A method for preparing porous polyetheretherketone microspheres
The preparation of porous PEEK microspheres through liquid-liquid phase replacement method has solved the high cost and biocompatibility of PEEK microsphere preparation in the prior art, achieved efficient and simple preparation of porous microspheres, and improved the biological activity of the material and Value of industrial application.
Patent Information
- Application Number
- CN202411258973.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-10
AI Technical Summary
The existing PEEK porous microsphere preparation methods have problems such as high cost, complex processes, and the inability to prepare microspheres with small pore sizes and materials with reduced biocompatibility and mechanical strength.
By liquid-liquid phase replacement method, the polyether etherketone powder is dissolved in dichloroacetic acid, and then dripped into a mixture of ethanol and water for solid-liquid separation to prepare porous microspheres. By controlling the dropping speed and temperature, looseness is formed. The porous structure is washed and hydrothermal treatment is performed to enhance the bioactivity of the microspheres.
The production of porous PEEK microspheres is achieved by low-cost and simple processes, retaining the excellent properties of the material, improving the bioactivity and hydrophilicity of the microspheres, and having great industrial application potential.
Smart Images

Figure CN118772480B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of porous materials, and in particular to a method for preparing porous polyetheretherketone microspheres. Background Art
[0002] Porous microspheres have a special periodic structure, high specific surface area, low relative density, high specific strength, good assemblability, and high porosity. They have shown broad application prospects in the fields of biomedicine, adsorption separation, catalysis, optics, sensors, and electrochemistry. Polyetheretherketone (PEEK) material has good biocompatibility and chemical stability, high mechanical properties, high temperature resistance, corrosion resistance, and radiation resistance. It is a high-quality material for preparing porous microspheres. However, due to the defects of PEEK such as high melting point and high viscosity in the molten state, the preparation of its porous microspheres is technically difficult.
[0003] The reported preparation methods of PEEK porous microspheres include adding pore-forming agent, sintering, 3D printing and concentrated sulfuric acid sulfonation. Among them, the addition of pore-forming agent and sintering are complex processes; 3D printing technology is costly and cannot achieve the preparation of PEEK microspheres with smaller pore sizes; concentrated sulfuric acid sulfonation, PEEK material will have residual sulfuric acid groups after concentrated sulfuric acid sulfonation, affecting its biocompatibility, and PEEK will reduce its molecular weight after being degraded by concentrated sulfuric acid, resulting in a decrease in the mechanical strength of the material. Summary of the invention
[0004] In view of this, the object of the present invention is to provide a method for preparing porous polyetheretherketone microspheres. The preparation method provided by the present invention has simple process, low cost, and does not change the chemical properties of the surface functional groups of the polyetheretherketone material.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing porous polyetheretherketone microspheres, comprising the following steps:
[0007] dissolving polyetheretherketone powder in dichloroacetic acid to obtain a polyetheretherketone solution;
[0008] The polyetheretherketone solution is dripped into a mixed solution of ethanol and water, and the porous polyetheretherketone microspheres are obtained through solid-liquid separation.
[0009] Preferably, the usage ratio of the polyetheretherketone powder to dichloroacetic acid is (12-18) g:100 mL.
[0010] Preferably, the dissolving temperature is 170-200°C.
[0011] Preferably, the volume fraction of ethanol in the mixture of ethanol and water is 30-70%.
[0012] Preferably, the volume fraction of ethanol in the mixture of ethanol and water is 50%.
[0013] Preferably, the dripping is performed using a syringe, and the needle of the syringe is a 22-26G Teflon-lined needle.
[0014] Preferably, the distance between the needle and the liquid surface of the mixture of ethanol and water is 5 to 10 cm.
[0015] Preferably, the dripping speed is 40 to 60 drops per minute.
[0016] Preferably, after the solid-liquid separation, the obtained microspheres are sequentially washed, hydrothermally treated and dried, and the hydrothermal treatment temperature is 160-180° C. and the time is 6-8 hours.
[0017] Preferably, the porous polyetheretherketone microspheres have an average pore size of 20-100 nm, a porosity of 28-70%, and a specific surface area of 40-80 m 2 / g.
