Preparation method of polyolefin microporous membrane
By using organic salts as processing aids, the problems of high pressure, high die temperature and poor environmental protection in the preparation of polyolefin microporous membranes for lithium-ion batteries have been solved, and high-performance polyolefin microporous membranes have been obtained, improving battery performance. safety performance and cycle life.
Patent Information
- Application Number
- CN202410995898.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-09-01
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-15
AI Technical Summary
The existing PE microporous membrane preparation process for lithium-ion batteries has problems such as high pressure, high die temperature, poor environmental protection and poor performance, resulting in insufficient ionic conductivity, wettability and membrane surface defects of the polyolefin microporous membrane. Good, affecting the safety performance and cycle life of the battery.
Using organic salts as processing aids, the polyolefin resin and organic salts are mixed and heated to a molten state, cooled to form a cast sheet, stretched in one direction to extract the organic salts, and finally stretched and shaped to obtain a product with high ionic conductivity. Polyolefin microporous membrane with high efficiency, low electrostatic voltage and low membrane surface defects.
The pressure and temperature during the preparation process are reduced, and the environmental protection is improved. The obtained polyolefin microporous membrane has higher ionic conductivity, good wetting effect and lower electrostatic voltage, which reduces membrane surface defects and improves battery performance. safety performance and cycle life.
Smart Images

Figure CN118772479A_ABST
Abstract
Description
[0001] This application claims the priority right to a patent application filed on September 1, 2023, with application number 2023111278823 and invention name “A method for preparing a polyolefin microporous membrane”. Technical Field
[0002] The present application relates to the field of diaphragm technology, and in particular to a method for preparing a polyolefin microporous membrane. Background Art
[0003] Currently, lithium-ion batteries have been widely used in the power field, but the safety issues that come with it have attracted great attention from the society. As the core component of lithium battery safety, the diaphragm, PE microporous membrane plays a role in ensuring the mechanical isolation of the two poles and ensuring good permeability during the transmission of lithium ions.
[0004] Currently, PE microporous membranes used in lithium-ion batteries are often prepared using a wet asynchronous stretching process. The preparation process usually includes: heating a system containing polyolefin and a pore-forming solvent to a melt on an extruder, passing through a T-die, and cooling to form a thin sheet. Then heating and stretching along the production line direction (MD direction). Then stretching in the direction perpendicular to the production line (TD). Without heating, after removing the pore-forming agent at 0-20°C, stretching again in at least one direction to obtain a PE microporous membrane.
[0005] In the prior art process, a high pressure is usually required during the mixing process, and a high die temperature is usually required during the extrusion stage, which makes the processing difficult. In addition, the preparation process is less environmentally friendly, and the ionic conductivity, wettability, or number of membrane surface defects of the prepared polyolefin microporous membrane are poor. Summary of the invention
[0006] Based on the above-mentioned deficiencies, the present application provides a method for preparing a polyolefin microporous membrane, so as to partially or completely improve the preparation problems of the polyolefin microporous membrane in the related art.
[0007] This application is implemented as follows:
[0008] In a first aspect, an example of the present application provides a method for preparing a polyolefin microporous membrane, comprising the following steps performed in sequence:
[0009] (1) mixing and heating a polyolefin resin and a processing aid into a molten mixture;
[0010] (2) extruding the mixture from a die head and cooling it to form a cast sheet containing a processing aid;
[0011] (3) stretching the cast sheet in at least one direction to obtain a base film;
[0012] (4) extracting the processing aid in the basement membrane to obtain an extracted basement membrane;
[0013] (5) stretching and shaping the extracted base film in at least one direction to obtain a polyolefin microporous membrane; wherein the processing aid includes an organic salt.
[0014] In the prior art, white oil and the like are usually used as processing aids, which easily form white smoke during the smelting process and pollute the environment. In the above implementation process, when preparing a polyolefin microporous membrane, the organic salt and the polyolefin resin can be mixed and heated at a relatively low pressure to obtain a molten mixture. The use of organic salt as a processing aid can also reduce the probability of white smoke. When the cast sheet is subsequently extruded from the die head, the die head temperature can be reduced, thereby improving processability and environmental protection. Moreover, when the processing aid is extracted from the base membrane obtained by subsequent stretching, the extraction process is simple. After the extracted base membrane is stretched and shaped, the obtained polyolefin microporous membrane has a high ionic conductivity, a good wetting effect (i.e., a low water contact angle), a low electrostatic voltage, and a low number of membrane surface defects, thereby improving the quality of the porous membrane, and thereby improving the safety performance and cycle life of the battery prepared using the porous membrane.
[0015] In combination with the first aspect, in an optional embodiment of the present application, the organic salt is a liquid organic salt.
[0016] In combination with the first aspect, in an optional embodiment of the present application, the organic salt includes at least one of an imidazole salt compound and a piperidine salt compound.
[0017] In the above implementation process, not only can the die temperature and pressure be reduced, the probability of white smoke can be reduced, and environmental protection can be improved, but also the ionic conductivity of the polyolefin microporous membrane can be improved, the water contact angle and electrostatic voltage can be reduced, the crystal points, bright spots and transparent defects on the membrane surface of the polyolefin microporous membrane can be reduced, and the quality of the porous membrane can be improved, thereby improving the safety performance and cycle life of the battery prepared using the porous membrane.
[0018] In combination with the first aspect, in an optional embodiment of the present application, the imidazole salt compound includes at least one of an imidazole salt or a salt of an imidazole structure containing a substituent; the piperidine salt compound includes at least one of a piperidine salt or a salt of a piperidine structure containing a substituent.
