Modified calcium carbonate as well as preparation method and application thereof

By forming a double-layer coating technology of calcium silicate and fatty acid calcium on the surface of calcium carbonate, it solves the quality problem when the stretching rate is high in the preparation of breathable membranes, improves the dispersion of calcium carbonate and the performance of the breathable membrane, and achieves high efficiency preparation.

CN118772486APending Publication Date: 2024-10-15GUANGZHOU HUAXINKE ENTERPRISE +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410970485.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

When preparing breathable films with the existing technology, problems such as rib marks, uneven thickness, perforation, and film breakage are likely to occur when the stretching rate exceeds 160 mm/min. Moreover, fatty acids and their salts do not completely coat calcium carbonate and have a low degree of activation. , cannot effectively improve the dispersion of calcium carbonate.

Method used

Using double-layer coating technology, a needle-like calcium silicate layer is first formed on the surface of calcium carbonate, and then a fatty acid calcium layer is coated to improve the dispersion and coating effect of calcium carbonate, and prepare modified calcium carbonate with high activation degree.

Benefits of technology

It achieves uniform micropore distribution, good mechanical properties, and high air permeability of the breathable film, and significantly increases the stretching rate during the preparation of the breathable film, with an activation degree of ≥95% and a moisture content of ≤0.1%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772486A_ABST
    Figure CN118772486A_ABST
Patent Text Reader

Abstract

The invention relates to modified calcium carbonate and a preparation method and application thereof, and belongs to the technical field of calcium carbonate. The modified calcium carbonate provided by the invention comprises calcium carbonate and a calcium silicate layer coated on the surface of the calcium carbonate, wherein the surface of the calcium silicate layer is also coated with a fatty acid calcium layer. Calcium carbonate is modified through double-layer coating, firstly, the surface of calcium carbonate is coated with a layer of calcium silicate inorganic matter, a supporting effect is formed on the surface of calcium carbonate, and calcium carbonate agglomeration is prevented; according to the present invention, the surface of the calcium carbonate can be completely coated under the action of the double-layer coating treatment, such that the agglomeration of the calcium carbonate can be effectively prevented, the prepared calcium carbonate has good dispersibility, and the gas-permeable membrane preparation speed can achieve 200 mm / min.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of calcium carbonate, and particularly relates to modified calcium carbonate and a preparation method and application thereof. Background Art

[0002] The breathable membrane is made by using polyethylene and calcium carbonate to produce micropores at the interface between the surface of calcium carbonate particles and polyethylene during the stretching process. It has the functions of waterproof and breathable and is mainly used in protective clothing, diapers, sanitary napkins, food preservation and other fields.

[0003] Currently, modified ground calcium carbonate used in breathable membranes is primarily modified with stearic acid and its salts. Patent CN116438231A discloses an ultrafine, surface-treated filler for thin, breathable membranes. The membrane comprises at least one thermoplastic polymer and a surface-treated filler material, wherein the surface-treated filler material comprises at least one calcium carbonate-containing filler material, and a treatment layer on the surface of the at least one calcium carbonate-containing filler material, the treatment layer comprising at least one monosubstituted succinic anhydride and / or at least one monosubstituted succinic acid and / or a salt thereof. This method primarily modifies calcium carbonate with monosubstituted succinic anhydride, acid, or salt thereof, following the same principle as modification with stearic acid and its salts. Patent CN117777760A discloses a modified ground calcium carbonate, its preparation method, and application. The method comprises the following steps: preliminary grinding, grading, and screening the calcium carbonate to obtain semi-finished particles; ball milling and grading the semi-finished particles to obtain a particle population; acidifying the particle population to obtain acidified calcium carbonate particles; and mixing the acidified calcium carbonate particles with stearic acid for surface treatment to obtain the modified ground calcium carbonate. The modified ground calcium carbonate can be used in the production of ground calcium carbonate for polyolefin breathable film masterbatches with various requirements. This patent utilizes stearic acid to modify the acidified calcium carbonate.

