Method for manufacturing surface treated sheet

By applying a liquid to the cellulose triacetate film and volatilizing the solvent at a specific temperature, the problems of adhesion durability and poor appearance of the surface-treated sheet were solved, and the use of a cellulose triacetate film containing an aromatic ring polyester component was solved Methods for manufacturing high quality surface treated sheets.

CN118772469APending Publication Date: 2024-10-15NITTO DENKO CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410393013.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-04
Filing Date
2024-04-02
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In the prior art, when cellulose triacetate films containing specific polyester components are used to manufacture surface-treated sheets, it is easy to cause poor adhesion durability and appearance of the surface part, and it is difficult to fully form a mixed layer, affecting the reliability of the product.

Method used

Apply a coating liquid containing at least a solvent and a tackifier to the cellulose triacetate film, and volatilize the solvent at a maximum temperature of 70°C or more and 100°C or less, using toluene and ethyl acetate as solvents, and The coating liquid contains curable components and polymerization initiators to improve the adhesion durability and appearance quality of the surface-treated sheet.

Benefits of technology

Through this method, even if a cellulose triacetate film containing an aromatic ring polyester component is used, a surface-treated sheet with excellent adhesion durability and good appearance on the surface can be produced, thereby improving product reliability and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772469A_ABST
    Figure CN118772469A_ABST
Patent Text Reader

Abstract

Provided is a method for producing a surface-treated sheet, the method comprising a step for applying a coating liquid containing at least a solvent and a tackifier to a cellulose triacetate film containing a polyester component having an aromatic ring at a molecular terminal, and a step for volatilizing the solvent from the coating liquid. The solvent contains at least toluene and ethyl acetate, the content of the ethyl acetate in the solvent is 7% by mass or more and 11% by mass or less, and in the step of volatilizing the solvent, the solvent is volatilized at a maximum temperature of 70 DEG C or more and 100 DEG C or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a surface-treated sheet that can be used as a member of an image display device, for example. Background Art

[0002] Conventionally, there is known a method for producing a surface treated sheet by subjecting one surface of a base film to a surface treatment. The surface treated sheet obtained by such a production method can be used as a member of an image display device, for example.

[0003] As a method for producing such a surface-treated sheet, there is known a method comprising, for example, a step of applying a coating liquid containing a plurality of specific components and a solvent onto one side of a substrate film such as a triacetylcellulose film, and a step of volatilizing the solvent after the step.

[0004] It should be noted that, in order to increase the yield rate during production, to reduce production costs, or to reduce the burden on the global environment during production, the triacetate cellulose film as the base film has been improved by changing the process in its production process. With the improvement of the process in production, there are products containing by-components as triacetate cellulose film.

[0005] Specifically, as a method for manufacturing a surface treatment sheet, the following method is known: a coating liquid containing low-refractive particles, an adhesive matrix, a functional compound and a specific solvent is applied to a triacetate cellulose film as a base film, the solvent in the coating liquid is volatilized, and then the coating film after the solvent volatilization is cured, thereby manufacturing an anti-reflection film as a surface treatment sheet (for example, Patent Document 1).

[0006] In the manufacturing method described in Patent Document 1, for example, when the solvent is volatilized, it is first set to be above 20°C and below 30°C, and then the solvent is further volatilized at above 50°C and below 150°C. The anti-reflection film obtained by the manufacturing method described in Patent Document 1 can have good hardness. In addition, according to the manufacturing method described in Patent Document 1, the solvent of the coating liquid dissolves or swells a part of the substrate film, so the above-mentioned adhesive matrix and solvent penetrate into the substrate film side to form a mixed layer. Therefore, by one coating, an anti-reflection film having a multilayer structure having a low-refractive layer containing low-refractive particles and a hard coating layer formed by curing the above-mentioned mixed layer can be manufactured.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2013-205644 Summary of the invention

[0010] Problems to be solved by the invention

[0011] On the other hand, in order to suppress the sedimentation of particulate components contained in the coating liquid as much as possible, a surface treatment film may be produced using a coating liquid that has been appropriately thickened by adding a thickening agent.

[0012] However, if the coating liquid containing a thickener and a solvent is simply applied to the cellulose triacetate film, a surface treatment film having a poor appearance on the surface portion may be produced due to the coagulation of the thickener. In addition, a part of the cellulose triacetate film is not easily dissolved by the solvent of the coating liquid, and a mixed layer cannot be fully formed, resulting in a tendency for the adhesion durability of the surface portion to deteriorate and peeling to occur on the surface portion. The reliability of the surface treatment film produced by such a method as a product may be reduced.