[0019] In the above implementation process, the organic salt is selected from at least one of a salt compound including imidazole salts or an imidazole structure containing a substituent and a salt compound including piperidine salts or a piperidine structure containing a substituent, which can reduce the pressure and die temperature during mixed melting and extrusion and reduce the probability of white smoke. After subsequent extraction and stretching shaping, a polyolefin microporous membrane with good ionic conductivity, good wetting effect, lower electrostatic voltage and a lower number of membrane surface defects can be obtained.
[0020] In combination with the first aspect, in an optional embodiment of the present application, on the thermogravimetric curve of the organic salt, the thermal weight loss between 300-400° C. accounts for 10-25wt%.
[0021] In combination with the first aspect, in an optional embodiment of the present application, through inductively coupled plasma emission spectroscopy analysis, the organic salt includes at least one of Al element, Ca element, Na element, Si element, Ti element, K element, B element, Fe element, Mg element, Zn element, Au element, Cr element, Hg element, P element, Pt element, Sb element, Sn element, Cu element or Zr element.
[0022] In combination with the first aspect, in an optional implementation manner of the present application, quantitative analysis by energy spectrum method shows that the C element percentage of the organic salt is 60-70%, and the N element percentage is 30-40%.
[0023] In combination with the first aspect, in an optional embodiment of the present application, the content of S element in the organic salt is 1.0-1.2% as analyzed by X-ray fluorescence spectroscopy.
[0024] In combination with the first aspect, in an optional embodiment of the present application, the viscosity of the organic salt is 10-14 cp; and / or, the conductivity of the organic salt is 400-650 uS / cm; and / or, the density of the organic salt is 0.9-0.97 g / cm 3 .
[0025] In the above implementation process, a viscosity of 10-14 cp, a conductivity of 400-650 uS / cm and / or a density of 0.9-0.97 g / cm is used. 3 The organic salt can make the prepared porous membrane have better performance.
[0026] In combination with the first aspect, in an optional embodiment of the present application, the organic salt is selected from one or more of imidazole tetrafluoroborate, betaine salt, imidazole acetate, piperidine hydrochloride, imidazole dinitrile ammonium salt, imidazole ethyl sulfate salt, imidazole bisfluorosulfonyl imide salt and bistrifluorosulfonyl imide salt.
[0027] In the above implementation process, the use of organic salts of imidazole tetrafluoroborate, betaine salt, imidazole acetate, piperidine hydrochloride, imidazole dinitrile ammonium salt, imidazole ethyl sulfate salt, imidazole bisfluorosulfonyl imide salt and bistrifluorosulfonyl imide salt can reduce the melting pressure, die head temperature, the probability of white smoke and the environmental friendliness of the extractant in the preparation process, and obtain a polyolefin microporous membrane with good ionic conductivity, good wetting effect, lower electrostatic voltage and a lower number of membrane surface defects.
[0028] In combination with the first aspect, in an optional embodiment of the present application, in step (4), the extractant used for extraction is a non-halogenated hydrocarbon.
[0029] In combination with the first aspect, in an optional embodiment of the present application, the extractant is water.
[0030] In combination with the first aspect, in an optional embodiment of the present application, the water is deionized water.
[0031] In the above implementation process, a cast sheet is obtained by extruding a mixture containing an organic salt and a polyolefin resin. When the base film obtained after stretching the cast sheet is extracted, a non-halogenated hydrocarbon extractant such as deionized water can be used. This can reduce the adverse effects of the extraction process on the ionic conductivity or wettability of the polyolefin microporous membrane, improve the environmental friendliness of the extraction process, and reduce the number of membrane surface defects such as crystal points, transparency or bright spots on the polyolefin microporous membrane.
[0032] In combination with the first aspect, in an optional embodiment of the present application, no other auxiliary agent is added in step (1).
[0033] In combination with the first aspect, in an optional embodiment of the present application, no antioxidant is added in step (1).
[0034] In the above implementation process, since the mixture contains an organic salt processing aid, the stability of the mixed melt can be improved without adding any other additives such as antioxidants, and a polyolefin microporous membrane with good ionic conductivity, wetting effect and a low number of membrane surface defects can be obtained after subsequent extrusion, stretching, extraction and stretching shaping.
[0035] In combination with the first aspect, in an optional embodiment of the present application, the weight average molecular weight of the polyolefin resin is 4.0×10 5 -15.0×10 5 .
[0036] In combination with the first aspect, in an optional embodiment of the present application, the polyolefin resin is selected from one or more of polyethylene, polypropylene, polyisoprene or polybutylene.
[0037] In combination with the first aspect, in an optional embodiment of the present application, the stretching in step (3) is asynchronous biaxial stretching or synchronous biaxial stretching.
[0038] In the above implementation process, the cast sheet obtained by using the mixture of the processing aid containing organic salt and the polyolefin resin has good stretchability, and the sheet can be stretched by asynchronous biaxial stretching or synchronous biaxial stretching.
[0039] In combination with the first aspect, in an optional embodiment of the present application, the organic salt accounts for 40%-80% of the total mass of the mixture.
[0040] In the above-mentioned implementation process, the mixture contains 40%-80% organic salt, which can reduce the pressure, die temperature and the probability of white smoke in the subsequent mixing, melting and extrusion processes. After subsequent stretching, extraction and stretching molding, a polyolefin microporous membrane with good ionic conductivity, good wetting effect, lower electrostatic voltage and lower number of membrane surface defects can be obtained.
[0041] In combination with the first aspect, in an optional embodiment of the present application, the residual rate of organic salt in the polyolefin microporous membrane is less than 1%.