[0004] However, the use of fatty acids and their salts to coat calcium carbonate cannot completely coat the calcium carbonate, and the activation degree is basically between 80-90%. At the same time, it is also impossible to coat calcium carbonate with fine particles. When added to the resin, it will be unevenly dispersed and agglomerated, resulting in the appearance of rib patterns, uneven thickness, perforations, and film breakage when preparing breathable membranes at a speed exceeding 160 mm / min.

[0005] Therefore, it is of great significance to provide a modified calcium carbonate that can effectively improve the stretching rate of the breathable membrane and prepare a breathable membrane with uniform micropore distribution. Summary of the Invention

[0006] The purpose of the present invention is to overcome the problems existing in the above-mentioned prior art and provide a modified calcium carbonate and a preparation method and application thereof.

[0007] The present invention is achieved through the following technical solutions:

[0008] In a first aspect, the present invention provides a modified calcium carbonate, comprising calcium carbonate and a calcium silicate layer coated on the surface of the calcium carbonate, wherein the surface of the calcium silicate layer is further coated with a fatty acid calcium layer; the mass ratio of the calcium carbonate to the calcium silicate layer and the fatty acid calcium layer is: (35-45): (0.5-1.5): (1.5-2.5).

[0009] The present invention adopts double-layer coating to modify calcium carbonate. First, the surface of the calcium carbonate is coated with a layer of calcium silicate inorganic substance. The inorganic substance is a needle-shaped substance that forms a support on the surface of the calcium carbonate to prevent the calcium carbonate from agglomerating. Then, a layer of fatty acid calcium is coated on the outermost layer. Under the effect of this double-layer coating treatment, the surface of the calcium carbonate can be well and completely coated to prevent the agglomeration of the calcium carbonate. The prepared calcium carbonate has good dispersibility and the speed of preparing the breathable film can reach 200 mm / min.

[0010] Preferably, the modified calcium carbonate has a D50 of 3.5 μm-5.5 μm, a D98 of ≤12 μm, and a moisture content of ≤0.1%.

[0011] Preferably, the calcium silicate layer is obtained by the reaction of silicate ions and calcium ions, and the fatty acid calcium layer is obtained by the reaction of fatty acid ions and calcium ions.

[0012] Preferably, the mass ratio of the calcium carbonate to the calcium silicate layer and the fatty acid calcium layer is 42:1:2.

[0013] Preferably, the fatty acid calcium includes at least one of calcium palmitate, calcium stearate, calcium erucate, and calcium oleate, more preferably calcium stearate.

[0014] Preferably, the modified calcium carbonate comprises the following raw materials by mass: 100-200 parts of calcium carbonate, 200-400 parts of water, 5%-10% of the mass of the calcium carbonate silicate solution, 20%-40% of the mass of the calcium carbonate calcium ion solution, and 10%-20% of the mass of the calcium carbonate fatty acid salt solution.

[0015] Preferably, the silicate includes sodium silicate, the calcium ion solution includes at least one of calcium hydroxide solution and calcium chloride solution, the fatty acid salt is a soluble fatty acid salt, and the soluble fatty acid salt includes at least one of palmitate, stearate, erucate, and oleate.

[0016] Preferably, the fatty acid salt is stearate.

[0017] Preferably, the calcium carbonate is heavy calcium carbonate with a particle size D50 of 3 μm-5 μm and D98 ≤ 13 μm.

[0018] Preferably, the water is deionized water or purified water.

[0019] Preferably, the solvent of the silicate solution, calcium ion solution and fatty acid salt solution is water, that is, the silicate solution, calcium ion solution and fatty acid salt solution are silicate aqueous solution, calcium ion aqueous solution and fatty acid salt aqueous solution.

[0020] Preferably, the mass ratio of silicate to solvent in the silicate solution is 1:(1-2).

[0021] Preferably, the mass ratio of the compound containing calcium ions to the solvent in the calcium ion solution is 1:(3-5).

[0022] Preferably, the mass ratio of the fatty acid salt to the solvent in the fatty acid salt solution is 1:(1-2).

[0023] In a second aspect, the present invention provides a method for preparing the modified calcium carbonate, comprising the following steps: uniformly mixing water, calcium carbonate, and a silicate solution, adding a calcium ion solution, reacting, then adding a fatty acid salt solution to continue the reaction, and drying the solid to obtain the modified calcium carbonate.