[0013] Furthermore, as the aforementioned secondary components that may be contained in the cellulose triacetate film, for example, a specific polyester component is included. This specific polyester component may also cause a problem of deterioration in the adhesion durability of the surface portion of the cellulose triacetate film.

[0014] In order to prevent the above-mentioned problems, it is conceivable to design the manufacturing method so that the adhesion durability and the appearance of the surface portion become good.

[0015] However, it can be said that a method for producing a surface treated sheet which uses a cellulose triacetate film containing the above-mentioned specific polyester component as a substrate and can produce a surface treated sheet having both excellent adhesion durability and appearance of the surface portion has not been fully studied.

[0016] Therefore, an object of the present invention is to provide a method for producing a surface treated sheet which can produce a surface treated sheet having excellent adhesion durability and appearance at the surface portion even when a cellulose triacetate film containing a specific polyester component is used as a substrate.

[0017] Solutions to the problem

[0018] In order to solve the above problems, the method for producing a surface-treated sheet of the present invention comprises:

[0019] a step of applying a coating liquid containing at least a solvent and a thickener to a cellulose triacetate film; and

[0020] a step of volatilizing the solvent from the coating liquid,

[0021] The cellulose triacetate film contains a polyester component having an aromatic ring at a molecular terminal.

[0022] The solvent contains at least toluene and ethyl acetate, and the content of the ethyl acetate in the solvent is 7% by mass or more and 11% by mass or less,

[0023] In the step of volatilizing the solvent, the solvent is volatilized under the condition that the maximum temperature is 70° C. or higher and 100° C. or lower. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a schematic diagram showing an example of a method for producing a surface-treated sheet.

[0025] Figure 2A It is a cross-sectional view schematically showing a state before the coating step in the production method of the present embodiment is performed.

[0026] Figure 2B It is a cross-sectional view schematically showing a state immediately after the coating step in the manufacturing method of the present embodiment is performed.

[0027] Figure 2C It is a cross-sectional view schematically showing a state after the volatilization step in the production method of this embodiment is performed.

[0028] Explanation of symbols

[0029] 10: Surface treatment film,

[0030] 11: base layer, 12: mixed layer, 13: surface layer,

[0031] X: cellulose triacetate film, Y: coating liquid,

[0032] 100: Manufacturing equipment,

[0033] 1: Pre-treatment section, 2: Coating section, 3: Heating section, 4: Curing treatment section. DETAILED DESCRIPTION

[0034] Hereinafter, one embodiment of the method for producing a surface-treated sheet of the present invention will be described with reference to the accompanying drawings. It should be noted that each of the drawings is a schematic diagram and the aspect ratio is not necessarily the same as that of the actual object.

[0035] The method for manufacturing the surface treated sheet 10 of the present embodiment comprises:

[0036] A step of applying a coating liquid Y containing at least a solvent and a thickener to a triacetyl cellulose film X (hereinafter, sometimes referred to as a TAC film) (hereinafter referred to as a coating step); and

[0037] A step of volatilizing the solvent from the coating liquid Y (hereinafter referred to as a volatilization step).

[0038] The cellulose triacetate film X contains a polyester component having an aromatic ring at a molecular terminal. The solvent contains at least toluene and ethyl acetate, and the content of the ethyl acetate in the solvent is 7% by mass or more and 11% by mass or less.

[0039] In the volatilization step, the solvent is volatilized under the condition that the maximum temperature is 70° C. or higher and 100° C. or lower.

[0040] According to such a method for producing a surface-treated sheet, even when a cellulose triacetate film containing a polyester component having an aromatic ring at a molecular terminal is used as a substrate, a surface-treated sheet having excellent adhesion durability and appearance of the surface portion can be produced.

[0041] The coating liquid Y preferably further contains a curable component and a polymerization initiator. The method for producing the surface treatment sheet 10 of this embodiment includes the coating step, the volatilization step, and a step of curing the curable component (hereinafter referred to as a curing step).

[0042] For example, Figure 1 As shown, the manufacturing method of the surface treatment sheet 10 of the present embodiment can be implemented using a manufacturing device 100, and the manufacturing device 100 comprises: a coating section 2 for implementing the above-mentioned coating process, a heating section 3 with a heating mechanism for implementing the above-mentioned volatilization process, and a curing treatment section 4 for implementing the above-mentioned curing treatment process.