[0042] In the above implementation process, the residual rate of organic salt in the polyolefin microporous membrane prepared by the preparation method provided in the example of this application is less than 1%, the purity of the polyolefin microporous membrane is high, and the membrane surface performance is good.
[0043] In combination with the first aspect, in an optional embodiment of the present application, the die temperature in step (2) is 150-180° C.; and / or the pressure of the molten mixture in the pipeline in step (1) is 1.5-2.5 MPa.
[0044] In the above implementation process, when the polyolefin resin and the organic salt are mixed and heated to obtain a molten mixture, the pressure of the mixture can be reduced to 1.5-2.5 MPa, and during subsequent extrusion, the temperature of the die can be reduced to 150-180°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below.
[0046] Figure 1 Schematic diagram of the preparation process of the polyolefin microporous membrane provided as an example in this application. DETAILED DESCRIPTION
[0047] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0048] At present, the preparation process of polyolefin microporous membranes for lithium-ion batteries generally includes the following steps: heating a system containing polyolefin and a pore-forming solvent to melt on an extruder, passing through a T-die, and cooling to form a sheet. Then stretching in the MD (along the production line direction) or in the TD (vertical to the production line) direction. After removing the pore-forming agent, stretching in at least one direction again to obtain a polyolefin microporous membrane.
[0049] Typically, the pore-forming solvent is selected from white oil, liquid wax, castor oil, palm oil, rapeseed oil, soybean oil or linseed oil and derivatives thereof.
[0050] However, according to the preparation process of the prior art, a high pressure is usually required during the mixing process, and a large amount of white smoke is easily generated; a high die head temperature is usually required during the extrusion stage, and the processing is difficult. In addition, the ionic conductivity, wettability or number of membrane surface defects of the prepared polyolefin microporous membrane are poor.
[0051] The inventors analyzed and found that the pore-forming solvents in the prior art are usually selected from white oil, liquid wax, castor oil, palm oil, rapeseed oil, soybean oil or linseed oil and their derivatives. These pore-forming agents require a higher pressure when the mixture passes through the pipeline, and white smoke is easily generated during the preparation process. The preparation process is difficult and easily pollutes the environment.
[0052] Furthermore, when a mixture obtained by melting and mixing white oil, liquid wax, castor oil, palm oil, rapeseed oil, soybean oil or linseed oil and its derivatives with polyolefin resin is extruded, the temperature of the extrusion die is high and the processing is difficult.
[0053] In addition, when white oil, liquid wax, castor oil, palm oil, rapeseed oil, soybean oil or linseed oil and their derivatives are used as pore-forming agents, halogenated hydrocarbon extractants, such as dichloromethane, are usually required for subsequent extraction and removal of the pore-forming agents. Halogenated hydrocarbon extractants such as dichloromethane are hazardous chemicals and will also affect the performance of the prepared polyolefin microporous membrane.
[0054] Based on this, the present application provides an example of a method for preparing a polyolefin microporous membrane to improve the problems of high process difficulty and low environmental protection in the preparation process of the polyolefin microporous membrane, and to improve the performance of the polyolefin microporous membrane.
[0055] The preparation method of the polyolefin microporous membrane provided by the example of the present application is further described in detail below in conjunction with the accompanying drawings.
[0056] See also Figure 1 The method for preparing the polyolefin microporous membrane provided in the present application example includes:
[0057] S1. Mixing a polyolefin resin and a processing aid and heating them to form a molten mixture, wherein the processing aid comprises an organic salt.
[0058] The polyolefin resin and processing aid are mixed and heated into a molten mixture for subsequent extrusion, and a cast sheet is obtained after cooling.
[0059] The present application does not limit the specific type of polyolefin resin, and relevant personnel can make corresponding selections as needed.
[0060] In a possible embodiment, the polyolefin resin is selected from one or more of polyethylene, polypropylene, polyisoprene or polybutylene.
[0061] For example, the polyolefin resin may be selected from polyethylene; or the polyolefin resin may be selected from polypropylene; or the polyolefin resin may be selected from polyisopropylene; or the polyolefin resin may be selected from polybutene.
[0062] Furthermore, a weight average molecular weight of 4.0×10 5 -15.0×10 5 For example, the weight average molecular weight of the polyolefin resin may be 4.0×10 5 5.0×10 5 , 6.0×10 5 , 7.0×10 5 , 8.0×10 5 9.0×10 5 , 10.0×10 5 , 11.0×10 5 , 12.0×10 5 , 13.0×10 5 , 14.0×10 5 or 15.0×10 5 One of them or a range between any two.
[0063] The mixture contains a processing aid, and after the processing aid in the base film is subsequently extracted, a polyolefin microporous membrane with a microporous structure can be obtained.
[0064] The processing aid provided in the example of this application is an organic salt, which can reduce the pressure of the mixture when passing through the wire tube, reduce the temperature of the die head during extrusion, and reduce the probability of white smoke during the process, so as to reduce the process difficulty and improve environmental protection. When extracting the organic salt, it is also possible to use a non-halogenated hydrocarbon extractant to extract the organic salt, reduce the use of halogenated hydrocarbons and other extractants in the preparation process, improve environmental protection, and reduce the adverse effects of halogenated hydrocarbons and other extractants on the performance of polyolefin microporous membranes.
[0065] In addition, the processing aid provided in the present application is an organic salt, which can also improve the performance of the prepared porous membrane; specifically, it can improve the ionic conductivity of the porous membrane, which is beneficial to improve the cycle performance and rate performance of the battery prepared using the porous membrane; it can reduce the water contact angle of the porous membrane, that is, improve the electrolyte wettability of the porous membrane, which is beneficial to enable the ion conduction of the electrolyte between the positive and negative electrodes to proceed smoothly; it can reduce the electrostatic voltage of the porous membrane to facilitate the transmission of ions in the porous membrane; it can also reduce the number of defects such as crystal points, bright spots and transparency on the membrane surface of the porous membrane, so that the porous membrane has a higher quality, thereby improving the safety performance and cycle life of the battery prepared using the porous membrane.