[0024] The preparation method of the modified calcium carbonate of the present invention is simple. Silicate ions and calcium ions first react on the surface of the calcium carbonate to coat a layer of calcium silicate. The remaining calcium ions then react with fatty acid ions to obtain an outermost fatty acid calcium coating layer, thereby achieving double-layer coating modification of the calcium carbonate. The preparation method of the present invention is simple and suitable for industrial production.

[0025] Preferably, the temperature during the reaction and the continued reaction is 70° C.-80° C., and the time is 1 h-2 h.

[0026] Preferably, the calcium ion solution is added within 30 minutes to 1 hour; and the fatty acid salt solution is added within 30 minutes to 1 hour.

[0027] Preferably, the moisture content during the drying is controlled at ≤0.1%.

[0028] In a third aspect, the present invention provides the use of the modified calcium carbonate and the modified calcium carbonate prepared by the preparation method of the modified calcium carbonate in breathable membranes.

[0029] The breathable film prepared by mixing the modified calcium carbonate of the present invention with polyethylene can effectively improve the stretching rate during preparation, and the prepared breathable film has the advantages of uniform micropore distribution, good mechanical properties and high air permeability.

[0030] The present invention has the following beneficial effects:

[0031] The present invention aims to solve the problems of rib patterns, uneven thickness, perforation and film breakage in the prior art during the preparation of breathable films when the stretching rate exceeds 160 mm / min.

[0032] The activation degree of the coated calcium carbonate is ≥95%, and the moisture content is ≤0.1%.

[0033] The present invention aims to solve the problems in the prior art of preparing breathable membranes, such as rib patterns, uneven thickness, perforations, and film breakage, when the stretching rate exceeds 160 mm / min. The invention provides a double-layer coated modified calcium carbonate, which can effectively improve the dispersibility of calcium carbonate and prevent calcium carbonate agglomeration. The micropores of the prepared breathable membrane are evenly distributed, and the stretching rate during the preparation of the breathable membrane can be effectively increased. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a thermogravimetric analysis diagram of the modified calcium carbonate of Example 2;

[0035] Figure 2 This is the thermogravimetric analysis diagram of commercially available calcium carbonate;

[0036] Figure 3 This is a SEM image of the breathable membrane made from the modified calcium carbonate of Example 2;

[0037] Figure 4 This is a SEM image of a breathable membrane made from commercially available calcium carbonate;

[0038] Figure 5 This is an optical photograph of a breathable film prepared using the modified calcium carbonate of Example 2 at a stretching speed of 200 mm / min;

[0039] Figure 6 This is an optical photograph of a breathable film made using commercially available calcium carbonate at a stretching speed of 160 mm / min. DETAILED DESCRIPTION

[0040] To better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments. Those skilled in the art should understand that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0041] Unless otherwise specified, the experimental methods used in the examples are conventional methods; the materials, reagents, etc. used are all available from commercial sources unless otherwise specified.

[0042] Example 1

[0043] A modified calcium carbonate comprises calcium carbonate and a calcium silicate layer coated on the surface of the calcium carbonate, wherein the surface of the calcium silicate layer is further coated with a calcium stearate layer; the calcium carbonate is heavy calcium carbonate with a particle size D50 of 3 μm and a particle size D98 of 10 μm; and the mass ratio of the calcium carbonate to the calcium silicate layer and the calcium stearate layer is 42:1:2.

[0044] The modified calcium carbonate includes the following raw materials by mass: 100 parts of calcium carbonate, 200 parts of water, 5 parts of sodium silicate aqueous solution, 20 parts of calcium hydroxide aqueous solution, and 10 parts of sodium stearate aqueous solution; the mass ratio of sodium silicate to water in the sodium silicate aqueous solution is 1:1, the mass ratio of calcium hydroxide to water in the calcium hydroxide aqueous solution is 1:3, and the mass ratio of sodium stearate to water in the sodium stearate aqueous solution is 1:1.

[0045] The preparation method of the modified calcium carbonate comprises the following steps:

[0046] S1. Add water into a stirred tank and add calcium carbonate while stirring at a stirring speed of 200 r / min. At the same time, the stirred tank is heated and the temperature is turned on at 70 ° C.