[0018] Beneficial effects of the present invention: The present invention utilizes a liquid-liquid phase replacement method to prepare polyetheretherketone porous microspheres. When a good solvent (dichloroacetic acid) containing polyetheretherketone powder is dropped into a poor solvent (a mixture of ethanol and water), the rapid exchange between the good solvent and the poor solvent causes the polyetheretherketone to undergo liquid-liquid phase separation, forming condensed phase droplets and gradually solidifying. When the exchange between the two is completed, loose and porous polyetheretherketone microspheres are prepared. The present invention has low cost for preparing porous polyetheretherketone microspheres, simple process, and great industrial application potential; using dichloroacetic acid as a good solvent for dissolving polyetheretherketone powder, the preparation process will not change the chemical properties of the surface functional groups of the polyetheretherketone material, and the excellent performance of the polyetheretherketone is retained; in addition, the hydrophilicity of the prepared porous polyetheretherketone microspheres is improved to a certain extent compared with the polyetheretherketone powder raw material, so that the biological activity of the polyetheretherketone material is also improved to a certain extent. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The actual photos of the PEEK powder raw material and the prepared PEEK porous microspheres in Example 2 are shown in FIG. Figure 1 From left to right in the figure are the real photos of PEEK powder, the real photos of PEEK porous microspheres, and the size of PEEK porous microspheres;
[0020] Figure 2 The surface and internal SEM morphology images of the PEEK porous microspheres prepared in Example 2 are shown in FIG. Figure 2(a) is the complete morphology of PEEK porous microspheres, (b) is the surface morphology of PEEK porous microspheres, and (c) is the cross-sectional morphology of PEEK porous microspheres;
[0021] Figure 3 The infrared spectra of the PEEK powder raw material and the prepared PEEK porous microspheres in Example 2;
[0022] Figure 4 The surface and internal SEM morphology pictures of the PEEK porous microspheres prepared in Example 3 are as follows: Figure 4 (a) is the complete morphology of PEEK porous microspheres, (b) is the surface morphology of PEEK porous microspheres, and (c) is the cross-sectional morphology of PEEK porous microspheres. DETAILED DESCRIPTION
[0023] The present invention provides a method for preparing porous polyetheretherketone microspheres, comprising the following steps:
[0024] dissolving polyetheretherketone powder in dichloroacetic acid to obtain a polyetheretherketone solution;
[0025] The polyetheretherketone solution is dripped into a mixed solution of ethanol and water, and the porous polyetheretherketone microspheres are obtained through solid-liquid separation.
[0026] In the present invention, unless otherwise specified, the raw materials involved are commercially available products well known to those skilled in the art.
[0027] The present invention dissolves polyetheretherketone powder (PEEK powder) in dichloroacetic acid to obtain a polyetheretherketone solution. In the present invention, the particle size of the polyetheretherketone powder is preferably 100-800 mesh. The present invention has no special requirements for the polyetheretherketone powder, and the polyetheretherketone powder well known to those skilled in the art can be used. In an embodiment of the present invention, the polyetheretherketone powder is purchased from Victrex, UK, with a brand of 450G. In the present invention, the amount ratio of the polyetheretherketone powder to dichloroacetic acid is preferably (12-18) g:100 mL, more preferably (12.8-15) g:100 mL, and the dichloroacetic acid is used as a good solvent for dissolving PEEK powder. In the present invention, the dissolution temperature is preferably 170-200°C, more preferably 180-190°C.
[0028] In the present invention, the specific operation of the dissolution is preferably: placing the polyetheretherketone powder in a single-necked flask, adding dichloroacetic acid dried by magnesium sulfate thereto, sealing the flask with a bottle cap, placing the flask in an oil bath and heating it to 170-200° C., stirring with a magnetic force until the polyetheretherketone powder is completely dissolved in the dichloroacetic acid to obtain a polyetheretherketone solution.
[0029] After obtaining the polyetheretherketone solution, the present invention drips the polyetheretherketone solution into a mixture of ethanol and water, and obtains the porous polyetheretherketone microspheres through solid-liquid separation. In the present invention, the volume fraction of ethanol in the mixture of ethanol and water is preferably 30-70%, more preferably 50%; the water is preferably deionized water; the mixture of ethanol and water is used as a poor solvent for PEEK. In the present invention, it is preferred to use a syringe for the dripping, the syringe is preferably an inert polypropylene syringe, and the needle of the syringe is preferably a 22-26G Teflon-lined needle, specifically a 22G, 23G, 24G, 25G or 26G Teflon-lined needle. In the present invention, the needle model is different, the pore size of the needle is different, and the particle size of the porous polyetheretherketone microspheres is affected by the pore size of the needle. The larger the pore size of the needle, the larger the particle size of the prepared porous polyetheretherketone microspheres. In the present invention, the distance between the needle and the liquid surface of the mixture of ethanol and water is preferably 5-10 cm, specifically 5, 6, 7, 8, 9 or 10 cm; the dripping speed is preferably 40-60 drops / minute, specifically 40, 50 or 60 drops / minute. In the present invention, when polyetheretherketone dissolved in a good solvent (dichloroacetic acid) is dripped into a poor solvent (a mixture of ethanol and water), a rapid exchange occurs between the good solvent and the poor solvent, and the solubility of polyetheretherketone decreases, thereby forming polyetheretherketone microspheres, and at the same time, as the poor solvent inside the microspheres gradually diffuses outward, a pore structure is formed.
