Eucommia ulmoides rubber-based bio-based latex and preparation method thereof
By blending and emulsifying Eucommia rubber with other rubbers to prepare bio-based latex, the problem of insufficient performance of Eucommia rubber is solved, its hardness and tensile properties are improved, and the application fields are broadened.
Patent Information
- Application Number
- CN202411246024.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Eucommia rubber is non-sticky, has low flexibility, small deformation and low elasticity at room temperature. When improving its performance, existing technology has strict glass transition temperature requirements, which affects the mechanical properties of composite materials.
Eucommia rubber is blended synchronously or asynchronously with cis-polyisoprene rubber, butadiene rubber, styrene-butadiene rubber and other blended rubbers, and bio-based latex is prepared through synchronous or asynchronous emulsification methods, and then subjected to normal pressure distillation and The solvent is removed by distillation under reduced pressure and concentrated by high-speed centrifugation to form a stable bio-based latex.
It combines the performance advantages of soft and hard rubber, improves the hardness and shape memory characteristics of Eucommia rubber, enhances its tensile properties, and broadens its application fields.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention specifically relates to the field of polymer materials and preparation methods, and is a bio-based latex based on eucommia rubber and a preparation method. Background Art
[0002] At present, Eucommia rubber is a bio-based polymer material with the dual properties of rubber and plastic. Its main component is trans-1,4-polyisoprene, which is an isomer of natural rubber in terms of molecular chain configuration. The trans structure of Eucommia rubber makes its molecular chain highly ordered, regular, easy to crystallize, and has a large volume density. It is a hard plastic at room temperature, and it becomes a rubber state after crystallization and melting. Eucommia rubber has the characteristics of high molecular weight, high hardness and high modulus, but its crystallization area has no curling and winding, which makes Eucommia rubber have the defects of no viscosity, low flexibility, small deformation and low elasticity.
[0003] In order to change the above shortcomings of Eucommia rubber, Chinese patent CN107841229B discloses a method for degrading, liquefying and epoxidizing Eucommia rubber, and grafting and blending it with water-based epoxy resin to improve its flexibility, elongation and impact resistance. Chinese patent CN117050396A discloses a method for blending and vulcanizing Eucommia rubber and natural rubber, aiming to improve the heat aging resistance of the product. Chinese patent CN116199946A provides a method for blending Eucommia rubber with plastic powder to prepare a high-hardness rubber composite material with shape memory function. Although the above blending method can improve the aging resistance, low temperature resistance and tensile properties of the composite material, it has strict requirements on the glass transition temperature of the two materials, which affects the mechanical properties of the composite material.
[0004] Chinese patent CN117903339A discloses a method for blending epoxidized eucommia gum and damping rubber, wherein eucommia rubber and silicone rubber are blended and dissolved using toluene, deionized water is added to form a stable emulsion, and a composite material based on eucommia rubber is prepared by demulsification and drying. The emulsion system does not contain an emulsifier and the emulsion system is unstable. Chinese patent ZL201210332915.3 discloses a method for directly preparing polyisoprene latex using polyisoprene glue, wherein an anionic emulsification system is used to prepare polyisoprene latex through steps such as dissolution, emulsification, desolventization and concentration. Patent CN116891543A discloses a method for preparing artificial latex using a parallel-series continuous kettle distillation method, which greatly simplifies the process flow. Summary of the invention
[0005] The purpose of the present invention is to address the deficiencies of the prior art and provide a bio-based latex based on eucommia rubber and a preparation method thereof. The eucommia rubber is synchronously or asynchronously blended with blended rubbers such as cis-polyisoprene rubber, butadiene rubber, styrene-butadiene rubber and butyl rubber, then synchronously or asynchronously emulsified, and finally post-treated (including desolventizing and centrifugal concentration) to prepare the bio-based latex based on eucommia rubber. The bio-based latex based on eucommia rubber combines the performance advantages of soft and hard rubbers, and the preparation process is stable and reliable. The prepared bio-based latex based on eucommia rubber has excellent performance.
[0006] The present invention provides a method for preparing a bio-based latex based on eucommia rubber, which is carried out according to the following method: The eucommia rubber and the blended rubber are mixed by a synchronous mixing method to obtain a composite rubber liquid, or the eucommia rubber and the blended rubber are mixed by an asynchronous mixing method to obtain an eucommia rubber liquid and a blended rubber liquid respectively; The blended rubber is one of cis-polyisoprene rubber, butadiene rubber, styrene-butadiene rubber and butyl rubber; The composite rubber liquid is emulsified synchronously to obtain a composite crude emulsion; or, the eucommia rubber liquid and the blended rubber liquid are emulsified asynchronously to obtain a composite crude emulsion; The composite crude latex is post-treated to obtain a bio-based latex based on Eucommia rubber.
[0007] Preferably, the synchronous blending method is as follows: adding eucommia rubber and blended rubber into an organic solvent in proportion, heating and stirring, dissolving by reflux, and filtering to prepare a composite rubber glue solution; Asynchronous blending method: adding eucommia rubber to an organic solvent, heating and stirring, dissolving by reflux, filtering, and obtaining eucommia rubber glue liquid; adding the blended rubber to an organic solvent, and obtaining the blended rubber glue liquid under heating and stirring conditions.
[0008] Preferably, the synchronous blending method is specifically as follows: adding eucommia rubber and blended rubber to an organic solvent in proportion, stirring at 50°C to 60°C, refluxing and dissolving for 12h to 16h, and then removing insoluble matter in the eucommia rubber solid glue by suction filtration to prepare a composite rubber glue liquid, wherein the eucommia rubber accounts for 40% to 90% of the total mass of the rubber, the blended rubber accounts for 10% to 60% of the total mass of the rubber, and the total mass of the rubber accounts for 8% to 13% of the total mass of the composite rubber glue liquid; The asynchronous blending method is specifically as follows: adding eucommia rubber to an organic solvent, stirring at 50° C. to 60° C., refluxing to dissolve for 12 to 16 hours, and then removing insoluble matter in the eucommia rubber solid glue by suction filtration to prepare eucommia rubber glue liquid; adding the blended rubber to the solvent, stirring at 50° C. to 60° C. for 10 to 12 hours to obtain the blended rubber glue liquid; the eucommia rubber accounts for 40% to 90% of the total mass of the rubber, the blended rubber accounts for 10% to 60% of the total mass of the rubber, and the total mass of the rubber accounts for 8% to 13% of the total mass of the eucommia rubber glue liquid and the blended rubber glue liquid.
[0009] Preferably, the organic solvent is selected from C4 to C 10 The straight-chain alkane or cycloalkane is selected from natural eucommia rubber, trans-1,4-polyisoprene rubber, gutta-percha and balata gum; the number average molecular weight of eucommia rubber is 12,000 to 900,000; the cis-polyisoprene rubber is selected from natural hevea and cis-1,4-polyisoprene rubber; the butadiene rubber is selected from cis-1,4-polybutadiene rubber, trans-1,4-polybutadiene rubber, vinyl polybutadiene rubber and high cis-butadiene rubber; the styrene-butadiene rubber is selected from lithium-based styrene-butadiene rubber; the butyl rubber is selected from at least one of ordinary butyl rubber and brominated butyl rubber.
[0010] Preferably, the organic solvent is one or more of n-hexane, cyclohexane, n-pentane and cyclopentane; and the number average molecular weight of eucommia rubber is 300,000 to 600,000.
[0011] Preferably, the synchronous emulsification is specifically: 1) Prepare emulsifier aqueous solution Add the emulsifier to water, heat and stir at 55°C to 60°C for 4h to 8h, adjust the pH value to 10 to 12, and obtain a uniform and stable emulsifier aqueous solution, wherein the mass of the emulsifier accounts for 2% to 5% of the total mass of the emulsifier aqueous solution; 2) Synchronous emulsification The composite rubber glue and the emulsifier aqueous solution are emulsified in batches at a mass ratio of 1:1. The specific process is: at room temperature, first add a portion of the emulsifier aqueous solution to the composite rubber glue, and stir at a speed of 400r / min to 500r / min for 30min to 60min to form an oil-in-water pre-emulsified glue; then, add the remaining emulsifier aqueous solution to the oil-in-water pre-emulsified glue, and emulsify at a shear speed of 3000rpm to 4000rpm for 3min to 5min; subsequently, increase the shear speed to 4000rpm to 5000rpm, and shear homogenize for 5min to 10min to form a stable water-in-oil crude emulsion, i.e., a composite crude emulsion.