[0066] In a possible embodiment, the organic salt is a liquid organic salt.
[0067] In a possible embodiment, the organic salt can be selected from at least one of imidazole salt compounds and piperidine salt compounds. The organic salt selected from the above substances can not only reduce the die temperature and pressure, reduce the probability of white smoke, and improve environmental protection, but also improve the ionic conductivity of the polyolefin microporous membrane, reduce the water contact angle and electrostatic voltage, reduce the crystal points, bright spots and transparent defects on the membrane surface of the polyolefin microporous membrane, improve the quality of the porous membrane, and thus improve the safety performance and cycle life of the battery prepared using the porous membrane.
[0068] Exemplarily, the organic salt may be selected from imidazolium salt compounds.
[0069] Furthermore, the organic salt may be selected from imidazole salts.
[0070] Alternatively, the organic salt may be selected from salts of imidazole structures containing substituents.
[0071] Exemplarily, the organic salt may be selected from piperidine salt compounds.
[0072] Furthermore, the organic salt may be selected from piperidine salts, for example, piperidine hydrochloride.
[0073] Alternatively, the organic salt may be selected from salts of a piperidine structure having a substituent.
[0074] For example, the organic salt may be selected from one or more of imidazole tetrafluoroborate, betaine salt, imidazole acetate, piperidine hydrochloride, imidazole dinitrile ammonium salt, imidazole ethyl sulfate salt, imidazole bisfluorosulfonyl imide salt and bistrifluorosulfonyl imide salt.
[0075] By using organic salts of imidazole tetrafluoroborate, betaine salt, imidazole acetate, piperidine hydrochloride, imidazole dinitrile ammonium salt, imidazole ethyl sulfate salt, imidazole bisfluorosulfonyl imide salt and bistrifluorosulfonyl imide salt, the melting pressure, die head temperature, probability of white smoke generation and environmental friendliness of the extractant in the preparation process can be reduced, and a polyolefin microporous membrane with good ionic conductivity, good wetting effect, lower electrostatic voltage and lower number of membrane surface defects can be obtained.
[0076] Illustratively, the imidazole tetrafluoroborate is 1-butyl-3-methylimidazolium tetrafluoroborate.
[0077] In a possible embodiment, the viscosity of the organic salt may be 10-14 cp, which can make the prepared porous membrane have better performance.
[0078] For example, the viscosity of the organic salt may be in the range of one or any two of 10 cp, 11 cp, 12 cp, 13 cp or 14 cp.
[0079] In a possible embodiment, the conductivity of the organic salt may be 400-650 uS / cm, which can make the prepared porous membrane have better performance.
[0080] For example, the conductivity of the organic salt may be in the range of one or any two of 400uS / cm, 450uS / cm, 500uS / cm, 550uS / cm, 600uS / cm or 650uS / cm.
[0081] In a possible embodiment, the density of the organic salt may be 0.9-0.97 g / cm 3 ; It can make the prepared porous membrane have better performance.
[0082] For example, the density of the organic salt may be 0.9 g / cm 3 、0.91g / cm 3 , 0.92g / cm 3 、0.93g / cm 3 、0.94g / cm 3 , 0.95g / cm 3 、0.96g / cm 3 or 0.97g / cm 3 One of the above or a range between any two of the above.
[0083] In a possible embodiment, on the thermogravimetric curve of the organic salt, the thermal weight loss between 300-400° C. accounts for 10-25 wt %.
[0084] The thermogravimetric curve can be obtained by thermogravimetric analysis under the following conditions: sample mass 5-10 mg, purge gas is nitrogen with a gas flow rate of 25-40 mL / min, heating rate is 10°C / min, and test temperature range is 50-800°C.
[0085] In a possible embodiment, through quantitative analysis by energy spectrum method, the organic salt contains C element and N element, the percentage of C element to the total amount of C element and N element is 60-70%, and the percentage of N element to the total amount of C element and N element is 30%-40%.
[0086] Exemplarily, the C element accounts for one of 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69% or 70% of the total amount of the C element and the N element, or a range between any two of them.
[0087] Exemplarily, the N element accounts for one of or a range between any two of 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39% or 40% of the total amount of the C element and the N element.
[0088] In a possible embodiment, the organic salt contains S element; through X-ray fluorescence spectrometry analysis, the content of S element in the organic salt is 1.0-1.2%.
[0089] Exemplarily, the content of S element in the organic salt is in the range of 1.0%, 1.1% or 1.2%, or between any two of them.
[0090] In a possible embodiment, through inductively coupled plasma emission spectrometry analysis, the organic salt includes at least one of Al element, Ca element, Na element, Si element, Ti element, K element, B element, Fe element, Mg element, Zn element, Au element, Cr element, Hg element, P element, Pt element, Sb element, Sn element, Cu element or Zr element.
[0091] Exemplarily, the organic salt may be selected from sodium salt of imidazole tetrafluoroborate, sodium salt of betaine or sodium imidazole acetate.
[0092] Furthermore, the present application does not limit the specific ratio of the polyolefin resin to the organic salt. In a possible embodiment, the organic salt accounts for 40%-80% of the total mass of the mixture.