[0030] After the polyetheretherketone solution is dripped, the obtained mixed liquid is preferably allowed to stand, and then solid-liquid separation is performed. In the present invention, the standing time is preferably 2 to 3 hours. During the dripping of the polyetheretherketone solution, the rapid exchange between the good solvent and the poor solvent causes the polyetheretherketone to undergo liquid-liquid phase separation to form microspheres. The present invention allows the microspheres to stand in the poor solvent for 2 to 3 hours. The standing process helps the liquid-liquid phase separation process to reach equilibrium, allowing the microspheres to be further formed and stabilized, thereby obtaining microspheres with more uniform particle sizes.
[0031] The present invention has no special requirements for the solid-liquid separation method, and any solid-liquid separation method well known to those skilled in the art may be used.
[0032] In the present invention, after the solid-liquid separation, the obtained microspheres are preferably washed, hydrothermally treated and dried in sequence. In the present invention, the water washing is preferably carried out with deionized water, and the water washing is preferably carried out multiple times, the purpose of which is to remove the dichloroacetic acid and ethanol remaining in the microspheres. In the present invention, the temperature of the hydrothermal treatment is preferably 160-180°C, more preferably 170°C, the time is preferably 6-8h, more preferably 7-8h, and the heating rate to the temperature of the hydrothermal treatment is preferably 5°C per 5 minutes. In the present invention, the washed microspheres are preferably transferred to a hydrothermal synthesis reactor, deionized water not exceeding 80% of the volume of the reactor liner is added to the reactor, and then the hydrothermal treatment is carried out in a muffle furnace. The present invention utilizes the unique reaction conditions under the hydrothermal high temperature and high pressure environment to further enrich the surface properties and pore structure of polyetheretherketone microspheres. In the present invention, the drying is preferably carried out in a vacuum drying oven.
[0033] The present invention dissolves polyetheretherketone powder in dichloroacetic acid, and uses a liquid-liquid phase replacement method to prepare porous polyetheretherketone microspheres. The microspheres can be quickly formed by controlling the concentration and dissolution temperature of the solution. The method is simple and convenient, has strong controllability, good repeatability, and is easy to mass produce. In the present invention, the porous polyetheretherketone microspheres have an average pore size of 20-100 nm, a median pore size of 40-210 nm, a porosity of 28-70%, and a specific surface area of 40-80 m 2 / g, the bulk density is 0.35~0.75g / mL, and the skeleton density is 0.99~1.20g / mL.
[0034] The present invention prepares the polyetheretherketone material with excellent performance into porous microspheres without changing the chemical properties of the surface functional groups of the polyetheretherketone material. The obtained porous polyetheretherketone microspheres have significant advantages in the fields of catalyst carriers, drug release, filtration and separation, sensors, adsorption materials and optoelectronic devices due to their high specific surface area, good mass transfer performance and controllability. These characteristics make the porous polyetheretherketone microspheres have extremely high application value in scientific research and industrial applications.
[0035] In order to further illustrate the present invention, the preparation method of the porous polyetheretherketone microspheres provided by the present invention is described in detail below with reference to examples, but they should not be construed as limiting the scope of protection of the present invention.
[0036] Example 1
[0037] The preparation steps of porous polyetheretherketone microspheres (PEEK porous microspheres) are as follows:
[0038] 2.25 g of PEEK powder (100-800 mesh, purchased from Victrex, UK, brand 450G) was weighed and transferred to a 100 mL single-necked flask, 17.5 mL of dichloroacetic acid dried over magnesium sulfate was added, the flask was sealed with a cap and placed in an oil bath and heated to 180 °C with magnetic stirring to completely dissolve the PEEK powder in the dichloroacetic acid to obtain a PEEK solution.