[0012] Preferably, the asynchronous emulsification is specifically: 1) Prepare emulsifier aqueous solution Add the emulsifier to water, heat and stir at 55°C to 60°C for 4h to 8h, adjust the pH value to 10 to 12, and obtain a uniform and stable emulsifier aqueous solution, wherein the mass of the emulsifier accounts for 2% to 5% of the total mass of the emulsifier aqueous solution; 2) Asynchronous emulsification The specific process is as follows: at room temperature, a portion of the emulsifier aqueous solution is added to the eucommia rubber liquid for pre-emulsification, and stirred at a speed of 450r / min to 500r / min for 45min to 60min to form an oil-in-water pre-emulsified liquid; then a portion of the emulsifier aqueous solution is added to the pre-emulsified liquid, and shear emulsification is performed at a shear speed of 3500rpm to 4000rpm for 4min to 10min; the shear speed is continuously increased for shear homogenization, and homogenization is performed at a shear speed of 4500rpm to 5000rpm for 7min to 10min to obtain a crude eucommia rubber emulsion; At room temperature, a portion of the emulsifier aqueous solution is added to the blended rubber glue for pre-emulsification, and stirred at a speed of 450 r / min to 500 r / min for 45 min to 60 min to form an oil-in-water pre-emulsified glue; then a portion of the emulsifier aqueous solution is added to the pre-emulsified glue, and shear emulsification is performed at a shear speed of 3500 rpm to 4000 rpm for 4 min to 10 min; the shear speed is continued to be increased for shear homogenization, and the shear speed is homogenized at a shear speed of 4500 rpm to 5000 rpm for 7 min to 10 min to obtain a blended rubber crude emulsion; The obtained eucommia rubber crude emulsion and the blended rubber crude emulsion are mixed, and stirred at 45° C. to 50° C. for 2 h to 4 h to form a stable oil-in-water crude emulsion, namely, a composite crude emulsion.
[0013] Preferably, the post-treatment of the composite crude emulsion includes: removing the organic solvent by atmospheric distillation, removing the residual organic solvent by reduced pressure distillation, and preparing the bio-based latex based on eucommia rubber by high-speed centrifugal concentration; specifically: The composite crude emulsion is subjected to atmospheric distillation at a distillation temperature of 45° C. to 82° C. and a distillation residence time of 6 h to 9 h to remove 80% to 90% of the total amount of the organic solvent; then, a reduced pressure distillation is performed at 60° C. to 80° C. and 60 KPa for 1 h to 1.5 h to remove the residual organic solvent to obtain a dilute emulsion; The dilute emulsion is centrifuged and concentrated at a rotation speed of 6000 rpm to 10000 rpm for 5 to 20 minutes to obtain a bio-based latex based on eucommia rubber.
[0014] Preferably, the emulsifier includes one or more of anionic surfactants and nonionic surfactants, the anionic surfactants include one or more of benzene sulfonates, rosin acid soaps, naphthalene sulfonates, fatty acid salts, and oleic acid soaps, and the nonionic surfactants include one or more of fatty alcohol polyoxyethylene ethers, fatty amine polyoxyethylene ethers, alkylphenol polyoxyethylene ethers, and sorbitan oleate.
[0015] In the present invention, the benzene sulfonate may be sodium dodecylbenzene sulfonate, the sorbitan oleate may be sorbitan monooleate, and the fatty alcohol polyoxyethylene ether may be fatty alcohol polyoxyethylene ether AEO.
[0016] The invention provides a bio-based latex based on eucommia rubber obtained by the preparation method.
[0017] The present invention uses eucommia rubber as a basic material, and uses cis-polyisoprene rubber, butadiene rubber, styrene-butadiene rubber, butyl rubber and other blended rubbers to prepare a bio-based latex based on eucommia rubber. Among them, one of the core innovations of the present invention is: first, eucommia rubber and the blended rubber are synchronously or asynchronously blended; then synchronously or asynchronously emulsified, and finally atmospheric distillation is performed to remove the solvent, vacuum distillation is performed to remove the residual solvent, and high-speed centrifugation is used for concentration, so as to prepare a bio-based latex based on eucommia rubber with complementary properties.
[0018] The method of the present invention is characterized in that eucommia rubber and blended rubber are blended to concentrate the excellent properties of the two, and the performance advantages of soft and hard rubber are integrated, and the preparation process is stable and reliable. A bio-based latex based on eucommia rubber is prepared by a solution emulsification method, and the types and proportions of eucommia rubber and blended rubber can be adjusted to form a highly fused composite latex with diverse performance, that is, a bio-based latex based on eucommia rubber. The bio-based latex based on eucommia rubber maintains the characteristics of high hardness and good shape memory of eucommia rubber, and at the same time has better tensile properties, broadening the application field of eucommia rubber. DETAILED DESCRIPTION
[0019] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in combination with the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0020] Unless otherwise specified, all raw materials, reagents, instruments, etc. used in this application can be purchased from the market or prepared by existing methods. Unless otherwise specified, the percentages in this application are all mass percentages. Normal temperature in this application generally refers to a temperature of 15°C to 25°C, generally defined as 25°C.
[0021] The present invention is described in detail below in conjunction with specific embodiments.
[0022] Examples 1-8 are for preparing the bio-based latex based on eucommia rubber by a synchronous method, and Examples 9-12 are for preparing the bio-based latex based on eucommia rubber by an asynchronous method.
[0023] Comparative Example 1: Preparation process of bio-based latex containing eucommia rubber Sol: Eucommia rubber (gutta-percha, number average molecular weight 2.5×10 4 ) was added into n-hexane, stirred and refluxed at 50°C for 12 hours to dissolve, and then the insoluble matter in the eucommia rubber solid gum was removed by suction filtration to prepare eucommia rubber liquid. The eucommia rubber content in the eucommia rubber liquid was 8%.
[0024] 2% sodium dodecylbenzene sulfonate and 3% sorbitan monooleate were added to water, heated and stirred at 55° C. for 4 h, and the pH was adjusted to 10 using KOH to obtain a uniform and stable emulsifier aqueous solution.
[0025] Emulsification process: the eucommia rubber glue liquid and the emulsifier aqueous solution are mixed and emulsified in a mass ratio of 1:1, specifically: at room temperature, first add 1 / 3 of the emulsifier aqueous solution to the eucommia rubber glue liquid for pre-emulsification, and stir at a speed of 400r / min for 30min to form an oil-in-water pre-emulsified glue liquid; then slowly add the remaining emulsifier aqueous solution, and shear emulsify at the same time, emulsify at a shear speed of 3000rpm for 3min; continue to increase the speed of the shear machine for shear homogenization, and homogenize at a shear speed of 4000rpm for 5min to form a stable water-in-oil crude emulsion; Distillation to remove organic solvent: A two-stage method is used to remove organic solvent (n-hexane) from the crude oil-in-water emulsion. First, atmospheric distillation is performed at a distillation temperature of 70°C and a residence time of 6 hours to remove 80% of the total amount of organic solvent; then vacuum distillation is performed at 80°C and 60KPa for 1 hour to remove residual organic solvent and obtain a dilute emulsion that contains almost no organic solvent.
[0026] The experimental data of removing organic solvents by atmospheric distillation are shown in Table 1.
[0027] High-speed centrifugal concentration: The dilute emulsion was subjected to high-speed centrifugation, with the centrifugal speed set at 6000 rpm and the centrifugal time set at 20 min, to prepare a bio-based latex containing eucommia rubber with a solid content of 50%.
[0028] Comparative Example 2: Preparation process of bio-based latex containing cis-polyisoprene rubber Sol: Add cis-polyisoprene rubber (natural Hevea gum) into n-hexane, heat and stir at 55°C for 4 hours to obtain cis-polyisoprene rubber sol. The cis-polyisoprene rubber content in the prepared cis-polyisoprene rubber sol is 8%.