[0047] S2. After stirring, add sodium silicate aqueous solution while stirring;

[0048] S3. After the temperature is constant for 10 min, an aqueous solution of calcium hydroxide is added and the addition is completed within 30 min;

[0049] S4. After the reaction for 1h, an aqueous solution of sodium stearate was added within 30min;

[0050] S5. After continuing the reaction for 1 hour, the solution in the stirred tank was transported to a filter and the filtered solid was dried, the moisture content was controlled at ≤0.1% and the material was finally pulverized to obtain the modified calcium carbonate; the D50 of the obtained modified calcium carbonate was 3.5 μm and D98 was 9.1 μm.

[0051] Example 2

[0052] A modified calcium carbonate comprises calcium carbonate and a calcium silicate layer coated on the surface of the calcium carbonate, wherein the surface of the calcium silicate layer is further coated with a calcium stearate layer; the calcium carbonate is heavy calcium carbonate with a particle size D50 of 3.5 μm and a particle size D98 of 10 μm; and the mass ratio of the calcium carbonate to the calcium silicate layer and the calcium stearate layer is 42:1:2.

[0053] The modified calcium carbonate comprises the following raw materials by mass: 150 parts of calcium carbonate, 300 parts of water, 7.5 parts of sodium silicate aqueous solution, 30 parts of calcium hydroxide aqueous solution, and 15 parts of sodium stearate aqueous solution; the mass ratio of sodium silicate to water in the sodium silicate aqueous solution is 1:1, the mass ratio of calcium hydroxide to water in the calcium hydroxide aqueous solution is 1:3, and the mass ratio of sodium stearate to water in the sodium stearate aqueous solution is 1:1.

[0054] The preparation method of the modified calcium carbonate in this embodiment is the same as that in Example 1; the D50 of the obtained modified calcium carbonate is 3.8 μm and the D98 is 9 μm.

[0055] Example 3

[0056] A modified calcium carbonate comprises calcium carbonate and a calcium silicate layer coated on the surface of the calcium carbonate, wherein the surface of the calcium silicate layer is further coated with a calcium stearate layer; the calcium carbonate is heavy calcium carbonate with a particle size D50 of 5 μm and a particle size D98 of 13 μm; and the mass ratio of the calcium carbonate to the calcium silicate layer and the calcium stearate layer is 42:1:2.

[0057] The modified calcium carbonate includes the following raw materials by mass: 200 parts of calcium carbonate, 400 parts of water, 10 parts of sodium silicate aqueous solution, 40 parts of calcium hydroxide aqueous solution, and 20 parts of sodium stearate aqueous solution; the mass ratio of sodium silicate to water in the sodium silicate aqueous solution is 1:1, the mass ratio of calcium hydroxide to water in the calcium hydroxide aqueous solution is 1:3, and the mass ratio of sodium stearate to water in the sodium stearate aqueous solution is 1:1.

[0058] The preparation method of the modified calcium carbonate in this embodiment is the same as that in Example 1; the D50 of the obtained modified calcium carbonate is 5.4 μm and the D98 is 12 μm.

[0059] Example 4

[0060] A modified calcium carbonate comprises calcium carbonate and a calcium silicate layer coated on the surface of the calcium carbonate, wherein the surface of the calcium silicate layer is further coated with a calcium palmitate layer; the calcium carbonate is heavy calcium carbonate with a particle size D50 of 3 μm and a particle size D98 of 10 μm; and the mass ratio of the calcium carbonate to the calcium silicate layer and the calcium palmitate layer is 42:1:2.

[0061] The modified calcium carbonate includes the following raw materials by mass: 100 parts of calcium carbonate, 200 parts of water, 5 parts of sodium silicate aqueous solution, 20 parts of calcium hydroxide aqueous solution, and 10 parts of sodium palmitate aqueous solution; the mass ratio of sodium silicate to water in the sodium silicate aqueous solution is 1:1, the mass ratio of calcium hydroxide to water in the calcium hydroxide aqueous solution is 1:3, and the mass ratio of sodium palmitate to water in the sodium palmitate aqueous solution is 1:1.