[0039] The PEEK solution was injected into an ethanol / deionized water mixture using an inert polypropylene syringe with a 22G Teflon-lined needle. The volume concentration of ethanol in the ethanol / deionized water mixture was 50%, the distance between the needle and the liquid surface of the mixture was 5 cm, and the PEEK solution dripping rate was controlled at 40 drops / minute. After the PEEK solution was dripped, the resulting mixed liquid was allowed to stand for 3 hours, and the PEEK microspheres were collected by solid-liquid separation.
[0040] The collected PEEK microspheres were washed with deionized water for multiple times to remove residual dichloroacetic acid and ethanol, and then transferred to a 300 mL hydrothermal synthesis reactor. Deionized water not exceeding 80% of the volume of the reactor was added to the reactor. The temperature was set to 170° C. in a muffle furnace and hydrothermally treated for 8 hours. Finally, the PEEK microspheres were transferred to a vacuum drying oven for drying to obtain the PEEK porous microspheres.
[0041] Example 2
[0042] The preparation steps of porous polyetheretherketone microspheres (PEEK porous microspheres) are as follows:
[0043] 2.25 g of PEEK powder (100-800 mesh, purchased from Victrex, UK, brand 450G) was weighed and transferred to a 100 mL single-necked flask, 15.0 mL of dichloroacetic acid dried over magnesium sulfate was added, the flask was sealed with a cap and placed in an oil bath and heated to 180 °C with magnetic stirring to completely dissolve the PEEK powder in the dichloroacetic acid to obtain a PEEK solution.
[0044] Use an inert polypropylene syringe with a 22G Teflon-lined needle to inject the above PEEK solution into an ethanol / deionized water mixture, where the volume concentration of ethanol in the ethanol / deionized water mixture is 50%, the distance between the needle and the liquid surface of the mixture is 5 cm, and the PEEK solution dripping rate is controlled at 40 drops / minute. After the PEEK solution is dripped, the resulting mixed liquid is allowed to stand for 3 hours, and the PEEK microspheres are collected by solid-liquid separation.
[0045] The collected PEEK microspheres were washed with deionized water for several times to remove the residual dichloroacetic acid and ethanol, and then transferred to a 300 mL hydrothermal synthesis reactor. Deionized water not exceeding 80% of the volume of the reactor was added to the reactor. The temperature was set to 170°C in a muffle furnace and hydrothermally treated for 8 hours. Finally, the PEEK microspheres were transferred to a vacuum drying oven for drying to obtain PEEK porous microspheres.
[0046] Example 3
[0047] The preparation steps of porous polyetheretherketone microspheres (PEEK porous microspheres) are as follows:
[0048] 2.25 g of PEEK powder (100-800 mesh, purchased from Victrex, UK, brand 450G) was weighed and transferred to a 100 mL single-necked flask, 17.5 mL of dichloroacetic acid dried over magnesium sulfate was added, the flask was sealed with a cap and placed in an oil bath and heated to 180 °C with magnetic stirring to completely dissolve the PEEK powder in the dichloroacetic acid to obtain a PEEK solution.
[0049] The PEEK solution was injected into an ethanol / deionized water mixture using an inert polypropylene syringe with a 26G Teflon-lined needle. The volume concentration of ethanol in the ethanol / deionized water mixture was 50%, the distance between the needle and the liquid surface of the mixture was 5 cm, and the PEEK solution dripping rate was controlled at 40 drops / minute. After the PEEK solution was dripped, the resulting mixed liquid was allowed to stand for 3 hours, and the PEEK microspheres were collected by solid-liquid separation.
[0050] The collected PEEK microspheres were washed with deionized water for several times to remove the residual dichloroacetic acid and ethanol, and then transferred to a 300 mL hydrothermal synthesis reactor. Deionized water not exceeding 80% of the volume of the reactor was added to the reactor. The temperature was set to 170°C in a muffle furnace and hydrothermally treated for 8 hours. Finally, the PEEK microspheres were transferred to a vacuum drying oven for drying to obtain PEEK porous microspheres.
[0051] Figure 1 The actual photos of the PEEK powder raw material and the prepared PEEK porous microspheres in Example 2 are shown in FIG. Figure 1 From left to right are the actual photos of PEEK powder, the actual photos of PEEK porous microspheres, and the size of PEEK porous microspheres. Figure 1 It can be seen that the PEEK porous microspheres prepared in Example 2 have good morphology and particle sizes ranging from several hundred micrometers to 2 millimeters.