[0029] 2% sodium dodecylbenzene sulfonate and 3% sorbitan monooleate were added to water, heated and stirred at 55° C. for 4 h, and the pH was adjusted to 10 using KOH to obtain a uniform and stable emulsifier aqueous solution.
[0030] Emulsification process: the cis-polyisoprene rubber glue and the emulsifier aqueous solution are mixed and emulsified in a mass ratio of 1:1, specifically: at room temperature, first, 1 / 3 of the emulsifier aqueous solution is added to the cis-polyisoprene rubber glue for pre-emulsification, and stirred at a speed of 400r / min for 30min to form an oil-in-water pre-emulsified glue; then the remaining emulsifier aqueous solution is slowly added, and shear emulsification is performed at the same time, and emulsification is performed at a shear speed of 3000rpm for 3min; the shear speed is continued to be increased for shear homogenization, and homogenization is performed at a shear speed of 4000rpm for 5min to form a stable water-in-oil crude emulsion; Distillation to remove organic solvent: A two-stage method is used to remove organic solvent (n-hexane) from the crude oil-in-water emulsion. First, atmospheric distillation is performed at a distillation temperature of 70°C and a residence time of 6 hours to remove 80% of the total amount of organic solvent; then vacuum distillation is performed at 80°C and 60KPa for 1 hour to remove the residual organic solvent and obtain a dilute emulsion that is almost free of solvent.
[0031] The experimental data of removing solvent by atmospheric distillation are shown in Table 1.
[0032] High-speed centrifugal concentration: The dilute emulsion is subjected to high-speed centrifugation, the centrifugal speed is set to 6000 rpm, the centrifugal time is set to 20 minutes, and a cis-polyisoprene rubber bio-based latex with a solid content of 50% is prepared.
[0033] Example 1: Synchronous preparation of bio-based latex based on Eucommia rubber (Eucommia rubber / cis-polyisoprene rubber composite latex) Synchronous blending: Eucommia rubber (gutta-percha, number average molecular weight 2.5×10 4 ) and cis-1,4-polyisoprene rubber are added to n-hexane, stirred and refluxed to dissolve at 50°C for 12 hours, then centrifuged at 6000rpm for 5 minutes, and vacuum filtered to prepare a composite rubber solution, wherein the eucommia rubber accounts for 40% of the total mass of the rubber, and the total mass of the rubber accounts for 8% of the mass of the composite rubber solution.
[0034] 2% sodium dodecylbenzene sulfonate and 3% sorbitan monooleate were added to water, heated and stirred at 55° C. for 4 h, and the pH was adjusted to 10 using KOH to obtain a uniform and stable emulsifier aqueous solution.
[0035] Synchronous emulsification process: the composite rubber glue and the emulsifier aqueous solution are synchronously emulsified in a mass ratio of 1:1: at room temperature, first add 1 / 3 of the emulsifier aqueous solution to the composite rubber glue for pre-emulsification, and stir at a speed of 400r / min for 30min to form an oil-in-water pre-emulsified glue; then slowly add the remaining emulsifier aqueous solution and shear emulsify at the same time, emulsify at a shear speed of 3000rpm for 3min; continue to increase the shear speed for shear homogenization, and homogenize at a shear speed of 4000rpm for 5min to form a stable water-in-oil crude emulsion; Distillation to remove organic solvent: A two-stage method is used to remove organic solvent (n-hexane) from the crude oil-in-water emulsion. First, atmospheric distillation is performed at a distillation temperature of 45°C and a residence time of 6 hours to remove 80% of the total amount of organic solvent; then vacuum distillation is performed at 80°C and 60KPa for 1 hour to remove residual organic solvent and obtain a dilute emulsion that is almost free of solvent.
[0036] The experimental data of removing solvent by atmospheric distillation are shown in Table 1.
[0037] High-speed centrifugal concentration: The dilute emulsion is subjected to high-speed centrifugation, with the centrifugal speed set at 6000 rpm and the centrifugal time set at 20 min, to prepare a eucommia rubber-based bio-based latex with a solid content of 50%, namely, eucommia rubber / cis-polyisoprene rubber composite latex.
[0038] Example 2: Preparation of bio-based latex based on Eucommia rubber (Eucommia rubber / high cis-butadiene rubber composite latex) by simultaneous method Synchronous blending: Eucommia rubber (gutta-percha, number average molecular weight 2.5×10 4 ) and high cis-butadiene rubber are added into n-hexane, stirred and refluxed to dissolve at 55°C for 14 hours, and then the insoluble matter in the eucommia rubber solid gum is removed by suction filtration to prepare a composite rubber liquid, in which the eucommia rubber accounts for 65% of the total mass of the rubber, and the total mass of the rubber accounts for 10% of the mass of the composite rubber liquid.
[0039] 2% sodium dodecylbenzene sulfonate and 2% sorbitan monooleate were added to water, heated and stirred at 58° C. for 6 h, and the pH was adjusted to 11 using KOH to obtain a uniform and stable emulsifier aqueous solution.
[0040] Synchronous emulsification process: The composite rubber glue and the emulsifier aqueous solution are synchronously emulsified in a mass ratio of 1:1: At room temperature, firstly, add 1 / 3 of the emulsifier aqueous solution to the composite rubber glue for pre-emulsification, and stir at a speed of 450r / min for 45 minutes to form an oil-in-water pre-emulsified glue; then slowly add the remaining emulsifier aqueous solution and shear emulsify at the same time, emulsify at a shear speed of 3500rpm for 4 minutes; continue to increase the speed of the shear machine for shear homogenization, and homogenize at a shear speed of 4500rpm for 7 minutes to form a stable water-in-oil crude emulsion; Distillation to remove organic solvent: A two-stage method is used to remove organic solvent from the crude oil-in-water emulsion. First, atmospheric distillation is performed at a distillation temperature of 71°C and a residence time of 7 hours to remove 85% of the total amount of organic solvent. Then, reduced pressure distillation is performed at 80°C and 60KPa for 1.5 hours to remove residual organic solvent and obtain a dilute emulsion that is almost free of solvent.
[0041] The experimental data of removing solvent by atmospheric distillation are shown in Table 1.
[0042] High-speed centrifugal concentration: The dilute emulsion is subjected to high-speed centrifugation, with the centrifugal speed set at 8000 rpm and the centrifugal time set at 10 min, to prepare a eucommia rubber-based bio-based latex with a solid content of 55%, namely, eucommia rubber / high cis-butadiene rubber composite latex.
[0043] Example 3: Synchronous preparation of bio-based latex based on Eucommia rubber (Eucommia rubber / lithium-based styrene-butadiene rubber composite latex) Synchronous blending: Eucommia rubber (balata gum, number average molecular weight 1.5×10 4 ) and lithium-based styrene-butadiene rubber are added into cyclohexane, stirred and refluxed for dissolution at 60°C for 16 hours, and then the insoluble matter in the eucommia rubber solid gum is removed by suction filtration to prepare a composite rubber glue liquid, in which the eucommia rubber accounts for 90% of the total mass of the rubber, and the total mass of the rubber accounts for 13% of the mass of the composite rubber glue liquid.
[0044] 1% sodium dodecylbenzene sulfonate and 1% sorbitan monooleate were added to water, heated and stirred at 60°C for 8 hours, and the pH was adjusted to 12 using KOH to obtain a uniform and stable emulsifier aqueous solution.
[0045] Synchronous emulsification process: the composite rubber glue and the emulsifier aqueous solution are synchronously emulsified in batches according to a mass ratio of 1:1: at room temperature, first add 1 / 3 of the emulsifier aqueous solution to the composite rubber glue for pre-emulsification, and stir at a speed of 500r / min for 60min to form an oil-in-water pre-emulsified glue; then slowly add the remaining emulsifier aqueous solution, and shear emulsify at the same time, emulsify at a shear speed of 4000rpm for 5min; continue to increase the shear speed for shear homogenization, and homogenize at a shear speed of 5000rpm for 10min to form a stable water-in-oil crude emulsion; Distillation to remove organic solvent: A two-stage method is used to remove organic solvent from the crude oil-in-water emulsion. First, atmospheric distillation is performed at a distillation temperature of 82°C and a residence time of 8 hours to remove 90% of the total amount of organic solvent. Then, reduced pressure distillation is performed at 80°C and 60KPa for 1 hour to remove residual organic solvent and obtain a dilute emulsion that is almost free of solvent.
