,4'-dithiodiphenylamine to 2,5-furandicarboxylic acid is 1:1.2), 0.9 g of sodium hypophosphite (0.2% of the total mass of 4,4'-dithiodiphenylamine and 2,5-furandicarboxylic acid) and 261.4 g of deionized water (60% of the total mass of 4,4'-dithiodiphenylamine and 2,5-furandicarboxylic acid) into a magnetically driven high-pressure reactor, and introduce a protective atmosphere of N 2 Replace the air in the kettle; The steps of S2 to S4 are the same as those in Example 1, and bio-based degradable nylon (PA-SF-3) is obtained.

[0037] The structural formula of the obtained bio-based degradable nylon is the same as that of Example 1.

[0038] Example 4 The step of S1 is the same as that of Example 1; S2, start stirring of the magnetically driven high-pressure reactor, set the stirring speed to 300 r / min, heat the reactor to 140 °C and then stop heating, inflate and pressurize to 0.5 MPa, and carry out condensation reaction for 2 h to obtain reactant 1; S3, raising the temperature of the magnetically driven high-pressure reactor to 270 °C at a rate of 20 °C / min, and setting the pressure of the reactor to 3 MPa. After reaching the temperature, react for 1 h to obtain reactant 2; S4, release the pressure to 0.4 MPa, increase the temperature to 320 °C, and vacuum the reaction for 2 h, then pressurize and discharge the material to obtain bio-based degradable nylon (PA-SF-4).

[0039] The structural formula of the obtained bio-based degradable nylon is the same as that of Example 1.

[0040] Example 5 The step of S1 is the same as that of Example 1; S2, start stirring of the magnetically driven high-pressure reactor, set the stirring speed to 400 r / min, heat the reactor to 170 °C and then stop heating, inflate and pressurize to 0.9 MPa, and carry out condensation reaction for 4 h to obtain reactant 1; S3, raising the temperature of the magnetically driven high-pressure reactor to 310 °C at a rate of 40 °C / min, and setting the pressure of the reactor to 4 MPa. After reaching the temperature, react for 3 h to obtain reactant 2; S4, release the pressure to 0.8 MPa, increase the temperature to 360 °C, and vacuum the reaction for 4 h, then pressurize and discharge the material to obtain bio-based degradable nylon (PA-SF-5).

[0041] The structural formula of the obtained bio-based degradable nylon is the same as that of Example 1.

[0042] Example 6 Same as Example 1, except that: The mass of the deionized water accounts for 50% of the sum of the mass of the degradable diamine and the bio-based dibasic acid; The mass of the sodium hypophosphite accounts for 0.15% of the sum of the mass of the degradable diamine and the bio-based dibasic acid; Bio-based degradable nylon (PA-SF-6) was obtained.

[0043] The structural formula of the obtained bio-based degradable nylon is the same as that of Example 1.

[0044] Example 7 Same as Example 1, except that: The mass of the deionized water accounts for 70% of the sum of the mass of the degradable diamine and the bio-based dibasic acid; The mass of the sodium hypophosphite accounts for 0.31% of the sum of the mass of the degradable diamine and the bio-based dibasic acid; Bio-based degradable nylon (PA-SF-7) was obtained.

[0045] The structural formula of the obtained bio-based degradable nylon is the same as that of Example 1.

[0046] Comparative Example 1 S1. Add 136.2 g p-phenylenediamine, 156.1 g 2,5-furandicarboxylic acid (the molar ratio of p-phenylenediamine to 2,5-furandicarboxylic acid is 1:1), 0.6 g sodium hypophosphite (0.2% of the total mass of p-phenylenediamine and 2,5-furandicarboxylic acid), and 175.4 g deionized water (60% of the total mass of p-phenylenediamine and 2,5-furandicarboxylic acid) into a magnetically driven high-pressure reactor, and introduce a protective atmosphere of N 2 Replace the air in the kettle; The steps of S2 to S4 are the same as those of Example 1 to obtain nylon (PA-1).