[0062] The preparation method of the modified calcium carbonate in this embodiment is the same as that in Example 1; the D50 of the obtained modified calcium carbonate is 3.6 μm and the D98 is 9.5 μm.

[0063] Comparative Example 1

[0064] A modified calcium carbonate comprises calcium carbonate and a calcium silicate layer coated on the surface of the calcium carbonate; the calcium carbonate is heavy calcium carbonate with a particle size D50 of 3.5 μm and a D98 of 10 μm; and the mass ratio of the calcium carbonate to the calcium silicate layer is 42:1.

[0065] The modified calcium carbonate includes the following raw materials by mass: 100 parts of calcium carbonate, 200 parts of water, 5 parts of sodium silicate aqueous solution, and 20 parts of calcium hydroxide aqueous solution; the mass ratio of sodium silicate to water in the sodium silicate aqueous solution is 1:1, and the mass ratio of calcium hydroxide to water in the calcium hydroxide aqueous solution is 1:3.

[0066] The preparation method of the modified calcium carbonate comprises the following steps:

[0067] S1. Add water into a stirred tank and add calcium carbonate while stirring at a speed of 200 r / min. At the same time, turn on the stirring tank heating and set the temperature to 70 ° C.

[0068] S2. After stirring, add sodium silicate aqueous solution while stirring;

[0069] S3. After the temperature is constant for 10 min, an aqueous solution of calcium hydroxide is added and the addition is completed within 30 min;

[0070] S4. After the reaction is continued for 1 hour, the solution in the stirred tank is filtered and the filtered solid is dried, the moisture content is controlled to ≤0.1% and the material is discharged. Finally, the material is crushed to obtain the modified calcium carbonate; the D50 of the obtained modified calcium carbonate is 3.6 μm and the D98 is 10 μm.

[0071] Comparative Example 2

[0072] A modified calcium carbonate comprises calcium carbonate and a calcium stearate layer coated on the surface of the calcium carbonate; the calcium carbonate is heavy calcium carbonate with a particle size D50 of 3.5 μm and a D98 of 10 μm; and the mass ratio of the calcium carbonate to the calcium stearate layer is 20.2:1.

[0073] The modified calcium carbonate includes the following raw materials by mass: 100 parts of calcium carbonate, 200 parts of water, 20 parts of calcium hydroxide aqueous solution, and 10 parts of sodium stearate aqueous solution; the mass ratio of calcium hydroxide to water in the calcium hydroxide aqueous solution is 1:1, and the mass ratio of sodium stearate to water in the sodium stearate aqueous solution is 1:1.

[0074] The preparation method of the modified calcium carbonate comprises the following steps:

[0075] S1. Add water into a stirred tank and add calcium carbonate while stirring at a speed of 200 r / min. At the same time, turn on the stirring tank heating and set the temperature to 70 ° C.

[0076] S2. After stirring, add calcium hydroxide aqueous solution while stirring, and add within 30min;

[0077] S3. Then add sodium stearate aqueous solution and add within 30min;

[0078] S4. After continuing the reaction for 1 hour, the solution in the stirred tank was transported to a filter and the filtered solid was dried, the moisture content was controlled at ≤0.1% and the material was finally pulverized to obtain the modified calcium carbonate; the D50 of the obtained modified calcium carbonate was 3.5 μm and D98 was 10 μm.

[0079] Comparative Example 3

[0080] A modified calcium carbonate comprises calcium carbonate and a calcium stearate layer coated on the surface of the calcium carbonate; the surface of the calcium stearate layer is further coated with an aluminate coupling agent; the calcium carbonate is heavy calcium carbonate with a particle size D50 of 3.5 μm and a particle size D98 of 10 μm; and the mass ratio of the calcium carbonate to the calcium stearate layer and the aluminate coupling agent is 50:1:1.

[0081] The modified calcium carbonate comprises the following raw materials by mass: 100 parts of calcium carbonate, 2 parts of aluminate coupling agent, and 2 parts of calcium stearate.