[0046] The experimental data of removing solvent by atmospheric distillation are shown in Table 1.
[0047] High-speed centrifugal concentration: The dilute emulsion is subjected to high-speed centrifugation, the centrifugal speed is set to 10000 rpm, the centrifugal time is set to 5 minutes, and a bio-based latex based on eucommia rubber with a solid content of 60% is prepared, namely, eucommia rubber / lithium-based styrene-butadiene rubber composite latex.
[0048] Example 4: Preparation of Eucommia Rubber-Based Bio-Based Latex (Eucommia Rubber / Butyl Rubber Composite Latex) by Synchronous Method Synchronous blending: Eucommia rubber (balata gum, number average molecular weight 1.5×10 4 ) and butyl rubber (ordinary butyl rubber) are added into n-hexane, stirred and refluxed to dissolve at 60°C for 16 hours, and then the insoluble matter in the eucommia rubber solid gum is removed by suction filtration to prepare a composite rubber glue liquid, in which the eucommia rubber accounts for 70% of the total mass of the rubber, and the total mass of the rubber accounts for 12% of the mass of the composite rubber glue liquid.
[0049] 1% sodium dodecylbenzene sulfonate and 1% sorbitan monooleate were added to water, heated and stirred at 60°C for 8 hours, and the pH was adjusted to 12 using KOH to obtain a uniform and stable emulsifier aqueous solution.
[0050] Synchronous emulsification process: the composite rubber glue and the emulsifier aqueous solution are synchronously emulsified in batches according to a mass ratio of 1:1: at room temperature, first add 1 / 3 of the emulsifier aqueous solution to the composite rubber glue for pre-emulsification, and stir at a speed of 500r / min for 60min to form an oil-in-water pre-emulsified glue; then slowly add the remaining emulsifier aqueous solution and shear emulsify at the same time, emulsify at a shear speed of 4000rpm for 5min; continue to increase the speed of the shear machine for shear homogenization, and homogenize at a shear speed of 5000rpm for 10min to form a stable water-in-oil crude emulsion; Distillation to remove organic solvent: A two-stage method is used to remove organic solvent from the crude oil-in-water emulsion. First, atmospheric distillation is performed at a distillation temperature of 45°C and a residence time of 8 hours to remove 90% of the total amount of organic solvent. Then, reduced pressure distillation is performed at 60°C and 60KPa for 1 hour to remove residual organic solvent and obtain a dilute emulsion that is almost free of solvent.
[0051] The experimental data of removing solvent by atmospheric distillation are shown in Table 1.
[0052] High-speed centrifugal concentration: The dilute emulsion is subjected to high-speed centrifugation, with the centrifugal speed set at 10,000 rpm and the centrifugal time set at 5 min, to prepare a eucommia rubber-based bio-based latex having a solid content of 60%, namely, eucommia rubber / butyl rubber composite latex.
[0053] Example 5: Synchronous preparation of bio-based latex based on Eucommia rubber (Eucommia rubber / cis-polyisoprene rubber composite latex) Synchronous blending: Eucommia rubber (trans-1,4-polyisoprene rubber, number average molecular weight 1.7×10 4 ) and cis-1,4-polyisoprene rubber are added into n-pentane, stirred and refluxed for dissolution at 50°C for 12 hours, and then the insoluble matter in the eucommia rubber solid gum is removed by suction filtration to prepare a composite rubber liquid, in which the eucommia rubber accounts for 60% of the total mass of the rubber, and the total mass of the rubber accounts for 9% of the mass of the composite rubber liquid.
[0054] 2% sodium dodecylbenzene sulfonate and 3% sorbitan monooleate were added to water, heated and stirred at 55° C. for 4 h, and the pH was adjusted to 10 using KOH to obtain a uniform and stable emulsifier aqueous solution.
[0055] Synchronous emulsification process: the composite rubber glue and the emulsifier aqueous solution are synchronously emulsified in batches according to a mass ratio of 1:1: at room temperature, first add 1 / 3 of the emulsifier aqueous solution to the composite rubber glue for pre-emulsification, and stir at a speed of 400r / min for 30min to form an oil-in-water pre-emulsified glue; then slowly add the remaining emulsifier aqueous solution and shear emulsify at the same time, emulsify at a shear speed of 3000rpm for 3min; continue to increase the shear speed for shear homogenization, and homogenize at a shear speed of 4000rpm for 5min to form a stable water-in-oil crude emulsion; Distillation to remove organic solvent: A two-stage method is used to remove organic solvent from the crude oil-in-water emulsion. First, atmospheric distillation is performed at a distillation temperature of 45°C and a residence time of 7 hours to remove 80% of the total amount of organic solvent. Then, reduced pressure distillation is performed at 80°C and 60KPa for 1.5 hours to remove residual organic solvent and obtain a dilute emulsion that is almost free of solvent.
[0056] The experimental data of removing solvent by atmospheric distillation are shown in Table 1.
[0057] High-speed centrifugal concentration: The dilute emulsion is subjected to high-speed centrifugation, with the centrifugal speed set at 6000 rpm and the centrifugal time set at 20 min, to prepare a eucommia rubber-based bio-based latex with a solid content of 50%, namely, eucommia rubber / cis-polyisoprene rubber composite latex.
[0058] Example 6: Preparation of bio-based latex based on Eucommia rubber (Eucommia rubber / high cis-butadiene rubber composite latex) by simultaneous method Synchronous blending: Eucommia rubber (trans-1,4-polyisoprene rubber, number average molecular weight 1.7×10 4 ) and high cis-butadiene rubber are added into n-pentane, stirred and refluxed for dissolution at 55°C for 14 hours, and then the insoluble matter in the eucommia rubber solid gum is removed by suction filtration to prepare a composite rubber liquid, in which the eucommia rubber accounts for 80% of the total mass of the rubber, and the total mass of the rubber accounts for 10% of the mass of the composite rubber liquid.
[0059] 2% sodium dodecylbenzene sulfonate and 2% fatty alcohol polyoxyethylene ether AEO were added to water, heated and stirred at 58°C for 6 hours, and the pH was adjusted to 11 using KOH to obtain a uniform and stable emulsifier aqueous solution.
[0060] Synchronous emulsification process: the composite rubber glue and the emulsifier aqueous solution are synchronously emulsified in batches according to a mass ratio of 1:1: at room temperature, first add 1 / 3 of the emulsifier aqueous solution to the composite rubber glue for pre-emulsification, and stir at a speed of 450r / min for 45min to form an oil-in-water pre-emulsified glue; then slowly add the remaining emulsifier aqueous solution and shear emulsify at the same time, emulsify at a shear speed of 3500rpm for 4min; continue to increase the shear speed for shear homogenization, and homogenize at a shear speed of 4500rpm for 7min to form a stable water-in-oil crude emulsion; Distillation to remove organic solvent: A two-stage method is used to remove organic solvent from the crude oil-in-water emulsion. First, atmospheric distillation is performed at a distillation temperature of 48°C and a residence time of 8 hours to remove 85% of the total amount of organic solvent. Then, reduced pressure distillation is performed at 80°C and 60KPa for 1 hour to remove residual organic solvent and obtain a dilute emulsion that is almost free of solvent.
[0061] The experimental data of removing solvent by atmospheric distillation are shown in Table 1.
[0062] High-speed centrifugal concentration: The dilute emulsion is subjected to high-speed centrifugation, with the centrifugal speed set at 8000 rpm and the centrifugal time set at 10 min, to prepare a eucommia rubber-based bio-based latex with a solid content of 55%, namely, eucommia rubber / high cis-butadiene rubber composite latex.
[0063] Example 7: Synchronous preparation of bio-based latex based on Eucommia rubber (Eucommia rubber / lithium-based styrene-butadiene rubber composite latex) Synchronous blending: Eucommia rubber (gutta-percha, number average molecular weight 2.5×10 4 ) and lithium-based styrene-butadiene rubber are added into cyclopentane, stirred and refluxed for dissolution at 60°C for 16 hours, and then the insoluble matter in the eucommia rubber solid gum is removed by suction filtration to prepare a composite rubber glue liquid, in which the eucommia rubber accounts for 50% of the total mass of the rubber, and the total mass of the rubber accounts for 12% of the mass of the composite rubber glue liquid.