[0043] If necessary, the method for manufacturing the surface treated sheet 10 of the present embodiment may further include a pre-treatment unit 1 for pre-annealing the TAC film X. In the pre-treatment unit 1, for example, in order to sufficiently reduce wrinkles of the TAC film X or to sufficiently reduce foreign matter attached to the surface of the TAC film X, a pre-annealing process may be performed in the pre-treatment unit 1.

[0044] In the method for producing the surface treated sheet 10 of the present embodiment, the long strip-shaped TAC film X is continuously supplied to the coating section 2 and the surface treated sheet 10 obtained by passing through the heating section 3 and the curing treatment section 4 is continuously produced.

[0045] The above-mentioned cellulose triacetate film X (TAC film) contains, as a main component, cellulose triacetate in which three hydroxyl groups in the monosaccharide unit constituting cellulose are acetylated, and contains, as a trace component, a polyester component having an aromatic ring at a molecular terminal.

[0046] The content of the polyester component in the TAC film X is usually 1% by mass or more and 10% by mass or less.

[0047] The polyester component having an aromatic ring at a molecular terminal is mixed into the TAC film during the process of producing the TAC film X.

[0048] The polyester component is, for example, an esterification reaction product of terephthalic acid, adipic acid, and propylene glycol.

[0049] A commercially available product can be used as the TAC film X. Commercially available TAC film products can be obtained from, for example, Konica Minolta, Inc., etc.

[0050] The coating liquid Y used in the manufacturing method of this embodiment contains at least toluene and ethyl acetate as solvents, and further contains a thickener, a curing component, and a polymerization initiator. If necessary, the coating liquid Y may further contain a particulate additive or a leveling agent.

[0051] In the coating liquid Y, the content of ethyl acetate in the solvent is preferably 8 mass % or more, more preferably 9 mass % or more, and even more preferably more than 9 mass %. The above content is a mass ratio in the total amount of the solvent.

[0052] In the coating liquid Y, the mass ratio of toluene to ethyl acetate is preferably 8 or more. In addition, the mass ratio is preferably 13 or less, and more preferably 11 or less.

[0053] The coating liquid Y may contain a solvent other than toluene and ethyl acetate. Examples of such a solvent include cyclopentanone and methoxypropanol.

[0054] However, in the coating liquid Y, from the perspective of making the curable components (such as resins, etc.) more easily soluble or enabling the thickener to be more fully dispersed, the proportion of toluene and ethyl acetate in the total amount of the solvent is preferably 95% by mass or more, more preferably 98% by mass or more, and even more preferably 100% by mass.

[0055] The coating liquid Y may contain, for example, 10% by mass or more and 40% by mass or less of a nonvolatile component. In other words, the coating liquid Y may contain a solvent in an amount of 10% by mass or more and 40% by mass or less of a nonvolatile component.

[0056] As the thickener of the coating liquid Y used in the present embodiment, for example, there can be mentioned: a particulate clay mineral, etc. As such a clay mineral, for example, there can be mentioned: smectite, talc, bentonite, montmorillonite, or kaolinite, etc. The clay mineral is preferably an organic modified clay mineral (organoclay).

[0057] As the particulate clay mineral, commercially available products may be used, such as the "Lucentite series" manufactured by Co-op Chemical Co., Ltd., the "S-BEN series" manufactured by Hojun Co., Ltd., and the "Sumecton series" manufactured by Kunimine Industries Co., Ltd.

[0058] The coating liquid Y may contain 0.3% or more, or 0.5% or more of a thickener (non-volatile component). In addition, the coating liquid Y may contain 3.0% or less, or 1.0% or less of a thickener (non-volatile component).

[0059] In the above-mentioned coating liquid Y, the proportion of the tackifier in the non-volatile components other than the solvent can be 0.5 mass % or more, or 1.0 mass % or more, or 1.5 mass % or more. In addition, the proportion of the tackifier in the non-volatile components other than the solvent can be 5.0 mass % or less, or 3.0 mass % or less. It should be noted that the above-mentioned non-volatile components are components other than the solvent that will constitute a part of the surface treatment sheet.

[0060] Examples of the curable component of the coating liquid Y include (meth)acrylate monomers and the like. In addition, the term "(meth)acrylate" includes both "acrylate" and "methacrylate".

[0061] As a (meth)acrylate monomer, a polyfunctional (meth)acrylate monomer, an oligomer derived from a polyfunctional (meth)acrylate monomer, a prepolymer derived from a polyfunctional (meth)acrylate monomer, etc. are mentioned, for example.