[0082] The preparation method of the modified calcium carbonate comprises the following steps:

[0083] S1. Place calcium carbonate in a high-speed blender and stir for 10 minutes at 150°C;

[0084] S2. Add calcium stearate and stir at high speed for 3 minutes;

[0085] S3. Finally, an aluminate coupling agent was added and stirred at high speed for 3 minutes to obtain the modified calcium carbonate; the D50 of the obtained modified calcium carbonate was 3.6 μm and the D98 was 9.8 μm.

[0086] Comparative Example 4

[0087] A modified calcium carbonate comprises calcium carbonate and a stearic acid layer coated on the surface of the calcium carbonate; the surface of the stearic acid layer is further coated with an aluminate coupling agent; the calcium carbonate is heavy calcium carbonate with a particle size D50 of 3.5 μm and a particle size D98 of 10 μm; and the mass ratio of the calcium carbonate to the stearic acid layer and the aluminate coupling agent is 50:1:1.

[0088] The modified calcium carbonate comprises the following raw materials by mass: 100 parts of calcium carbonate, 2 parts of aluminate coupling agent, and 2 parts of stearic acid.

[0089] The preparation method of the modified calcium carbonate comprises the following steps:

[0090] S1. Place calcium carbonate in a high-speed blender and stir for 10 minutes at 150°C;

[0091] S2. Add stearic acid and stir at high speed for 3 minutes;

[0092] S3. Finally, an aluminate coupling agent was added and stirred at high speed for 3 minutes to obtain the modified calcium carbonate; the D50 of the obtained modified calcium carbonate was 3.6 μm and the D98 was 9.9 μm.

[0093] Comparative Example 5

[0094] A modified calcium carbonate comprises calcium carbonate and a calcium silicate layer coated on the surface of the calcium carbonate, wherein the surface of the calcium silicate layer is further coated with a calcium stearate layer; the calcium carbonate is heavy calcium carbonate with a particle size D50 of 3.5 μm and a particle size D98 of 10 μm; and the mass ratio of the calcium carbonate to the calcium silicate layer and the calcium stearate layer is 14:1:2.1.

[0095] The modified calcium carbonate includes the following raw materials by mass: 300 parts of calcium carbonate, 500 parts of water, 45 parts of sodium silicate aqueous solution, 150 parts of calcium hydroxide aqueous solution, and 90 parts of sodium stearate aqueous solution; the mass ratio of sodium silicate to water in the sodium silicate aqueous solution is 1:1, the mass ratio of calcium hydroxide to water in the calcium hydroxide aqueous solution is 1:3, and the mass ratio of sodium stearate to water in the sodium stearate aqueous solution is 1:1.

[0096] The preparation method of the modified calcium carbonate comprises the following steps:

[0097] S1. Add water into a stirred tank and add calcium carbonate while stirring at a speed of 200 r / min. At the same time, turn on the stirring tank heating and set the temperature to 70 ° C.

[0098] S2. After stirring, add sodium silicate aqueous solution while stirring;

[0099] S3. After the temperature is constant for 10 min, an aqueous solution of calcium hydroxide is added and the addition is completed within 30 min;

[0100] S4. After the reaction for 1h, an aqueous solution of sodium stearate was added within 30min;

[0101] S5. After continuing the reaction for 1 hour, the solution in the stirred tank was transported to a filter and the filtered solid was dried, the moisture content was controlled at ≤0.1% and the material was finally pulverized to obtain the modified calcium carbonate; the D50 of the obtained modified calcium carbonate was 3.8 μm and D98 was 9.5 μm.

[0102] Comparative Example 6

[0103] A modified calcium carbonate comprises calcium carbonate and a calcium silicate layer coated on the surface of the calcium carbonate, wherein the surface of the calcium silicate layer is further coated with an aluminate coupling agent; the calcium carbonate is heavy calcium carbonate with a particle size D50 of 3.5 μm and a particle size D98 of 10 μm; and the mass ratio of the calcium carbonate to the calcium silicate layer and the aluminate coupling agent is 48.8:1.2:1.

[0104] The modified calcium carbonate comprises the following raw materials by mass: 100 parts of calcium carbonate, 200 parts of water, 5 parts of sodium silicate aqueous solution, and 20 parts of calcium hydroxide aqueous solution; the aluminate coupling agent accounts for 2% of the mass of the calcium carbonate crushed in step S4; the mass ratio of sodium silicate to water in the sodium silicate aqueous solution is 1:1, and the mass ratio of calcium hydroxide to water in the calcium hydroxide aqueous solution is 1:3.