[0093] The mixture contains 40%-80% organic salt, which can reduce the pressure, die head temperature and the probability of white smoke in the subsequent mixing, melting and extrusion processes. After subsequent stretching, extraction and stretching molding, a polyolefin microporous membrane with good ionic conductivity, good wetting effect, lower electrostatic voltage and lower number of membrane surface defects can be obtained.
[0094] Exemplarily, the organic salt accounts for one of 40%, 50%, 60%, 70% or 80% of the total mass of the mixture, or a range between any two of them.
[0095] If white oil or the like is used as a pore-forming agent, in order to improve the stability of the mixed melt, it is usually necessary to add an auxiliary agent such as an antioxidant. For example, a phenolic antioxidant is added, specifically, 2,6-di-tert-butyl-4-methylphenol, pentaerythritol-tetrakis-[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, etc. can be listed. Moreover, a secondary antioxidant can also be used in combination. Specifically, phosphorus-based antioxidants such as tris(2,4-di-tert-butylphenyl) phosphite, tetrakis(2,4-di-tert-butylphenyl)-4,4-biphenylene-diphosphite, sulfur-based antioxidants such as dilaurylthiodipropionate, etc. can be listed.
[0096] In the preparation method provided in the example of the present application, since 40%-80% of organic salt is added to the mixture, no other additives need to be added to the mixture provided in the example of the present application, and the mixture has good stability.
[0097] In a possible embodiment, no antioxidant may be added to the provided mixture. Since the mixture contains an organic salt processing aid, the stability of the mixed melt can be improved without adding any other additives such as antioxidants, and a polyolefin microporous membrane with good ionic conductivity, wetting effect and a low number of membrane surface defects can be obtained after subsequent extrusion, stretching, extraction, and stretching shaping.
[0098] Furthermore, the present application does not limit the specific temperature for heating the polyolefin resin and the processing aid, and relevant personnel may make corresponding adjustments according to the type of polyolefin resin.
[0099] In a possible embodiment, the heating temperature may be 150-300°C.
[0100] For example, when the polyolefin resin is selected from polyethylene, the heating temperature may be 150°C.
[0101] For example, when the polyolefin resin is selected from polypropylene, the heating temperature may be 200°C.
[0102] The present application does not limit specific melting equipment. In a possible embodiment, the weighed polyolefin resin and organic salt can be put into an extruder at a certain flow rate, and the melting temperature is set to 150-300°C.
[0103] Since the mixture contains organic salt, in the extruder, the pressure of the metering pump and the mixture in the pipeline can be adjusted to as low as 1.5-2.5MPa to reduce the process difficulty.
[0104] For example, in the extruder, the pressure of the metering pump and the mixture in the pipeline can be one of 1.5 MPa, 2 MPa, 2.2 MPa, 2.5 MPa, or a range between any two of them.
[0105] S2. Extruding the mixture from a die head and cooling it to form a cast sheet containing a processing aid.
[0106] For example, the mixture can be extruded from a die and then cooled by contact with a cold roll to form a cast sheet.
[0107] Since the mixture contains organic salts, the temperature of the die head can be adjusted to as low as 150-180°C during extrusion to reduce the difficulty of the process.
[0108] For example, during extrusion, the temperature of the die head may be adjusted to one of 150° C., 160° C., 170° C., 171° C., or 180° C., or a range between any two thereof.
[0109] S3. Stretch the cast sheet in at least one direction to obtain a base film.
[0110] In a possible embodiment, the cast sheet may be subjected to asynchronous biaxial stretching.
[0111] For example, it can be stretched a certain multiple along the production line direction, and then stretched a certain multiple along the vertical direction of the production line.
[0112] For example, it can be stretched 10-20 times along the production line direction, and then stretched 5-10 times along the vertical direction of the production line.
[0113] Alternatively, the cast sheet may be subjected to simultaneous biaxial stretching.
[0114] For example, the cast sheet can be subjected to synchronous biaxial stretching along the production line direction and in the direction perpendicular to the production line at the same time, and the stretching ratio can be 10-20 times.
[0115] S4, extracting the processing aid in the base film to obtain an extracted base film.
[0116] The processing aid in the base film is extracted to obtain a base film with a microporous structure.
[0117] Since the processing aid provided in the examples of the present application is an organic salt, a non-halogenated hydrocarbon extractant can be used during extraction.
[0118] Illustratively, the organic salt may be extracted using water.
[0119] Furthermore, the organic salt can be extracted using deionized water.
[0120] In the extraction process, using water as an extractant can avoid the use of hazardous chemicals and improve the environmental friendliness of the preparation process. Moreover, compared with halogenated hydrocarbon extractants such as dichloromethane, non-halogenated hydrocarbon extractants such as water can reduce the adverse effects of the extractant on the base film, improve the ionic conductivity and wettability of the polyolefin microporous membrane, and reduce the number of membrane surface defects such as crystal points, transparent or bright spots in the polyolefin microporous membrane.
[0121] The present application is not limited to a specific extraction device. In a possible embodiment, the basement membrane can be transported to an extraction tank, in which a non-halogenated hydrocarbon extractant is contained.
[0122] When the extractant is selected from water or deionized water, the base membrane can be washed with water or deionized water while being transported to the extraction tank to extract the organic salt.
[0123] S5, stretching and shaping the extracted base film in at least one direction to obtain a polyolefin microporous membrane.
[0124] After removing the organic salt, the extracted base film can be stretched and shaped. Exemplarily, the stretching multiple of the stretching and shaping can be selected from 1-5 times.
[0125] After the extracted base film is stretched and shaped, a polyolefin microporous membrane with good mechanical properties, suitable thickness, high ionic conductivity, low electrostatic voltage and low water contact angle can be obtained.