[0062] Examples of the polyfunctional (meth)acrylate monomer include tricyclodecane dimethanol diacrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolpropane triacrylate, pentaerythritol tetra(meth)acrylate, dimethylolpropane tetraacrylate, dipentaerythritol hexa(meth)acrylate, 1,6-hexanediol (meth)acrylate, 1,9-nonanediol diacrylate, 1,10-decanediol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, dipropylene glycol diacrylate, isocyanuric acid tri(meth)acrylate, ethoxylated glycerol triacrylate, and ethoxylated pentaerythritol tetraacrylate.

[0063] The multifunctional (meth)acrylate monomer may contain urethane (meth)acrylate or an oligomer of urethane (meth)acrylate.

[0064] Urethane (meth)acrylate is, for example, a urethanization reaction product of hydroxy (meth)acrylate having an -OH group, diisocyanate, and polyol.

[0065] Examples of the polyol include ethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, diethylene glycol, dipropylene glycol, neopentyl glycol, 1,3-butylene glycol, 1,4-butylene glycol, 1,6-hexanediol, 1,9-nonanediol, 1,10-decanediol, 2,2,4-trimethyl-1,3-pentanediol, 3-methyl-1,5-pentanediol, hydroxypivalic acid neopentyl glycol ester, tricyclodecanedimethanol, 1,4-cyclohexanediol, spirodiol, hydrogenated bisphenol A, ethylene oxide-added bisphenol A, propylene oxide-added bisphenol A, trimethylolethane, trimethylolpropane, glycerol, 3-methylpentane-1,3,5-triol, pentaerythritol, dipentaerythritol, tripentaerythritol, and glucose.

[0066] The (meth)acrylate monomers mentioned above may be used alone or in combination of two or more. As the curable components such as the (meth)acrylate monomers mentioned above, commercially available products may be used.

[0067] In order to sufficiently cure the curable component, the coating liquid Y may contain a photopolymerization initiator or a thermal polymerization initiator. As the photopolymerization initiator or the thermal polymerization initiator, a commercially available product can be used.

[0068] In the above-mentioned coating liquid Y, the proportion of the curable component in the non-volatile components other than the solvent can be 70.0 mass % or more and 90.0 mass % or less. In addition, in the above-mentioned coating liquid Y, the proportion of the polymerization initiator in the non-volatile components other than the solvent can be 1.0 mass % or more and 10.0 mass % or less.

[0069] Examples of the particulate additives of the coating liquid Y include polymer particles and inorganic particles.

[0070] Examples of polymer particles include polymethyl methacrylate particles (PMMA particles), silicone polymer particles, polystyrene particles, polycarbonate particles, acrylic styrene particles, benzoguanamine particles, melamine resin particles, polyolefin particles, polyester particles, polyamide particles, polyimide particles, polyvinyl fluoride particles, etc. The polymer in the particles may be cross-linked.

[0071] Examples of the inorganic particles include silicon oxide particles, titanium oxide particles, aluminum oxide particles, zinc oxide particles, tin oxide particles, calcium carbonate particles, barium sulfate particles, talc particles, kaolin particles, and calcium sulfate particles.

[0072] The above particles may be used alone or in combination of two or more. As the above particles, commercially available products may be used.

[0073] The average particle size of the particulate additive is, for example, 1 μm or more and 10 μm or less. The average particle size can be obtained by measuring the diameters of 50,000 particulate additives (e.g., polystyrene particles) using a flow-type image analysis device and arithmetically averaging the measured values. It should be noted that when the particles in the image during the measurement are not truly circular but elliptical, the major diameter of each particle is measured.

[0074] The coating liquid Y may contain 1.0% by mass or more of a particulate additive (solid), or 2.0% or more. In addition, the coating liquid Y may contain 10.0% by mass or less of a thickener (non-volatile component), or 5.0% or less.

[0075] In the above-mentioned coating liquid Y, the proportion of the particulate additive in the non-volatile components other than the solvent may be 5.0 mass % or more, 20.0 mass % or less, or 15.0 mass % or less.

[0076] The coating liquid Y preferably contains 10% by mass or more and 20% by mass or less of polystyrene particles having an average particle diameter of 1 μm or more and 5 μm or less. Thereby, the produced surface-treated sheet can have better anti-glare properties.

[0077] In the above-described coating step, the coating liquid Y is coated on one surface of the TAC film X by the coating unit 2 .

[0078] In the coating step, a general coating method can be used, such as die coating, wire bar coating, roll coating, gravure coating, rod coating, slot coating, curtain coating, spray coating, or comma coating.