[0064] 1% sodium dodecylbenzene sulfonate and 1% sorbitan monooleate were added to water, heated and stirred at 60°C for 4 hours, and the pH was adjusted to 12 using KOH to obtain a uniform and stable emulsifier aqueous solution.
[0065] Synchronous emulsification: The composite rubber glue and the emulsifier aqueous solution are synchronously emulsified in batches according to a mass ratio of 1:1: at room temperature, first add 1 / 3 of the emulsifier aqueous solution to the composite rubber glue for pre-emulsification, and stir at a speed of 500r / min for 60min to form an oil-in-water pre-emulsified glue; then slowly add the remaining emulsifier aqueous solution and shear emulsify at the same time, emulsify at a shear speed of 4000rpm for 5min; continue to increase the speed of the shear machine for shear homogenization, and homogenize at a shear speed of 5000rpm for 10min to form a stable water-in-oil crude emulsion; Distillation to remove organic solvent: A two-stage method is used to remove organic solvent from the crude oil-in-water emulsion. First, atmospheric distillation is performed at a distillation temperature of 72°C and a residence time of 9 hours to remove 90% of the total amount of organic solvent. Then, reduced pressure distillation is performed at 80°C and 60KPa for 1 hour to remove residual organic solvent and obtain a dilute emulsion that is almost free of solvent.
[0066] The experimental data of removing solvent by atmospheric distillation are shown in Table 1.
[0067] High-speed centrifugal concentration: The dilute emulsion is subjected to high-speed centrifugation, the centrifugal speed is set to 10000 rpm, the centrifugal time is set to 5 minutes, and a bio-based latex based on eucommia rubber with a solid content of 60% is prepared, namely, eucommia rubber / lithium-based styrene-butadiene rubber composite latex.
[0068] Example 8: Preparation of bio-based latex based on Eucommia rubber (Eucommia rubber / butyl rubber composite latex) by simultaneous method Synchronous blending: Eucommia rubber (gutta-percha, number average molecular weight 2.5×10 4 ) and butyl rubber (bromobutyl rubber) are added into n-pentane, stirred and refluxed to dissolve at 50°C for 16 hours, and then the insoluble matter in the eucommia rubber solid gum is removed by suction filtration to prepare a composite rubber glue liquid, in which the eucommia rubber accounts for 40% of the total mass of the rubber, and the total mass of the rubber accounts for 12% of the mass of the composite rubber glue liquid.
[0069] 1% sodium dodecylbenzene sulfonate and 1% sorbitan monooleate were added to water, heated and stirred at 55° C. for 8 h, and the pH was adjusted to 12 using KOH to obtain a uniform and stable emulsifier aqueous solution.
[0070] Synchronous emulsification: The composite rubber glue and the emulsifier aqueous solution are synchronously emulsified in batches according to a mass ratio of 1:1: at room temperature, first add 1 / 3 of the emulsifier aqueous solution to the composite rubber glue for pre-emulsification, and stir at a speed of 500r / min for 60min to form an oil-in-water pre-emulsified glue; then slowly add the remaining emulsifier aqueous solution and shear emulsify at the same time, emulsify at a shear speed of 4000rpm for 5min; continue to increase the speed of the shear machine for shear homogenization, and homogenize at a shear speed of 5000rpm for 10min to form a stable water-in-oil crude emulsion; Distillation to remove organic solvent: A two-stage method is used to remove organic solvent from the crude oil-in-water emulsion. First, atmospheric distillation is performed at a distillation temperature of 50°C and a residence time of 9 hours to remove 90% of the total amount of organic solvent. Then, reduced pressure distillation is performed at 80°C and 60KPa for 1 hour to remove residual organic solvent and obtain a dilute emulsion that is almost free of solvent.
[0071] The experimental data of removing solvent by atmospheric distillation are shown in Table 1.
[0072] High-speed centrifugal concentration: The dilute emulsion is subjected to high-speed centrifugation, with the centrifugal speed set at 10,000 rpm and the centrifugal time set at 5 min, to prepare a eucommia rubber-based bio-based latex having a solid content of 60%, namely, eucommia rubber / butyl rubber composite latex.
[0073] Example 9: Preparation of bio-based latex based on Eucommia rubber (Eucommia rubber / cis-polyisoprene rubber composite latex) by asynchronous method Asynchronous blending: Eucommia rubber (gutta-percha, number average molecular weight 2.5×10 4 ) was added into n-hexane, stirred and refluxed at 50°C for 12 hours to dissolve, and then the insoluble matter in the eucommia rubber solid gum was removed by suction filtration to prepare eucommia rubber liquid, and cis-polyisoprene rubber (cis-1,4-polyisoprene rubber) was added into hexane, stirred at 50°C for 10 hours to obtain cis-polyisoprene rubber liquid.
[0074] The eucommia rubber accounts for 40% of the total mass of the rubber, and the total mass of the rubber accounts for 8% of the total mass of the eucommia rubber liquid and the mixed rubber liquid.
[0075] 1% sodium dodecylbenzene sulfonate and 1% sorbitan monooleate were added to water, heated and stirred at 60°C for 4 hours, and the pH was adjusted to 12 using KOH to obtain a uniform and stable emulsifier aqueous solution. The emulsifier aqueous solution was divided into two parts.
[0076] Asynchronous emulsification process: asynchronous emulsification of eucommia rubber liquid and cis-polyisoprene rubber liquid: at room temperature, first, add 1 / 3 of an emulsifier aqueous solution to the eucommia rubber liquid for pre-emulsification, and stir at a speed of 450r / min for 45min to form an oil-in-water pre-emulsified liquid; then slowly add the remaining emulsifier aqueous solution and shear emulsify at the same time, emulsify at a shear speed of 3500rpm for 4min; continue to increase the speed of the shear machine for shear homogenization, and homogenize at a shear speed of 4500rpm for 7min to obtain a eucommia rubber crude emulsion; At room temperature, first, add 1 / 3 of another emulsifier aqueous solution to the cis-polyisoprene rubber glue for pre-emulsification, and stir at a speed of 450r / min for 45 minutes to form an oil-in-water pre-emulsified glue; then slowly add the remaining emulsifier aqueous solution and shear emulsify at the same time, emulsify at a shear speed of 3500rpm for 4 minutes; continue to increase the shear speed for shear homogenization, homogenize at a shear speed of 4500rpm for 7 minutes to obtain a crude emulsion containing cis-polyisoprene; mix the obtained eucommia rubber crude emulsion and cis-polyisoprene rubber crude emulsion, stir at 45°C for 2h, and prepare a water-in-oil crude emulsion, that is, a composite crude emulsion.
[0077] Distillation to remove organic solvent: A two-stage method is used to remove organic solvent from the crude oil-in-water emulsion. First, atmospheric distillation is performed at a distillation temperature of 71°C and a residence time of 7 hours to remove 85% of the total amount of organic solvent. Then, reduced pressure distillation is performed at 80°C and 60KPa for 1 hour to remove residual organic solvent and obtain a dilute emulsion that is almost free of solvent.
[0078] The experimental data of removing solvent by atmospheric distillation are shown in Table 1.
[0079] High-speed centrifugal concentration: The dilute emulsion is subjected to high-speed centrifugation, with the centrifugal speed set at 6000 rpm and the centrifugal time set at 20 min, to prepare a eucommia rubber-based bio-based latex having a solid content of 60%, namely, eucommia rubber / cis-polyisoprene rubber composite latex.
[0080] Example 10: Preparation of bio-based latex based on Eucommia rubber (Eucommia rubber / high cis-butadiene rubber composite latex) by asynchronous method Asynchronous blending: Eucommia rubber (balata gum, number average molecular weight 2.5×10 4 ) was added into n-hexane, stirred and refluxed at 50°C for 16 hours to dissolve, and then the insoluble matter in the eucommia rubber solid gum was removed by suction filtration to prepare eucommia rubber liquid. High cis-butadiene rubber was added into n-hexane, stirred at 50°C for 10 hours to obtain butadiene rubber liquid.
[0081] The eucommia rubber accounts for 60% of the total mass of rubber, and the total mass of rubber accounts for 13% of the total mass of the eucommia rubber liquid and the mixed rubber liquid.