[0126] In a possible embodiment, the residual rate of organic salt in the polyolefin microporous membrane is less than 1%. The polyolefin microporous membrane prepared by the preparation method provided in the example of the present application has a residual rate of organic salt less than 1%, a high purity of the polyolefin microporous membrane, and good membrane surface performance.
[0127] The polyolefin microporous membrane provided by the examples of the present application is further described in detail below in conjunction with the embodiments.
[0128] Example 1
[0129] Embodiment 1 provides a method for preparing a polyolefin microporous membrane, comprising the following steps:
[0130] (1) 30% by weight of polyethylene and 70% by weight of 1-butyl-3-methylimidazolium tetrafluoroborate (i.e., organic salt) were put into an extruder and extruded at 105 rpm through a die head, and then cooled by contact with a cold roller at a temperature of 15° C. to form a cast sheet. The pressure of the extruder flange was 0.2 MPa, the pressure of the metering pump was 2.2 MPa, and the pressure of the melt line was 2.0 MPa; the temperature of the screw section was 160° C., the temperature of the filter / melt line was 174° C., and the temperature of the die head was 171° C.
[0131] (2) Using a stretching machine, the cast sheet obtained in step (1) is subjected to synchronous biaxial stretching at a temperature of 120° C. with a stretching ratio of 10*10 times to obtain a base film.
[0132] (3) The base film obtained in step (2) is transported to an extraction tank to extract the processing aid to obtain an extracted base film. The extractant in the extraction tank is selected from deionized water.
[0133] (4) The extracted base film was heat-set at 115° C. and wound up with a winding roller to obtain a polyolefin microporous membrane with a thickness of 9 μm.
[0134] Example 2
[0135] Example 2 provides a method for preparing a polyolefin microporous membrane, which differs from Example 1 in that:
[0136] In step (1), the pressure of the extruder flange is 0.4 MPa, the pressure of the metering pump is 4.9 MPa, and the pressure of the melt line is 4.3 MPa; the temperature of the screw section is 189°C, the temperature of the filter / melt line is 205°C, and the temperature of the die head is 201°C.
[0137] Example 3
[0138] Example 3 provides a method for preparing a polyolefin microporous membrane, which differs from Example 1 only in that 1-butyl-3-methylimidazolium tetrafluoroborate is replaced by piperidine hydrochloride (molecular formula: C 5 H 12 ClN).
[0139] Example 4
[0140] Example 4 provides a method for preparing a polyolefin microporous membrane, which is different from Example 1 only in that 60% by mass of polyethylene and 40% by mass of 1-butyl-3-methylimidazole tetrafluoroborate are put into an extruder for extrusion.
[0141] Example 5
[0142] Example 5 provides a method for preparing a polyolefin microporous membrane, which is different from Example 1 only in that 40% by mass of polyethylene and 60% by mass of 1-butyl-3-methylimidazole tetrafluoroborate are put into an extruder for extrusion.
[0143] Example 6
[0144] Example 6 provides a method for preparing a polyolefin microporous membrane, which is different from Example 1 only in that 20% by mass of polyethylene and 80% by mass of 1-butyl-3-methylimidazole tetrafluoroborate are put into an extruder for extrusion.
[0145] Example 7
[0146] Example 7 provides a method for preparing a polyolefin microporous membrane, which is different from Example 1 only in that 50% by mass of polyethylene and 50% by mass of 1-butyl-3-methylimidazolium tetrafluoroborate are put into an extruder for extrusion.
[0147] Comparative Example
[0148] The comparative example provides a method for preparing a polyolefin microporous membrane, which differs from Example 1 in that:
[0149] In step (1), 30% by weight of polyethylene and 70% by weight of white oil are put into an extruder for extrusion, and extruded through a die head at 105 rpm, and then contact-cooled by a cold roller at a temperature of 15° C. to form a cast sheet. The pressure of the extruder flange is 0.4 MPa, the pressure of the metering pump is 4.9 MPa, and the pressure of the melt line is 4.3 MPa; the temperature of the screw section is 189° C., the temperature of the filter / melt line is 205° C., and the temperature of the die head is 201° C.
[0150] In step (3), the basement membrane obtained in step (2) is transported to an extraction tank to extract the white oil to obtain an extracted basement membrane. The extractant in the extraction tank is selected from dichloromethane.
[0151] Experimental Example 1
[0152] The thickness, surface density, porosity, air permeability, needle puncture strength, MD tensile strength, TD tensile strength, MD elongation, TD elongation, breakdown voltage and residual amount of processing aid of the polyolefin microporous membranes of Examples 1-7 and the comparative example were tested, and the test results are shown in Table 1; the ionic conductivity, water contact angle and electrostatic voltage of the polyolefin microporous membranes of Examples 1-5 and the comparative example were tested, and the test results are shown in Table 2.
[0153] The test method is as follows:
[0154] The test steps for thickness, surface density and porosity are as follows: cut three pieces of polyolefin microporous membranes 150 mm apart in the longitudinal direction from the membrane roll (if the width of the polyolefin microporous membrane is ≥100 mm, the size of the sample is: 100 mm long and 100 mm wide; if the width of the polyolefin microporous membrane is <100 mm, the size of the sample is: 100 mm long and the width is the actual width of the polyolefin microporous membrane). Measure the length, width and thickness (i.e. the thickness in Table 1) of the cut sample in accordance with the provisions of GB / T6673-2001 and GB / T6672-2001 respectively. Weigh the mass of the cut sample using an analytical balance with a resolution of 0.0001 g, and then calculate the surface density and porosity according to formulas (1) and (2), respectively.