[0047] Comparative Example 2 S1. Add 248.4 g of 4,4'-dithiodiphenylamine, 166.1 g of terephthalic acid (the molar ratio of 4,4'-dithiodiphenylamine to terephthalic acid is 1:1), 0.8 g of sodium hypophosphite (0.2% of the total mass of 4,4'-dithiodiphenylamine and terephthalic acid), and 248.7 g of deionized water (60% of the total mass of 4,4'-dithiodiphenylamine and terephthalic acid) into a magnetically driven high-pressure reactor, and introduce a protective atmosphere of N 2 Replace the air in the kettle; The steps of S2 to S4 are the same as those in Example 1 to obtain nylon (PA-2).

[0048] Effect Example 1 Fourier Infrared Spectroscopy Characterization The biodegradable nylon (PA-SF-2) prepared in Example 2 was characterized by infrared spectroscopy. Figure 1 .

[0049] Depend on Figure 1 It can be seen that among them, 3407 cm -1 The characteristic peaks near 2940 cm-1 are attributed to the NH stretching vibration absorption peak on polyamide, while the peak at 2940 cm-1 is -1 The characteristic peaks near 1638 cm-1 are attributed to the antisymmetric and symmetric stretching vibrations of CH on polyamide (amide band I). -1 The characteristic peak at 1106 cm-1 is attributed to the -CO-NH- bending vibration of polyamide (amide band II). -1 The characteristic peaks nearby correspond to the stretching vibration peaks of SS.

[0050] Effect Example 2 Nylon Degradation Performance Test The degradation performance of the nylon prepared in the examples and comparative examples was tested, and the results are shown in Table 1.

[0051] Table 1 Degradation performance test results of Comparative Examples 1-2 and Examples 1-7

[0052] It can be seen from Table 1 that the weight loss rate of the bio-based degradable nylon prepared in the embodiment of the present invention is relatively high, which reflects the excellent degradation performance of the bio-based degradable nylon of the present invention. However, in Comparative Examples 1 and 2, which do not use the raw materials of the present invention, the weight loss rate is significantly reduced and the degradation performance is significantly deteriorated.

[0053] Effect Example 3 Nylon Mechanical Properties Test The mechanical properties of the nylon prepared in the examples and comparative examples were tested, and the results are shown in Table 2.

[0054] Table 2 Mechanical properties test results of comparative examples 1-2 and embodiments 1-7

[0055] It can be seen from Table 2 that the bio-based degradable nylon prepared in the embodiment of the present invention has a higher tensile strength, which reflects the excellent mechanical properties of the bio-based degradable nylon of the present invention. However, Comparative Examples 1 and 2, which do not use the raw materials of the present invention, have lower tensile strength and poorer mechanical properties.

[0056] Effect Example 4 Nylon Thermal Performance Test The bio-based degradable nylon prepared in the examples and comparative examples was tested for thermal properties. The results are shown in Table 3.

[0057] Table 3 Thermal performance test results of Comparative Examples 1-2 and Examples 1-7

[0058] It can be seen from Table 3 that the bio-based degradable nylon prepared in the embodiment of the present invention has T d5% and T g The value is relatively high, which reflects the excellent thermal properties of the bio-based degradable nylon of the present invention, while Comparative Examples 1 and Comparative Examples 2 which do not use the raw materials of the present invention, T d5% and T g The lower the value, the poorer the mechanical properties.

[0059] Effect Example 5 Nylon water absorption performance test The water absorption performance of the nylon prepared in the embodiment and the comparative example was tested, and the results are shown in Table 4.

[0060] Table 4 Water absorption test results of Comparative Examples 1-2 and Examples 1-7

[0061] It can be seen from Table 4 that the water absorption rate of the bio-based degradable nylon prepared in the embodiment of the present invention is relatively low, indicating that the bio-based degradable nylon of the present invention is not easy to absorb water, while the comparative examples 1 and 2 which do not use the raw materials of the present invention have relatively high water absorption rates.