[0082] 1% sodium dodecylbenzene sulfonate and 1% sorbitan monooleate were added to water, heated and stirred at 55°C for 8 hours, and the pH was adjusted to 12 using KOH to obtain a uniform and stable emulsifier aqueous solution. The emulsifier aqueous solution was divided into two parts.
[0083] Asynchronous emulsification process: asynchronously emulsify the eucommia rubber liquid and the butadiene rubber liquid: at room temperature, add 1 / 3 of the emulsifier aqueous solution to the eucommia rubber liquid for pre-emulsification, stir at a speed of 500r / min for 60min to form an oil-in-water pre-emulsified liquid; then slowly add the remaining emulsifier aqueous solution and shear emulsify at the same time, emulsify at a shear speed of 4000rpm for 10min; continue to increase the speed of the shear machine for shear homogenization, homogenize at a shear speed of 5000rpm for 10min to obtain a eucommia rubber crude emulsion; At room temperature, add 1 / 3 of another emulsifier aqueous solution to the butadiene rubber glue for pre-emulsification, and stir at a speed of 500r / min for 60min to form an oil-in-water pre-emulsified glue; then slowly add the remaining emulsifier aqueous solution and shear emulsify at the same time, emulsify at a shear speed of 4000rpm for 10min; continue to increase the shear speed for shear homogenization, homogenize at a shear speed of 5000rpm for 10min to obtain a crude emulsion containing butadiene; mix the obtained eucommia rubber crude emulsion and butadiene rubber crude emulsion, stir at 50°C for 2h, and prepare a water-in-oil crude emulsion, i.e., a composite crude emulsion.
[0084] Distillation to remove organic solvent: A two-stage method is used to remove organic solvent from the crude oil-in-water emulsion. First, atmospheric distillation is performed at a distillation temperature of 71°C and a residence time of 7 hours to remove 85% of the total amount of organic solvent. Then, reduced pressure distillation is performed at 60°C and 60KPa for 1.5 hours to remove residual organic solvent and obtain a dilute emulsion that is almost free of solvent.
[0085] The experimental data of removing solvent by atmospheric distillation are shown in Table 1.
[0086] High-speed centrifugal concentration: The dilute emulsion is subjected to high-speed centrifugation, with the centrifugal speed set at 8000 rpm and the centrifugal time set at 10 min, to prepare a eucommia rubber-based bio-based latex with a solid content of 60%, namely, eucommia rubber / high cis-butadiene rubber composite latex.
[0087] Example 11: Preparation of bio-based latex based on Eucommia rubber (Eucommia rubber / lithium-based styrene-butadiene rubber composite latex) by asynchronous method Asynchronous blending: Eucommia rubber (balata gum, number average molecular weight 2.5×10 4) was added into n-hexane, stirred and refluxed at 50°C for 14 hours to dissolve, and then the insoluble matter in the eucommia rubber solid gum was removed by suction filtration to prepare eucommia rubber liquid. Lithium-based styrene-butadiene rubber was added into n-hexane, stirred at 60°C for 10 hours to obtain styrene-butadiene rubber liquid.
[0088] The eucommia rubber accounts for 65% of the total mass of the rubber, and the total mass of the rubber accounts for 10% of the total mass of the eucommia rubber liquid and the mixed rubber liquid.
[0089] 1% sodium dodecylbenzene sulfonate and 1% sorbitan monooleate were added to water, heated and stirred at 60°C for 8 hours, and the pH was adjusted to 12 using KOH to obtain a uniform and stable emulsifier aqueous solution. The emulsifier aqueous solution was divided into two parts.
[0090] Asynchronous emulsification process: asynchronous emulsification of eucommia rubber liquid and styrene-butadiene rubber liquid: at room temperature, 1 / 3 of the emulsifier aqueous solution is added to the eucommia rubber liquid for pre-emulsification, and stirred at a speed of 450r / min for 45min to form an oil-in-water pre-emulsified liquid; then the remaining emulsifier aqueous solution is slowly added and sheared and emulsified at the same time, and the emulsification is carried out at a shear speed of 3500rpm for 4min; the shear speed is continued to be increased for shear homogenization, and the homogenization is carried out at a shear speed of 4500rpm for 7min to obtain a crude eucommia rubber emulsion; At room temperature, add 1 / 3 of another emulsifier aqueous solution to the styrene-butadiene rubber glue for pre-emulsification, and stir at a speed of 450r / min for 45 minutes to form an oil-in-water pre-emulsified glue; then slowly add the remaining emulsifier aqueous solution and shear emulsify at the same time, emulsify at a shear speed of 3500rpm for 4 minutes; continue to increase the shear speed for shear homogenization, homogenize at a shear speed of 4500rpm for 7 minutes to obtain a crude emulsion containing styrene-butadiene rubber; mix the obtained eucommia rubber crude emulsion and styrene-butadiene rubber crude emulsion, stir at 50°C for 4 hours, and prepare a stable water-in-oil crude emulsion, i.e., a composite crude emulsion.
[0091] Distillation to remove organic solvent: A two-stage method is used to remove organic solvent from the crude oil-in-water emulsion. First, atmospheric distillation is performed at a distillation temperature of 72°C and a residence time of 9 hours to remove 85% of the total amount of organic solvent. Then, reduced pressure distillation is performed at 80°C and 60KPa for 1 hour to remove residual organic solvent and obtain a dilute emulsion that is almost free of solvent.
[0092] The experimental data of removing solvent by atmospheric distillation are shown in Table 1.
[0093] High-speed centrifugal concentration: The dilute emulsion is subjected to high-speed centrifugation, with the centrifugal speed set at 10,000 rpm and the centrifugal time set at 10 min, to prepare a eucommia rubber-based bio-based latex with a solid content of 60%, namely, eucommia rubber / lithium-based styrene-butadiene rubber composite latex.
[0094] Example 12: Preparation of Eucommia Rubber-Based Bio-Based Latex (Eucommia Rubber / Butyl Rubber Composite Latex) by Asynchronous Method Asynchronous blending: Eucommia rubber (balata gum, number average molecular weight 2.5×10 4 ) was added into n-hexane, stirred and refluxed at 60°C for 16 hours to dissolve, and then the insoluble matter in the eucommia rubber solid gum was removed by suction filtration to prepare eucommia rubber liquid. Butyl rubber (bromobutyl rubber) was added into n-hexane, stirred at 50°C for 12 hours to obtain butyl rubber liquid.
[0095] The eucommia rubber accounts for 90% of the total mass of rubber, and the total mass of rubber accounts for 8% of the total mass of the eucommia rubber liquid and the mixed rubber liquid.
[0096] 1% sodium dodecylbenzene sulfonate and 1% sorbitan monooleate were added to water, heated and stirred at 60°C for 8 hours, and the pH was adjusted to 12 using KOH to obtain a uniform and stable emulsifier aqueous solution. The emulsifier aqueous solution was divided into two parts.
[0097] Asynchronous emulsification process: asynchronous emulsification of eucommia rubber liquid and butyl rubber liquid: at room temperature, 1 / 3 of the emulsifier aqueous solution is added to the eucommia rubber liquid for pre-emulsification, and stirred at a speed of 450r / min for 45min to form an oil-in-water pre-emulsified liquid; then the remaining emulsifier aqueous solution is slowly added and sheared and emulsified at the same time, and the emulsification is carried out at a shear speed of 3500rpm for 4min; the shear speed is continued to be increased for shear homogenization, and the homogenization is carried out at a shear speed of 4500rpm for 7min to obtain a crude eucommia rubber emulsion; At room temperature, add 1 / 3 of another emulsifier aqueous solution to the butyl rubber glue for pre-emulsification, and stir at a speed of 450r / min for 45 minutes to form an oil-in-water pre-emulsified glue; then slowly add the remaining emulsifier aqueous solution and shear emulsify at the same time, emulsify at a shear speed of 3500rpm for 4 minutes; continue to increase the shear speed for shear homogenization, homogenize at a shear speed of 4500rpm for 7 minutes to obtain a crude emulsion containing butyl rubber; mix the obtained eucommia rubber crude emulsion and butyl rubber crude emulsion, stir at 45°C for 4 hours, and prepare a stable water-in-oil crude emulsion, i.e., a composite crude emulsion.