[0155] Formula (1) is:
[0156] In formula (1):
[0157] ρ1 represents the surface density of the cut sample, in grams per square centimeter (g / cm 2 );
[0158] m represents the mass of the sample cut, in grams (g);
[0159] L represents the length of the cut sample, in centimeters (cm);
[0160] b represents the width of the cut sample, in centimeters (cm).
[0161] The lengths of the cut samples corresponding to Examples 1-2 and the comparative examples are all 60 mm, and the widths are all 40 mm. The thicknesses of the cut samples corresponding to Examples 1-2 and the comparative examples are shown in Table 1.
[0162] Formula (2) is:
[0163] In formula (2):
[0164] ρ1 represents the surface density of the cut sample, in grams per square centimeter (g / cm 2 );
[0165] P represents the porosity of the sample, in %;
[0166] d represents the thickness of the cut sample, in micrometers (μm);
[0167] ρ0 represents the density of polyethylene resin, in grams per cubic centimeter (g / cm 3 ).
[0168] The test steps for air permeability are as follows: at room temperature, use a Wang Yan-type air permeability meter to set 100cc of gas to pass through the polyolefin microporous membrane, and record the stable value after 5 seconds of measurement.
[0169] The test steps for needle puncture strength are as follows: cut a 100mm×100mm polyolefin microporous membrane from the film roll, evenly divide the test points on the cut film according to the number of test points, use the XJ-830 puncture strength tester and connect it to the TESRER software, enter the software interface and adjust the angular velocity to 50mm / min, fix the cut film on the test platform of the XJ-830 puncture strength tester, pierce the diaphragm with a needle with a diameter of 2mm at the set rate, and then test the needle strength.
[0170] The test steps for MD tensile strength, TD tensile strength, MD stretch rate and TD stretch rate are as follows: use electronic universal material testing machine XJ830, test sample specifications: width 15mm × length 20cm, measure at a travel speed of 200mm / min, and obtain MD tensile strength and TD tensile strength respectively; MD stretch rate (%) = [(MD direction stretching length - MD direction stretching length before) / MD direction stretching length] × 100%, TD stretch rate (%) = [(TD direction stretching length - TD direction stretching length before) / TD direction stretching length] × 100%.
[0171] The test steps for breakdown voltage shall be carried out in accordance with 10.2 of GB / T1408.1-2006 Insulating Material Electrical Strength Test Method.
[0172] The test steps for ionic conductivity are carried out in accordance with 6.6.2 of GB / T36363-2018 Polyolefin separator for lithium-ion batteries.
[0173] The test steps of water contact angle are as follows: the prepared polyolefin microporous membrane is cut into a sample with a length × width of 25 mm × 100 mm, and the sample is fixed to a glass slide with double-sided tape for testing; the test steps are carried out according to GB / T 30693-2014 Measurement of contact angle of plastic film with water 10.2.
[0174] The test steps of electrostatic voltage are as follows: under the environmental conditions of temperature of 25°C and humidity of 50%, place the test head of the electrostatic meter at a distance of 1 in (i.e. 254 mm) from the polyolefin microporous membrane; turn on the switch of the electrostatic meter and the measurement begins; when the focusing light source of the electrostatic meter coincides, observe the displayed value after it becomes relatively stable.
[0175] Table 1
[0176]
[0177]
[0178] Note: The water contact angle in Table 1 refers to the water contact angle on the surface of the polyolefin microporous membrane. The detection temperature of the water contact angle is 23.3°C and the humidity is 45%. In Table 1, the processing aids corresponding to Examples 1-7 and the processing aids corresponding to the comparative examples are all white oil.
[0179] Table 2
[0180] Ionic conductivity (mS / cm) Water contact angle (°) Electrostatic voltage (kv) Example 1 1.2117 112 0.7 Example 2 1.3987 116.8 0.6 Example 3 1.1866 115 0.6 Example 4 1.2578 111 0.5 Example 5 1.345 113 0.5 Comparative Example 0.8561 119 0.8
[0181] It can be seen from Table 1 that compared with the polyolefin microporous membrane prepared in the comparative example, the comprehensive performance of the polyolefin microporous membrane prepared in Examples 1-7 is better.
[0182] It can be seen from Table 2 that, compared with the polyolefin microporous membrane prepared in the comparative example, the polyolefin microporous membrane prepared in Examples 1-5 has higher ion conductivity, lower water contact angle and lower electrostatic voltage.
[0183] From the comparison between Example 1 and the comparative example, it can be seen that since Example 1 uses organic salt, when preparing the polyolefin microporous membrane, the organic salt and the polyolefin resin can be mixed and heated at a relatively low pressure to obtain a molten mixture, which can reduce the process difficulty.
[0184] Experimental Example 2
[0185] The number of membrane surface defects of the polyolefin microporous membranes prepared in Example 1, Example 3 and the comparative example was statistically analyzed, and the statistical results are shown in Table 3.
[0186] The test method for membrane surface defects is as follows: using a CCD high-speed camera, the detection speed is 0-300m / min, the distance between the polyolefin microporous membrane and the CCD high-speed camera is 1m, and the shooting area is an area of 2000m×2m in length×width.
[0187] Table 3
[0188]
[0189] In Table 3, crystal points represent darker dots in the shooting field of view; transparency represents brighter dots in the shooting field of view; water stain defects are bright spot defects, and bright spots represent brighter blocks in the shooting field of view.
[0190] It can be seen from Table 3 that compared with the polyolefin microporous membrane prepared in the comparative example, the polyolefin microporous membranes prepared in Example 1 and Example 3 have fewer membrane surface defects.