[0052] Figure 2 The surface and internal SEM morphology images of the PEEK porous microspheres prepared in Example 2 are shown in FIG. Figure 2(a) is the complete morphology of PEEK porous microspheres, (b) is the complete surface morphology of PEEK porous microspheres, and (c) is the cross-sectional morphology of PEEK porous microspheres. Figure 2 It can be seen that the PEEK porous microspheres have an obvious honeycomb porous structure, and the internal pore size of the microspheres is larger than the surface pore size. The PEEK microspheres with porous structure have a large number of loading sites, so they are a very potential carrier.
[0053] Figure 3 The infrared spectra of the PEEK powder raw material and the prepared PEEK porous microspheres in Example 2 are shown in FIG. Figure 3 It can be seen that the peak positions of the infrared spectra of the PEEK porous microspheres are similar to those of the raw powder materials, indicating that the surface functional groups of the PEEK powder have not changed after being dissolved in dichloroacetic acid, which is different from the method of preparing microspheres by sulfonating the PEEK powder with concentrated sulfuric acid (the sulfonation reaction generates sulfonated polyetheretherketone, and the functional groups of the polyetheretherketone have changed), which is the main highlight of the present invention.
[0054] The hydrophilicity of the PEEK porous microspheres prepared in Example 2 was characterized after tableting. The water contact angle of the PEEK powder was measured to be 80.7 ± 7.3°, while the water contact angle of the PEEK porous microspheres decreased to 70.2 ± 5.1°, indicating that the hydrophilicity of the PEEK microspheres was improved to a certain extent compared with the powder raw materials, and thus the biological activity of the material was also improved to a certain extent.
[0055] Figure 4 The surface and internal SEM morphology pictures of the PEEK porous microspheres prepared in Example 3 are as follows: Figure 4 (a) is a complete morphology of PEEK porous microspheres, (b) is a complete surface morphology of PEEK porous microspheres, and (c) is a cross-sectional morphology of PEEK porous microspheres. The particle size has a significant effect on the pore structure of the surface and cross section of PEEK porous microspheres. The pore size inside the cross section of the microsphere sample of Example 3 with a smaller particle size is significantly smaller than that of the microsphere sample of Example 2 with a larger particle size.
[0056] The PEEK porous microspheres prepared under different conditions in the examples were analyzed by mercury porosimetry. The results are shown in Table 1.
[0057] It can be seen from Table 1 that although the mass concentration of PEEK is different in the preparation process of PEEK porous microspheres in Example 1 and Example 2, the physical properties of the two microsphere samples with similar particle sizes are similar, indicating that the mass concentration of PEEK in the preparation process will not affect the parameters such as the pore size, porosity, and specific surface area of the PEEK porous microspheres; from the comparison of the results of Example 2 and Example 3, it can be seen that the particle size of the microsphere sample is the main factor affecting the physical properties of the PEEK porous microspheres. The microsphere samples with larger particle sizes have better specific surface area and pore structure, which is consistent with Figure 2 and Figure 4 The characterization results are consistent.
[0058] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. A method for preparing porous polyetheretherketone microspheres, characterized in that: The following steps are involved: dissolving polyetheretherketone powder in dichloroacetic acid to obtain a polyetheretherketone solution; The polyetheretherketone solution is dripped into a mixture of ethanol and water, and the porous polyetheretherketone microspheres are obtained through solid-liquid separation; the volume fraction of ethanol in the mixture of ethanol and water is 50%; a syringe is used for the dripping, and the needle of the syringe is a 22~26G Teflon-lined needle; the distance between the needle and the liquid surface of the mixture of ethanol and water is 5~10 cm.
2. The method for preparing porous polyetheretherketone microspheres according to claim 1, characterized in that: The dosage ratio of the polyetheretherketone powder to dichloroacetic acid is (12-18) g:100 mL.
3. The method for preparing porous polyetheretherketone microspheres according to claim 1 or 2, characterized in that: The dissolving temperature is 170-200°C.
4. The method for preparing porous polyetheretherketone microspheres according to claim 1, characterized in that: The dripping speed is 40 to 60 drops per minute.
5. The method for preparing porous polyetheretherketone microspheres according to claim 1, characterized in that: The porous polyetheretherketone microspheres have an average pore size of 20-100 nm, a porosity of 28-70%, and a specific surface area of 40-80 m 2 / g.
Citation Information
Patent Citations
Polymer carrier with nanopore structure for cell culture as well as preparation method and application of polymer carrier
CN115093703A
Cable insulating material based on polyetherketoneketone and preparation method thereof
CN116239808A
Measurement of molecular weight distribution for aromatic straight chain polymer
JP1990008740A