[0098] Distillation to remove organic solvent: A two-stage method is used to remove organic solvent from the crude oil-in-water emulsion. First, atmospheric distillation is performed at a distillation temperature of 45°C and a residence time of 9 hours to remove 85% of the total amount of organic solvent. Then, reduced pressure distillation is performed at 80°C and 60KPa for 1 hour to remove residual organic solvent and obtain a dilute emulsion that is almost free of solvent.
[0099] The experimental data of removing solvent by atmospheric distillation are shown in Table 1.
[0100] High-speed centrifugal concentration: The dilute emulsion is subjected to high-speed centrifugation, with the centrifugal speed set at 8000 rpm and the centrifugal time set at 10 min, to prepare a eucommia rubber-based bio-based latex having a solid content of 60%, namely, eucommia rubber / butyl rubber composite latex.
[0101] Embodiment 13: According to the method of Example 1, a bio-based latex based on eucommia rubber (eucommia rubber / cis-polyisoprene rubber composite latex) was prepared by a synchronous method, wherein the mass ratio of the two rubbers was 5:95, and then a composite sponge was prepared: 170 parts of eucommia rubber / cis-polyisoprene rubber composite latex, 2.5 parts of sulfur, 1.0 part of accelerator ZDC (zinc diethyldithiocarbamate), 1.0 part of accelerator PX (zinc N-ethyl-N-phenyldithiocarbamate), 2.0 parts of antioxidant D (N-phenyl-2-naphthylamine), 0.0 parts of peregrin, and 1.0 parts of chlorinated parathion. 0.12 parts, 1.2 parts of potassium oleate, 1.6 parts of hexadecyltrimethylammonium bromide, stirring and ripening at 35°C for 8 hours to obtain a composite glue; the composite glue is stirred at a speed of 1500 rpm, and air is filled in at the same time to quickly foam to a specified volume, then slowly foamed at 100 rpm, and then 8 parts of activator zinc oxide diluted with soft water are added, and the foam is treated at a medium speed of 200 rpm for 2 minutes, 2 parts of sodium fluorsilicate and 0.15 parts of potassium hydroxide mixed with aqueous liquid are added together, and the foam is treated at a medium speed of 400 rpm for another 2 minutes, and the foam is evenly injected into a mold sprayed with release agent talcum powder, and solidified at 90°C for about 30 minutes. After vulcanization at 110°C to 120°C for 40 minutes, it is washed, dehydrated, and dried at 60°C to 80°C for 4 hours to obtain a composite sponge.
[0102] Embodiment 14: According to the method of Example 7, a bio-based latex based on eucommia rubber (eucommia rubber / lithium-based styrene-butadiene rubber composite latex) was prepared by a synchronous method, wherein the mass ratio of the two rubbers was 10:90, and then a composite sponge was prepared: 170 parts of eucommia rubber / lithium-based styrene-butadiene rubber composite latex, 2.5 parts of sulfur, 1.0 part of accelerator ZDC (zinc diethyldithiocarbamate), 1.0 part of accelerator PX (zinc N-ethyl-N-phenyldithiocarbamate), 2.0 parts of antioxidant D (N-phenyl-2-naphthylamine), 0.0 parts of peregrine, 1.0 parts of chlorinated parathion, 1.0 parts of sodium pyrochlore, 1.0 parts of sodium pyrochlore and 1.0 parts of sodium pyrochlore. 0.12 parts, 1.2 parts of potassium oleate, 1.6 parts of hexadecyltrimethylammonium bromide, stirring and ripening at 35°C for 8 hours to obtain a composite glue; the composite glue is stirred at a speed of 1500 rpm, and air is filled in at the same time to quickly foam to a specified volume, then slowly foamed at 100 rpm, and then 8 parts of activator zinc oxide diluted with soft water are added, and the foam is treated at a medium speed of 200 rpm for 2 minutes, 2 parts of sodium fluorsilicate and 0.15 parts of potassium hydroxide mixed with aqueous liquid are added together, and the foam is treated at a medium speed of 400 rpm for another 2 minutes, and the foam is evenly injected into a mold sprayed with release agent talcum powder, and solidified at 90°C for about 30 minutes. After vulcanization at 110°C to 120°C for 40 minutes, it is washed, dehydrated, and dried at 60°C to 80°C for 4 hours to obtain a composite sponge.
[0103] Embodiment 15: According to the method of Example 9, a bio-based latex based on eucommia rubber (eucommia rubber / cis-polyisoprene rubber composite latex) prepared by an asynchronous method, wherein the ratio of the two rubbers used in combination is 10:90, is then used to prepare a composite sponge: 170 parts of eucommia rubber / cis-polyisoprene rubber composite latex, 2.5 parts of sulfur, 1.0 part of accelerator ZDC (zinc diethyldithiocarbamate), 1.0 part of accelerator PX (zinc N-ethyl-N-phenyldithiocarbamate), 2.0 parts of antioxidant D (N-phenyl-2-naphthylamine), 0.0 parts of peregrin, and 1.0 parts of chlorinated paraben. 0.12 parts, 1.2 parts of potassium oleate, 1.6 parts of hexadecyltrimethylammonium bromide, stirring and ripening at 30°C for 12 hours to obtain a composite glue; the composite glue is stirred at a speed of 1500 rpm, and air is filled in at the same time to quickly foam to a specified volume, then slowly foamed at 100 rpm, and then 8 parts of activator zinc oxide diluted with soft water are added, and the foam is treated at a medium speed of 200 rpm for 2 minutes, 2 parts of sodium fluorsilicate and 0.15 parts of potassium hydroxide mixed with aqueous liquid are added together, and the foam is treated at a medium speed of 400 rpm for another 2 minutes, and the foam is evenly injected into a mold sprayed with release agent talcum powder, and solidified at 90°C for about 30 minutes. After vulcanization at 110°C to 120°C for 40 minutes, it is washed, dehydrated, and dried at 60°C to 80°C for 4 hours to obtain a composite sponge.
[0104] Comparative Example 3: The difference from Example 13 is that when preparing the composite sponge, the eucommia rubber-containing bio-based latex prepared in Comparative Example 1 is used instead of the eucommia rubber-based bio-based latex.
[0105] Comparative Example 4: The difference from Example 15 is that, when preparing the composite sponge, the bio-based latex containing cis-polyisoprene rubber prepared in Comparative Example 2 is used instead of the bio-based latex based on eucommia rubber.
[0106] The composite sponges prepared in Examples 13 to 15 and Comparative Examples 3 to 4 were subjected to performance tests. The test parameters and test methods are shown in Table 2.
[0107] It can be seen from Table 2 that, compared with the composite sponge prepared in Comparative Example 3, the composite sponge prepared in Example 13 has a Shore C hardness of the same level, and its rebound rate and tensile strength are significantly better than those of the composite sponge prepared in Comparative Example 3; compared with the composite sponge prepared in Comparative Example 4, the Shore C hardness, rebound rate and tensile strength of the composite sponge prepared in Example 15 are significantly better than those of the composite sponge prepared in Comparative Example 4.
[0108] It can be seen that the bio-based latex based on eucommia rubber prepared in the present invention has the properties of both eucommia rubber and blended rubber, and is superior in some performance parameters. For example, the Shore C hardness, rebound rate and tensile strength of the composite sponge prepared in Example 15 are better than those of the composite sponge prepared in Comparative Example 4. This shows that the preparation method makes the eucommia rubber and the blended rubber highly integrated, has good shape memory (rebound rate), and has better tensile properties (tensile strength).
[0109] Table 1 Experimental data of atmospheric distillation to remove solvent
[0110] Table 2 Performance test results of composite sponges obtained in some examples .