[0105] The preparation method of the modified calcium carbonate comprises the following steps:

[0106] S1. Add water into a stirred tank and add calcium carbonate while stirring at a stirring speed of 200 r / min. At the same time, the stirred tank is heated and the temperature is turned on at 70 ° C.

[0107] S2. After stirring, add sodium silicate aqueous solution while stirring;

[0108] S3. After the temperature is constant for 10 min, an aqueous solution of calcium hydroxide is added and the addition is completed within 30 min;

[0109] S4. After the reaction was continued for 1h, the solution in the stirred tank was transported to the filter and the filtered solid was dried, the moisture content was controlled at ≤0.1% and the material was finally crushed;

[0110] S5. The crushed calcium carbonate was placed in a high-speed stirrer and stirred for 10 minutes at a temperature of 150°C, and then an aluminate coupling agent was added and stirred at high speed for 3 minutes to obtain the modified calcium carbonate; the D50 of the modified calcium carbonate obtained was 3.7μm and D98 was 10μm.

[0111] Performance testing:

[0112] The modified calcium carbonate of the embodiment and comparative example and commercially available calcium carbonate (Omya 757) were tested for moisture and activation. The calcium carbonate samples were dried before the moisture test. When the sample moisture was ≤0.1%, the sample was cooled to room temperature, taken out, and exposed to air for 48 hours before the moisture test. The test standard was GB / T19281-2014. The test results are shown in Table 1 below.

[0113] Table 1 Test results of moisture and activation of modified calcium carbonate and commercially available calcium carbonate in the examples and comparative examples

[0114]

[0115] As can be seen from Table 1, the modified calcium carbonate of the present invention covers the calcium carbonate more completely and does not absorb moisture. At the same time, the modified calcium carbonate of the present invention has a high degree of activation. The modified calcium carbonate of Example 2 and commercially available calcium carbonate were further subjected to thermogravimetric analysis. The thermogravimetric analysis graph of the modified calcium carbonate of Example 2 is shown in FIG. Figure 1 As shown, the thermogravimetric analysis of commercial calcium carbonate is as follows Figure 2 As shown, compared Figure 1 and Figure 2 It can be seen that the thermal decomposition temperature peak of the modified calcium carbonate of the present invention is high, indicating that the present invention can improve the dispersibility of calcium carbonate through the chemical double-layer coating treatment, which helps to improve the heat resistance.

[0116] The modified calcium carbonate of the embodiment and comparative example and commercially available calcium carbonate were placed in a polyolefin composite material to prepare a breathable membrane. The breathable membrane was prepared using an offline double-drawing device. The specific process is shown in Table 2. The composition formula of the breathable membrane is shown in Table 3. The test results of the prepared breathable membrane are shown in Table 4. The tensile performance test, air permeability test, and dispersibility test were all tested on breathable membranes prepared at a longitudinal stretching rate of 120 mm / min.

[0117] Table 2 Breathable membrane preparation process

[0118]

[0119] Table 3 Preparation formula

[0120] raw material polyethylene calcium carbonate Erucamide Antioxidant 1010 Antioxidant 168 Proportion(%) 49.2 50 0.3 0.2 0.3

[0121] Table 4 Comparison of breathable membrane performance

[0122]

[0123]

[0124] Figure 3 This is a SEM image of the breathable membrane made from the modified calcium carbonate of Example 2. Figure 4 This is a SEM image of a breathable membrane made of commercially available calcium carbonate. Figure 5 This is an optical photograph of a breathable film prepared using the modified calcium carbonate of Example 2 at a stretching speed of 200 mm / min. Figure 6 This is an optical photograph of a breathable membrane made of commercially available calcium carbonate at a stretching speed of 160 mm / min. Figure 3-Figure 6 As can be seen from the data in Table 4, the breathable membrane prepared using the modified calcium carbonate of the present invention has good dispersion of calcium carbonate, relatively uniform pore distribution, good air permeability, good mechanical properties, and can significantly improve the stretching speed during the processing of the breathable membrane.