[0079] The period from the completion of coating in the coating step to the start of heating in the volatilization step is preferably 10 seconds to 30 seconds.

[0080] In the volatilization step, the cellulose triacetate film X coated with the coating liquid Y is subjected to a heat treatment at a predetermined temperature for a predetermined time. The lowest temperature in the heat treatment is, for example, 45° C., and the solvent in the coating liquid Y is volatilized by heating the coated coating liquid Y at a temperature condition where the highest temperature is 70° C. or higher and 100° C. or lower.

[0081] The maximum temperature during the heat treatment in the volatilization step can be set to 75°C or above, 80°C or above, 85°C or above, or 90°C or above. By making the heating temperature higher, the time required for the above-mentioned polyester component to be eluted from the TAC film is shortened. The adhesion durability of the surface portion of the manufactured surface-treated sheet can be further improved corresponding to the portion where the amount of elution of the above-mentioned polyester component is reduced. It should be noted that the maximum temperature during the heat treatment can be set to 95°C or below.

[0082] In addition, the duration of the maximum temperature set as described above may be 5 seconds or more, or 10 seconds or more. The duration of the maximum temperature set as described above may be 30 seconds or less, or 20 seconds or less.

[0083] The heat treatment time in the volatilization step (the total time for which the heat treatment is continued) is preferably 60 seconds or longer, and more preferably 80 seconds or longer. By making the heat treatment time longer, the solvent can be volatilized from the coating liquid Y more fully.

[0084] The heat treatment time is preferably 120 seconds or less, and more preferably 100 seconds or less. By shortening the heat treatment time, the volatilization step can be completed in a shorter time.

[0085] In addition, the minimum temperature set in the heat treatment is preferably 45°C, more preferably 50°C.

[0086] The heat treatment time in the volatilization step can be adjusted by, for example, increasing or decreasing the speed at which the TAC film X passes through the heating unit 3 .

[0087] In the volatilization step, it is preferred that the maximum temperature in the heat treatment be set as described above, and the heat treatment at the maximum temperature be continued for 10 seconds to 20 seconds.

[0088] In the manufacturing method of this embodiment, the curing process is performed in the above-mentioned curing treatment part 4. In the curing treatment part 4, the curing process is performed in order to cure the curable component remaining after the solvent volatilizes.

[0089] The curing treatment unit 4 includes, for example, a light irradiation device capable of irradiating light such as ultraviolet rays. When the coating liquid Y contains a curable component that can be cured by light irradiation, the curable component can be cured by light irradiation from the light irradiation device. In addition, when the coating liquid Y contains a curable component that can be cured by heat treatment, the curable component can be cured by heat treatment.

[0090] In the light irradiation in the curing treatment step, for example, the dried coating film after the solvent has volatilized is irradiated with active energy rays such as ultraviolet rays to cure the dried coating film.

[0091] As active energy rays, for example, ultraviolet rays, visible light, or infrared rays can be used. It should be noted that as active energy rays, α rays, β rays, γ rays, electron beams, neutron rays, or radiation such as X-rays can be used. From the perspective of high safety to the human body and high energy, it is preferred to irradiate light containing ultraviolet rays.

[0092] The surface-treated sheet 10 manufactured through the curing treatment step can be rolled up and stored, for example.

[0093] In the manufacturing method of this embodiment, in the coating step, on the TAC film X (refer to Figure 2A ) is coated with coating liquid Y (refer to Figure 2B ). In addition, in the volatilization step, the coating liquid Y applied on the TAC film X is heated to volatilize the solvent in the coating liquid Y. Figure 2C As shown, the manufactured surface treatment sheet 10 has, for example, a surface layer 13, a base layer 11 located closer to the inside than the surface layer 13, and a mixed layer 12 (also referred to as a compatibility layer) located between the surface layer 13 and the base layer 11 and composed of a part of the components constituting the surface layer 13 and a part of the components constituting the base layer 11. That is, the manufactured surface treatment sheet 10 may also be a multilayer sheet having a structure in which multiple layers are stacked on the surface portion.

[0094] The coating liquid Y used in the coating step contains at least ethyl acetate and toluene as solvents, and the solvent contains ethyl acetate and toluene at predetermined content ratios, respectively.