Claims
1. A method for preparing a bio-based latex based on Eucommia rubber, characterized in that: Proceed as follows: The eucommia rubber and the blended rubber are mixed by a synchronous mixing method to obtain a composite rubber liquid, or the eucommia rubber and the blended rubber are mixed by an asynchronous mixing method to obtain an eucommia rubber liquid and a blended rubber liquid respectively; The blended rubber is one of cis-polyisoprene rubber, butadiene rubber, styrene-butadiene rubber and butyl rubber; The composite rubber liquid is emulsified synchronously to obtain a composite crude emulsion; or, the eucommia rubber liquid and the blended rubber liquid are emulsified asynchronously to obtain a composite crude emulsion; After the composite crude latex is post-treated, a bio-based latex based on eucommia rubber is obtained; The synchronous blending method comprises: adding eucommia rubber and blended rubber into an organic solvent in proportion, heating and stirring, dissolving by reflux, and filtering to prepare a composite rubber glue solution; Asynchronous blending method: adding eucommia rubber to an organic solvent, heating and stirring, dissolving by reflux, filtering, and obtaining eucommia rubber glue liquid; adding the blended rubber to an organic solvent, and obtaining the blended rubber glue liquid under heating and stirring conditions.
2. The method for preparing the bio-based latex based on eucommia rubber according to claim 1, characterized in that: The synchronous blending method is specifically as follows: adding eucommia rubber and blended rubber to an organic solvent in proportion, stirring at 50° C. to 60° C., refluxing and dissolving for 12 to 16 hours, and then removing insoluble matter in the eucommia rubber solid glue by suction filtration to prepare a composite rubber glue liquid, wherein the eucommia rubber accounts for 40% to 90% of the total mass of the rubber, the blended rubber accounts for 10% to 60% of the total mass of the rubber, and the total mass of the rubber accounts for 8% to 13% of the total mass of the composite rubber glue liquid; The asynchronous blending method is specifically as follows: adding eucommia rubber to an organic solvent, stirring at 50° C. to 60° C., refluxing to dissolve for 12 to 16 hours, and then removing insoluble matter in the eucommia rubber solid glue by suction filtration to prepare eucommia rubber glue liquid; adding the blended rubber to the solvent, stirring at 50° C. to 60° C. for 10 to 12 hours to obtain the blended rubber glue liquid; the eucommia rubber accounts for 40% to 90% of the total mass of the rubber, the blended rubber accounts for 10% to 60% of the total mass of the rubber, and the total mass of the rubber accounts for 8% to 13% of the total mass of the eucommia rubber glue liquid and the blended rubber glue liquid.
3. The method for preparing the bio-based latex based on Eucommia rubber according to claim 2, characterized in that: Organic solvents are selected from C4 to C 10 The straight-chain alkane or cycloalkane is selected from natural eucommia rubber, trans-1,4-polyisoprene rubber, gutta-percha and balata gum; the number average molecular weight of eucommia rubber is 12,000 to 900,000; the cis-polyisoprene rubber is selected from natural hevea and cis-1,4-polyisoprene rubber; the butadiene rubber is selected from cis-1,4-polybutadiene rubber, trans-1,4-polybutadiene rubber, high cis-butadiene rubber, vinyl polybutadiene rubber and high cis-butadiene rubber; the styrene-butadiene rubber is selected from lithium styrene-butadiene rubber; the butyl rubber is selected from ordinary butyl rubber and brominated butyl rubber.
4. The method for preparing the bio-based latex based on eucommia rubber according to claim 3, characterized in that: The organic solvent is one or more of n-hexane, cyclohexane, n-pentane and cyclopentane; the number average molecular weight of eucommia rubber is 300,000 to 600,000.
5. The method for preparing the bio-based latex based on Eucommia rubber according to any one of claims 1 to 4, characterized in that: Synchronous emulsification is specifically: 1) Prepare emulsifier aqueous solution Add the emulsifier to water, heat and stir at 55°C to 60°C for 4h to 8h, adjust the pH value to 10 to 12, and obtain a uniform and stable emulsifier aqueous solution, wherein the mass of the emulsifier accounts for 2% to 5% of the total mass of the emulsifier aqueous solution; 2) Synchronous emulsification The composite rubber glue and the emulsifier aqueous solution are emulsified in batches at a mass ratio of 1:
1. The specific process is: at room temperature, first add a portion of the emulsifier aqueous solution to the composite rubber glue, and stir at a speed of 400r / min to 500r / min for 30min to 60min to form an oil-in-water pre-emulsified glue; then, add the remaining emulsifier aqueous solution to the oil-in-water pre-emulsified glue, and emulsify at a shear speed of 3000rpm to 4000rpm for 3min to 5min; subsequently, increase the shear speed to 4000rpm to 5000rpm, and shear homogenize for 5min to 10min to form a stable water-in-oil crude emulsion, i.e., a composite crude emulsion.
6. The method for preparing the bio-based latex based on Eucommia rubber according to any one of claims 1 to 4, characterized in that: Asynchronous emulsification is specifically as follows: 1) Prepare emulsifier aqueous solution Add the emulsifier to water, heat and stir at 55°C to 60°C for 4h to 8h, adjust the pH value to 10 to 12, and obtain a uniform and stable emulsifier aqueous solution, wherein the mass of the emulsifier accounts for 2% to 5% of the total mass of the emulsifier aqueous solution; 2) Asynchronous emulsification The specific process is as follows: at room temperature, a portion of the emulsifier aqueous solution is added to the eucommia rubber liquid for pre-emulsification, and stirred at a speed of 450r / min to 500r / min for 45min to 60min to form an oil-in-water pre-emulsified liquid; then a portion of the emulsifier aqueous solution is added to the pre-emulsified liquid, and shear emulsification is performed at a shear speed of 3500rpm to 4000rpm for 4min to 10min; the shear speed is continuously increased for shear homogenization, and homogenization is performed at a shear speed of 4500rpm to 5000rpm for 7min to 10min to obtain a crude eucommia rubber emulsion; At room temperature, a portion of the emulsifier aqueous solution is added to the blended rubber glue for pre-emulsification, and stirred at a speed of 450 r / min to 500 r / min for 45 min to 60 min to form an oil-in-water pre-emulsified glue; then a portion of the emulsifier aqueous solution is added to the pre-emulsified glue, and shear emulsification is performed at a shear speed of 3500 rpm to 4000 rpm for 4 min to 10 min; the shear speed is continued to be increased for shear homogenization, and the shear speed is homogenized at a shear speed of 4500 rpm to 5000 rpm for 7 min to 10 min to obtain a blended rubber crude emulsion; The obtained eucommia rubber crude emulsion and the blended rubber crude emulsion are mixed, and stirred at 45° C. to 50° C. for 2 h to 4 h to form a stable oil-in-water crude emulsion, namely, a composite crude emulsion.
7. The method for preparing the bio-based latex based on Eucommia rubber according to any one of claims 1 to 4, characterized in that: The post-treatment of the composite crude emulsion includes: removing the organic solvent by atmospheric distillation, removing the residual organic solvent by reduced pressure distillation, and preparing the bio-based latex based on eucommia rubber by high-speed centrifugal concentration; specifically: The composite crude emulsion is subjected to atmospheric distillation at a distillation temperature of 45° C. to 82° C. and a distillation residence time of 6 h to 9 h to remove 80% to 90% of the total amount of the organic solvent; then, a reduced pressure distillation is performed at 60° C. to 80° C. and 60 KPa for 1 h to 1.5 h to remove the residual organic solvent to obtain a dilute emulsion; The dilute emulsion is centrifuged and concentrated at a rotation speed of 6000 rpm to 10000 rpm for 5 to 20 minutes to obtain a bio-based latex based on eucommia rubber.
8. The method for preparing the bio-based latex based on Eucommia rubber according to claim 6, characterized in that: The emulsifier includes one or more of anionic surfactants and nonionic surfactants, wherein the anionic surfactant includes one or more of benzene sulfonate, rosin acid soap, naphthalene sulfonate, fatty acid salt, and oleic acid soap, and the nonionic surfactant includes one or more of fatty alcohol polyoxyethylene ether, fatty amine polyoxyethylene ether, alkylphenol polyoxyethylene ether, and sorbitan oleate.
9. A bio-based latex based on eucommia rubber obtained according to the preparation method according to any one of claims 1 to 8.
Citation Information
Patent Citations
Preparation method of synthetic Eucommea rubber latex
CN107602877A
Biology-based new rubber material EU (Eucommia Ulmoides)-hevea rubber
CN108707254A
Gutta-percha / natural latex sponge product and preparation method thereof
CN110437510A
Bio-based damping vibration attenuation rubber composite material with long service life and preparation method thereof
CN116444924A