[0125] Comparative Examples 1 and 2 use a single coating layer to coat calcium carbonate, which cannot improve the dispersibility of calcium carbonate. Calcium carbonate will still agglomerate, and there will be film breakage or perforation under high-speed stretching. In Comparative Example 3, calcium stearate and aluminate coupling agents are used as coating layers, wherein the amount of aluminate coupling agent added is at a conventional level (2% of the mass of calcium carbonate). The use of the two for coating modification cannot effectively improve the dispersibility and stretching speed of calcium carbonate. In Comparative Example 4, stearic acid and aluminate coupling agents are used as coating layers, and the amount of both added is at a conventional level (2% of the mass of calcium carbonate). Calcium carbonate cannot be effectively modified, and perforation and film breakage will occur under high-speed stretching. In Comparative Example 5, the amount of calcium silicate layer and calcium stearate layer is too much, resulting in a significant decrease in the overall performance of the breathable membrane. In Comparative Example 6, aluminate coupling agent is used as the outermost coating layer, which still cannot effectively improve the stretching speed of the breathable membrane, and perforation and film breakage problems occur at 160 mm / min.

[0126] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the essence and scope of the technical solutions of the present invention.

Claims

1. A modified calcium carbonate, It is characterized in that It comprises calcium carbonate and a calcium silicate layer coated on the surface of the calcium carbonate, wherein the surface of the calcium silicate layer is further coated with a fatty acid calcium layer; the mass ratio of the calcium carbonate to the calcium silicate layer and the fatty acid calcium layer is: (35-45): (0.5-1.5): (1.5-2.5).

2. The modified calcium carbonate according to claim 1, It is characterized in that The calcium silicate layer is obtained by the reaction of silicate ions and calcium ions, and the fatty acid calcium layer is obtained by the reaction of fatty acid ions and calcium ions.

3. The modified calcium carbonate according to claim 1, It is characterized in that The fatty acid calcium includes at least one of calcium palmitate, calcium stearate, calcium erucate and calcium oleate.

4. The modified calcium carbonate according to claim 1, It is characterized in that The modified calcium carbonate comprises the following raw materials by mass: 100-200 parts of calcium carbonate, 200-400 parts of water, 5%-10% of silicate solution by mass of the calcium carbonate, 20%-40% of calcium ion solution by mass of the calcium carbonate, and 10%-20% of fatty acid salt solution by mass of the calcium carbonate.

5. The modified calcium carbonate according to claim 4, It is characterized in that The silicate includes sodium silicate, the calcium ion solution includes at least one of a calcium hydroxide solution and a calcium chloride solution, the fatty acid salt is a soluble fatty acid salt, and the soluble fatty acid salt includes at least one of palmitate, stearate, erucate, and oleate.

6. The modified calcium carbonate according to claim 1, It is characterized in that The calcium carbonate is heavy calcium carbonate, with a particle size D50 of 3 μm-5 μm and D98≤13 μm.

7. The modified calcium carbonate according to claim 1, It is characterized in that The mass ratio of silicate to solvent in the silicate solution is 1:(1-2); and / or the mass ratio of the compound containing calcium ions to solvent in the calcium ion solution is 1:(3-5); and / or the mass ratio of fatty acid salt to solvent in the fatty acid salt solution is 1:(1-2).

8. A method for preparing the modified calcium carbonate according to any one of claims 1 to 7, It is characterized in that The following steps are involved: The modified calcium carbonate is obtained by mixing water, calcium carbonate and silicate solution evenly, adding calcium ion solution to react, then adding fatty acid salt solution to continue the reaction, and drying the solid.

9. The method for preparing modified calcium carbonate according to claim 8, It is characterized in that The temperature during the reaction and continued reaction is 70° C.-80° C., and the time is 1 h-2 h.

10. Use of the modified calcium carbonate according to any one of claims 1 to 7 or the modified calcium carbonate prepared by the preparation method of the modified calcium carbonate according to any one of claims 8 to 9 in a breathable film.

Citation Information

Patent Citations

  • Ultrafine surface-treated filler for thin gas-permeable membranes

    CN116438231A

  • Modified heavy calcium carbonate as well as preparation method and application thereof

    CN117777760A