[0095] Ethyl acetate easily dissolves TAC in the TAC film, so a part of TAC, which is the main component of the substrate layer 11, dissolves and transfers to the above-mentioned mixed layer 12, thereby being able to reliably form a mixed layer containing TAC. Therefore, by providing a mixed layer between the surface layer 13 and the substrate layer 11, the adhesion durability becomes good. However, if the content of ethyl acetate in the solvent is too high, it is difficult for the tackifier to be dispersed in the solvent of the coating liquid Y, so that the tackifier aggregates are easily generated in the surface layer 13 or the mixed layer 12, and the appearance of the surface portion of the surface treatment sheet 10 may become poor.

[0096] On the other hand, toluene can fully disperse the tackifier, so it is possible to suppress the aggregation of the tackifier. Therefore, the appearance of the surface treatment sheet 10 can be made good. However, when the content of toluene in the solvent is too much, TAC becomes difficult to dissolve in the solvent, so the formation of the mixed layer 12 containing TAC may become insufficient. Therefore, the adhesion durability between the surface layer 13 and the base layer 11 may become poor.

[0097] In addition, the heat treatment temperature (particularly the maximum temperature) in the volatilization step is within the given range as described above.

[0098] When the heating temperature for volatilizing the solvent is too high, after the coating liquid Y is applied on the TAC film, most of the solvent will volatilize before TAC is fully dissolved in the solvent (before TAC is fully dissolved in the mixed layer 12). Therefore, the adhesion durability between the surface layer 13 and the base layer 11 may become poor.

[0099] On the other hand, if the heat treatment temperature (particularly the maximum temperature) is too low when the solvent is volatilized, a long time is required for volatilization. Although the solvent can fully dissolve TAC, it takes a long time for the solvent to completely volatilize, so production efficiency may be deteriorated.

[0100] It should be noted that, when the TAC film contains a large amount of the above-mentioned polyester component, if the time until the solvent of the coating liquid Y evaporates becomes too long, such polyester component may be dissolved from the TAC film and segregated between the substrate layer 11 and the mixed layer 12. The segregated polyester component may cause the adhesion between the substrate layer 11 and the mixed layer 12 to deteriorate. Therefore, it may cause the adhesion durability between the surface layer 13 and the substrate layer 11 to deteriorate.

[0101] In the manufacturing method of this embodiment, the coating liquid Y contains ethyl acetate and toluene in a given content ratio in the organic solvent, and the organic solvent of the coating liquid Y is volatilized at a given heating temperature, so that the poor adhesion durability between the surface layer 13 and the base layer 11 and the aggregation of the tackifier can be suppressed. Therefore, the surface treatment sheet 10 with good adhesion durability and appearance of the surface portion can be manufactured.

[0102] The method for producing the surface-treated sheet of the present embodiment is as exemplified above, and the present invention is not limited to the method for producing the surface-treated sheet exemplified above.

[0103] That is, various modes that can be used in a general method for producing a surface-treated sheet can be adopted within a range that does not impair the effects of the present invention.

[0104] The solutions disclosed in this specification include the following aspects.

[0105] (1) A method for producing a surface-treated sheet, comprising:

[0106] a step of applying a coating liquid containing at least a solvent and a thickener to a cellulose triacetate film; and

[0107] a step of volatilizing the solvent from the coating liquid,

[0108] The cellulose triacetate film contains a polyester component having an aromatic ring at a molecular terminal.

[0109] The solvent contains at least toluene and ethyl acetate, and the content of the ethyl acetate in the solvent is 7% by mass or more and 11% by mass or less,

[0110] In the step of volatilizing the solvent, the solvent is volatilized under the condition that the maximum temperature is 70° C. or higher and 100° C. or lower.

[0111] (2) The method for producing a surface-treated sheet according to (1) above, wherein:

[0112] The content of the polyester component in the cellulose triacetate film is 10% by mass or less.

[0113] (3) The method for producing a surface-treated sheet according to (1) or (2), wherein:

[0114] The coating liquid contains the thickener (non-volatile component) in an amount of 0.3% by mass to 3.0% by mass.

[0115] (4) The method for producing a surface-treated sheet according to any one of (1) to (3), wherein:

[0116] The coating liquid contains 1.0 mass % or more and 10.0 mass % or less of polystyrene particles having an average particle diameter of 1 μm or more and 5 μm or less.

[0117] (5) The method for producing a surface-treated sheet according to any one of (1) to (4) above, wherein:

[0118] The coating liquid further contains a curable component, and contains a polyfunctional (meth)acrylate monomer as the curable component.

[0119] (6) The method for producing a surface-treated sheet according to any one of (1) to (5), wherein:

[0120] The thickener includes a particulate clay mineral.