[0062] Effect Example 6 Nylon Yield and Molecular Weight Test The yield and molecular weight of the nylon prepared in the examples and comparative examples were tested, and the results are shown in Table 5.

[0063] Table 5 Yield and molecular weight test results of Comparative Examples 1-2 and Examples 1-7

[0064] It can be seen from Table 5 that the yield and molecular weight of the bio-based degradable nylon prepared in the embodiment of the present invention are both high, and higher than those of the nylon prepared in the comparative example.

[0065] The above are only preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be regarded as limiting the present invention, and the protection scope of the present invention should be based on the scope defined by the claims. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A bio-based degradable nylon, characterized in that: The raw materials for its preparation include degradable diamines and bio-based dibasic acids; The degradable diamine is selected from at least one of 4,4'-dithiodiphenylamine, 2,2'-dimethoxy-4,4'-dithiodiphenylamine, and 3,3'-dithiobispropylamine; The bio-based dibasic acid is selected from at least one of 2,5-furandicarboxylic acid, 2-hydroxysuccinic acid, itaconic acid, malonic acid, succinic acid, glutaric acid, adipic acid, and sebacic acid.

2. The bio-based degradable nylon according to claim 1, characterized in that: The molar ratio of the degradable diamine to the bio-based dibasic acid is 1:(0.6-1.2).

3. The bio-based degradable nylon according to claim 1 or 2, characterized in that: The structural formula of the bio-based degradable nylon is shown in Formula I below: Formula I.

4. A method for preparing bio-based degradable nylon, characterized in that: The following steps are involved: S1. Mixing a degradable diamine, a bio-based dibasic acid and a solvent in a protective atmosphere to obtain a mixture; the degradable diamine is selected from at least one of 4,4'-dithiodiphenylamine, 2,2'-dimethoxy-4,4'-dithiodiphenylamine and 3,3'-dithiobispropylamine; the bio-based dibasic acid is selected from at least one of 2,5-furandicarboxylic acid, 2-hydroxysuccinic acid, itaconic acid, malonic acid, succinic acid, glutaric acid, adipic acid and sebacic acid; S2, stirring the mixture under elevated temperature, stopping the temperature increase after reaching the target temperature and pressurizing to carry out condensation reaction to obtain reactant 1; S3, subjecting the reactant 1 to a reaction after gradually increasing the temperature under a pressurized environment to obtain a reactant 2; S4, releasing the pressure of the reactant 2, raising the temperature, and reacting in a vacuum environment to obtain bio-based degradable nylon.

5. The preparation method according to claim 4, characterized in that: A catalyst is also added to the S1.

6. The preparation method according to claim 5, characterized in that: The catalyst is selected from at least one of sodium hypophosphite, sodium hypophosphite, potassium hypophosphite, calcium hypophosphite, phosphate ester, propyl titanate, and boric acid.

7. The preparation method according to claim 4, characterized in that The stirring speed in S2 is 300-400 r / min, and the target temperature is 140-170 °C.

8. The preparation method according to claim 4, characterized in that The conditions for the gradient heating in S3 are: heating to 270-310°C at a heating rate of 20-40°C / min.

9. The preparation method according to claim 4, characterized in that The pressure after decompression in S4 is 0.4-0.8 MPa.

10. The preparation method according to claim 4, characterized in that In the S4, the temperature is raised to 320-360°C.

Citation Information

Patent Citations

  • Preparation method of bio-based polyamide copolymer elastomer

    CN104193989A

  • Polyhexahydrotriazine structure polyimide film and preparation method and application thereof

    CN115216008A

  • Degradable bio-based polyester as well as preparation method and application thereof

    CN115322350A

  • Degradable polyester as well as preparation method, degradation method and application thereof

    CN115572380A

  • Thermal-adaptability polyether amide elastomer material based on dynamic disulfide bonds and preparation method of thermal-adaptability polyether amide elastomer material

    CN116120563A