[0191] Experimental Example 3
[0192] With reference to the Integrated Emission Standard of Air Pollutants (GB16297-1996), the tail gas of the process for preparing the polyolefin microporous membrane of Example 1 and the comparative example was measured respectively. The measurement results are shown in Table 4.
[0193] Table 4
[0194]
[0195] It can be seen from Table 4 that compared with the comparative example using white oil to prepare the polyolefin resin porous membrane, the tail gas emission of Example 1 using imidazole tetrafluoroborate to prepare the polyolefin resin porous membrane is lower, indicating that the process of preparing the polyolefin resin porous membrane using imidazole tetrafluoroborate is more environmentally friendly.
[0196] In summary, the present application utilizes organic salt as a processing aid, and can extrude at a lower temperature and pressure in the extruder, making the preparation process more environmentally friendly, and the obtained polyolefin microporous membrane has higher ionic conductivity, lower water contact angle, lower electrostatic voltage and fewer mask defects.
[0197] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A method for preparing a polyolefin microporous membrane, characterized in that: The method comprises the following steps performed in sequence: (1) mixing and heating a polyolefin resin and a processing aid into a molten mixture; (2) extruding the mixture from a die head and cooling it to form a cast sheet containing the processing aid; (3) stretching the cast sheet in at least one direction to obtain a base film; (4) extracting the processing aid in the base film to obtain an extracted base film; (5) stretching the extracted base film in at least one direction to obtain the polyolefin microporous membrane; Wherein, the processing aid comprises an organic salt.
2. The method for preparing a polyolefin microporous membrane according to claim 1, characterized in that: The organic salt is a liquid organic salt.
3. The method for preparing a polyolefin microporous membrane according to claim 1, characterized in that: The organic salt includes at least one of an imidazole salt compound and a piperidine salt compound.
4. The method for preparing a polyolefin microporous membrane according to claim 3, characterized in that: The imidazole salt compound includes at least one of an imidazole salt or a salt having an imidazole structure containing a substituent; the piperidine salt compound includes at least one of a piperidine salt or a salt having a piperidine structure containing a substituent.
5. The method for preparing a polyolefin microporous membrane according to claim 3, characterized in that: On the thermogravimetric curve of the organic salt, the thermal weight loss between 300-400° C. accounts for 10-25 wt %.
6. The method for preparing a polyolefin microporous membrane according to claim 3, characterized in that: Through inductively coupled plasma emission spectrometry analysis, the organic salt contains at least one of Al element, Ca element, Na element, Si element, Ti element, K element, B element, Fe element, Mg element, Zn element, Au element, Cr element, Hg element, P element, Pt element, Sb element, Sn element, Cu element or Zr element.
7. The method for preparing a polyolefin microporous membrane according to claim 3, characterized in that: Through quantitative analysis by energy spectrum method, the organic salt contains C element and N element, the C element accounts for 60%-70% of the total amount of the C element and the N element, and the N element accounts for 30%-40% of the total amount of the C element and the N element.
8. The method for preparing a polyolefin microporous membrane according to claim 3, characterized in that: According to the analysis by X-ray fluorescence spectrometry, the content of S element in the organic salt is 1.0-1.2%.
9. The method for preparing a polyolefin microporous membrane according to claim 3, characterized in that: The viscosity of the organic salt is 10-14 cp; And / or, the conductivity of the organic salt is 400-650uS / cm; And / or, the density of the organic salt is 0.9-0.97 g / cm 3 .
10. The method for preparing a polyolefin microporous membrane according to claim 1, characterized in that: The organic salt is selected from one or more of imidazole tetrafluoroborate, betaine salt, imidazole acetate, piperidine hydrochloride, imidazole dinitrile ammonium salt, imidazole ethyl sulfate salt, imidazole bisfluorosulfonyl imide salt and bistrifluorosulfonyl imide salt.
11. The method for preparing a polyolefin microporous membrane according to any one of claims 1 to 10, characterized in that: In the step (4), the extractant used in the extraction is a non-halogenated hydrocarbon.
12. The method for preparing a polyolefin microporous membrane according to claim 11, characterized in that: The extractant is water.
13. The method for preparing a polyolefin microporous membrane according to claim 12, characterized in that: The water is deionized water.
14. The method for preparing a polyolefin microporous membrane according to any one of claims 1 to 10, characterized in that: No other auxiliary agent is added in the step (1).
15. The method for preparing a polyolefin microporous membrane according to any one of claims 1 to 10, characterized in that: No antioxidant is added in step (1).
16. The method for preparing a polyolefin microporous membrane according to claim 1, characterized in that: The weight average molecular weight of the polyolefin resin is 4.0×10 5 -15.0×10 5 .
17. The method for preparing a polyolefin microporous membrane according to claim 1, characterized in that: The polyolefin resin is selected from one or more of polyethylene, polypropylene, polyisoprene or polybutylene.
18. The method for preparing a polyolefin microporous membrane according to claim 1, characterized in that: The stretching in the step (3) is asynchronous biaxial stretching or synchronous biaxial stretching.
19. The method for preparing a polyolefin microporous membrane according to claim 1, characterized in that: In the step (1), the organic salt accounts for 40% to 80% of the total mass of the mixture.
20. The method for preparing a polyolefin microporous membrane according to claim 1, characterized in that: In the polyolefin microporous membrane obtained in the step (5), the residual rate of the organic salt is less than 1%.
21. The method for preparing a polyolefin microporous membrane according to claim 1, characterized in that: The temperature of the die in step (2) is 150-180°C; And / or, the pressure of the molten mixture in the pipeline in step (1) is 1.5-2.5 MPa.
Citation Information
Cited By
Microporous film for composite current collector, preparation method therefor, and composite current collector
WO2026158594A1