[0121] (7) The method for producing a surface-treated sheet according to any one of (1) to (6), wherein:

[0122] In the step of volatilizing the solvent, the solvent is volatilized by continuing the temperature condition in which the maximum temperature is 70° C. or higher and 100° C. or lower for 10 seconds or longer and 20 seconds or shorter.

[0123] (8) The method for producing a surface-treated sheet according to (7) above, wherein:

[0124] In the step of volatilizing the solvent, the solvent is volatilized by maintaining the temperature condition of 45° C. or higher for 60 seconds or more and 120 seconds or less while maintaining the temperature condition of 70° C. or higher and 100° C. or lower for 10 seconds or more and 20 seconds or less.

[0125] Example

[0126] Next, the present invention will be described in more detail with reference to experimental examples, but the present invention is not limited to these experimental examples.

[0127] use Figure 1 The manufacturing apparatus shown above carried out the method for manufacturing a surface-treated sheet as described below.

[0128] <Raw materials for surface treatment sheets>

[0129] (cellulose triacetate film)

[0130] (Contains about 8% by mass of a polyester component having an aromatic ring at a molecular terminal)

[0131] Product name: "KC4UA" (manufactured by Konica Minolta, Inc.) Thickness: 40 μm

[0132] (Coating liquid)

[0133] Organic solvent: ethyl acetate (the concentration in the solvent shown in Table 1) and toluene (the balance in the solvent)

[0134] Thickener: Clay mineral (organized montmorillonite with montmorillonite as the main component)

[0135] Product name: "Sumecton SAN" (manufactured by Kunimine Industries, Ltd.)

[0136] The thickening stock solution prepared in advance (containing 4.6% by mass of clay mineral) was used.

[0137] Photopolymerization initiator: product name "OMNIRAD907" (manufactured by BASF)

[0138] · Additive in particle form: cross-linked polystyrene particles with an average particle size of 3.5 μm

[0139] Product name: SX-350H (manufactured by Soken Chemical Co., Ltd.)

[0140] Curing component: UV curable urethane acrylate resin solution

[0141] Product name: "LUXYDIR 17-806" (manufactured by DIC Corporation) (non-volatile content: 80% by mass)

[0142] Leveling agent: fluorinated surfactant

[0143] Product name: "Megafac F-556" (manufactured by DIC Corporation) (non-volatile content: 40% by mass)

[0144] <Preparation of coating solution (amount of each raw material)>

[0145] Thickening stock solution containing the above-mentioned thickening agent (containing 4.6% by mass of non-volatile components): 2.5 parts by mass

[0146] Cross-linked polystyrene particles: 14 parts by mass

[0147] Photopolymerization initiator: 5 parts by mass

[0148] The above raw materials were stirred and mixed for 15 minutes using a disperser, and then further stirred for 20 minutes using a homomixer (rotation speed: 2500 rpm) to prepare an intermediate mixed liquid.

[0149] Furthermore, the following raw materials were added to the intermediate mixed liquid, and the mixture was stirred and mixed for 15 minutes using a disperser, and then further stirred for 20 minutes using a homomixer (rotation speed: 2500 rpm) to prepare a coating liquid.

[0150] · Organic solvent: The amount of non-volatile components in the coating liquid is 32% by mass

[0151] Ultraviolet curing urethane acrylate resin solution (non-volatile content 80% by mass): 100 parts by mass

[0152] Leveling agent (non-volatile content 40% by mass): 0.5 parts by mass

[0153] <Production conditions of surface-treated sheets>

[0154] (Pre-treatment process)

[0155] Perform 15 seconds of pre-annealing in the pre-treatment section

[0156] (Coating process)

[0157] ·Coating unit: Equipped with die coating device

[0158] The coating liquid was applied to one side of the triacetylcellulose film so that the coating film thickness before curing treatment would be 6 μm.

[0159] (Volatilization process)

[0160] · Volatilization section: equipped with a heater capable of heating the heating object passing through the internal space at a given set temperature (the length of the section subjected to heating treatment by the heater: 30m)

[0161] The solvent contained in the coating liquid was volatilized by heating, thereby forming a dry coating film with a thickness of 6 μm.

[0162] In addition, the details of the heat treatment time are as follows.

[0163] Total time of heating treatment: 80 to 120 seconds (the set minimum temperature of heating treatment is 50°C), duration of maximum temperature: 15 seconds (the set maximum temperature of heating treatment is shown in Table 1)

[0164] (Curing process)

[0165] Curing treatment section: equipped with high pressure mercury lamp

[0166] The accumulated light intensity reaches 245mJ / cm 2 The dried coating film after the solvent was evaporated was irradiated with ultraviolet light of 365 nm wavelength.

[0167] The production conditions in each example and each comparative example are shown in Table 1. Unless otherwise specified, the production conditions in each example and each comparative example are the same.

[0168] [Table 1]

[0169]

[0170] <Evaluation of performance of manufactured surface treatment films>

[0171] (Adhesion durability of the surface portion (durable peeling suppression performance))

[0172] The test pieces of each surface-treated sheet produced as described above were irradiated with ultraviolet rays for a long period of time as described below, and then the adhesion of the surface portion was evaluated.

[0173] Evaluation of long-term lighting conditions and adhesion

[0174] The test sample was irradiated with light from the surface layer side using an ultraviolet long-life discoloration meter (manufactured by SUGA Test Instruments Co., Ltd., model: U48HB).

[0175] Temperature: 40℃

[0176] Humidity: 20%RH

[0177] Lamp: (wavelength) 300nm~700nm, (illuminance) 500W / m 2

[0178] Continuous lighting time: 144 hours, 192 hours

[0179] After ultraviolet irradiation was implemented as described above, the adhesion of the surface portion of the surface treated sheet was evaluated. In detail, the test piece after 144 hours from the start of ultraviolet irradiation and the test piece after 192 hours (reference experiment) were subjected to the following checkerboard peeling test. In the checkerboard test, 100 (10×10) 1mm square small segments (grids) were formed in a checkerboard shape on the surface layer of each test piece using a cutting knife. Next, after an adhesive tape (manufactured by Sekisui Chemical Co., Ltd., trade name "Cellotape (registered trademark) No. 252") was pasted on the surface layer, the adhesive tape was peeled off. Repeat this operation twice, and the number of small segments that were peeled off together with the adhesive tape was counted.

[0180] 0 (zero): (excellent) No peeling (flaking) of small sections of the surface was observed.

[0181] △: (Good) There is a phenomenon that only a small section has peeled off (partial peeling)

[0182] ×: (bad) one or more small sections peeled off completely (one or more small sections peeled off completely)

[0183] (Appearance: confirmed by naked eye observation)

[0184] In a dark room, the coating surface of the surface treatment film (150 mm × 100 mm rectangle) was irradiated with light from a three-wavelength fluorescent lamp to reflect the light, and the presence of aggregates on the coating surface was confirmed by naked eye observation. The absence of aggregates was judged as good (○), and the presence of aggregates was judged as bad (×).

[0185] As can be seen from Table 1, in the surface treatment sheet manufactured by the manufacturing method of the example, even if a cellulose triacetate film containing a polyester component having an aromatic ring at a molecular terminal is used as a substrate, both the adhesion durability and the appearance of the surface portion (surface layer) are good. On the other hand, in the surface treatment sheet manufactured by the manufacturing method of the comparative example, any of the adhesion durability and the appearance of the surface portion (surface layer) is poor.

[0186] Industrial Applicability

[0187] The method for producing a surface-treated sheet of the present invention can be suitably used, for example, in the production of components of image display devices, such as optical sheets, specifically, anti-reflection sheets, anti-glare sheets, anti-reflection protection sheets, or anti-fingerprint sheets.

Claims

1. A method for manufacturing a surface-treated sheet, the method comprising: a step of applying a coating liquid containing at least a solvent and a thickener to a cellulose triacetate film; and a step of volatilizing the solvent from the coating liquid, The cellulose triacetate film contains a polyester component having an aromatic ring at a molecular terminal. The solvent contains at least toluene and ethyl acetate, and the content of the ethyl acetate in the solvent is 7% by mass or more and 11% by mass or less. In the step of volatilizing the solvent, the solvent is volatilized under the condition of a maximum temperature of 70° C. or higher and 100° C. or lower.

2. The method for producing a surface-treated sheet according to claim 1, in, The content of the polyester component in the cellulose triacetate film is 10% by mass or less.

3. The method for producing a surface-treated sheet according to claim 1 or 2, in, The coating liquid contains 0.3 mass % or more and 3.0 mass % or less of the thickener.

4. The method for producing a surface-treated sheet according to claim 1 or 2, in, The coating liquid contains 1.0 mass % or more and 10.0 mass % or less of polystyrene particles having an average particle diameter of 1 μm or more and 5 μm or less.

Citation Information

Patent Citations

  • Curable composition for forming antireflection film, antireflection film and method for manufacturing the same, polarizing plate, and display device