Nanometer sulfur modified silicon carbide and graphene composite rubber and preparation method and application thereof
Through the preparation method of nano-sulfur modified silicon carbide/graphene composite rubber, combined with latex blending and mechanical mixing, the integration problem of thermal conductivity and mechanical properties of rubber materials is solved, large-scale production and performance improvement are achieved, and it is suitable for tires, etc. Applications with high performance requirements.
Patent Information
- Application Number
- CN202411130269.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-10-15
AI Technical Summary
Existing technology is difficult to achieve the integration of thermal conductivity and low energy consumption without sacrificing the mechanical properties of rubber materials. Especially in tire materials, it is difficult to prepare high-performance graphene/rubber composites using traditional mechanical stirring methods.
Using the preparation method of nano-sulfur modified silicon carbide/graphene composite rubber, by first blending latex and combining mechanical mixing with specific parameters, a composite rubber masterbatch with good dispersion and improved performance is prepared.
It achieves large-scale generation of composite rubber with uniform dispersion, excellent mechanical properties and thermal conductivity, breaking the limitations of traditional latex blending methods and mechanical mixing methods, and improving the mechanical properties and thermal conductivity of composite materials.
Smart Images

Figure BDA0004997613880000071 
Figure BDA0004997613880000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rubber, and in particular to nano-sulfur-modified silicon carbide and graphene composite rubber, and a preparation method and application thereof. Background Art
[0002] As the automobile and transportation industries continue to develop in the direction of high speed, high load, green and environmental protection, rubber materials with excellent mechanical properties, thermal conductivity and low energy consumption are urgently needed in application fields such as seals, sensors, and tires, especially tire rubber materials. This material requires good thermal conductivity and low heat accumulation without sacrificing its excellent mechanical properties. However, it is still a challenge for rubber composites to integrate all beneficial properties into rubber materials through a simple and single approach. Raw rubber cannot meet the requirements of practical applications due to its poor strength and elastic properties, so fillers are usually added to meet the requirements of most practical applications. Common fillers include carbon black, silica, clay, silicon carbide (SiC), graphene and other nanoparticles. Compared with other fillers, graphene and its derivatives can give rubber composites excellent thermal conductivity, electrical conductivity, pressure-sensitive response, gas barrier and other properties due to their unique structure and excellent physical and chemical properties. At the same time, the preparation of graphene does not rely on petroleum, so it has been widely studied.
[0003] At present, the graphene / rubber composite materials with good effects are mainly prepared by in-situ polymerization, solution blending and latex mixing, which makes its large-scale production greatly limited by industrial facilities. The traditional mechanical stirring method is more widely used in industry because of its industrial simplicity and cost saving. However, it is often difficult to achieve the desired effect by mechanical mixing using a two-roll mill and a mixer to manufacture graphene / rubber composite materials.
[0004] Therefore, in order to solve the above technical problems, the present invention designs a method for preparing nano-sulfur modified silicon carbide / graphene composite rubber. Summary of the invention
[0005] In order to optimize the existing technology and solve the technical difficulties, the present invention designs a method with simple process, green environmental protection, low cost and excellent performance for preparing nano-sulfur modified silicon carbide / graphene composite rubber masterbatch. The specific technical scheme is as follows.
[0006] The first aspect of the present invention provides a method for preparing a nano-sulfur-modified silicon carbide and graphene composite rubber, the preparation method comprising the following steps:
[0007] S1. Preparation of f-SiC dispersion: dispersing silicon carbide powder in an alkaline solution, adding an amination agent, reacting at 60-100°C for 6-24h, washing and drying to obtain f-SiC particles, and dispersing the f-SiC particles in water to obtain f-SiC dispersion;
[0008] S2. Preparation of SG composite filler: adding carboxyl activator, amidation catalyst, f-SiC dispersion to graphene oxide dispersion, stirring at 100-1000r / min for 1-24h at 20-90°C to obtain a mixed solution, and the mixed solution was vacuum frozen and dried to obtain SG composite filler;
[0009] S3. Preparation of SG-S filler: The SG composite filler was dispersed in water to obtain a SG dispersion, and the sulfur-containing solution and the reducing agent were added and stirred for 2-24h, washed and filtered, and the solid material was vacuum frozen and dried to obtain a SG-S filler;
[0010] S4. Preparation of SG-S / natural latex composite materials: Add SG-S filler to natural latex and add CaCl2 solution for flocculation, filter and wash to obtain SG-S / natural latex masterbatch, further add natural latex and rubber additives and stir and mix for 1-10 hours, and after vulcanization, obtain nano-sulfur modified silicon carbide and graphene composite rubber.
[0011] In some embodiments, the particle size of the silicon carbide powder is 1-5 μm, preferably 3 μm.
[0012] In some embodiments, the alkaline solution includes at least one of an aqueous sodium hydroxide solution, an aqueous potassium hydroxide solution, an aqueous sodium carbonate solution, an aqueous sodium bicarbonate solution, and an aqueous ammonia monohydrate solution.
[0013] Preferably, the alkaline solution is an aqueous sodium hydroxide solution.
[0014] Preferably, the concentration of the alkaline solution is 0.1-2 mol / L.
[0015] Preferably, the concentration of the alkaline solution is 1 mol / L.
[0016] In some embodiments, the amination agent includes at least one of 3-aminopropyltriethoxysilane, ammonia water, ammonium bicarbonate, hydroxylamine, and urea.
[0017] Preferably, the amination agent is 3-aminopropyltriethoxysilane, CAS: 919-30-2.
[0018] In some embodiments, the mass ratio of the silicon carbide powder to the amination reagent is 1:(1-15).
[0019] Preferably, the mass ratio of the silicon carbide powder to the amination reagent is 1:7.
[0020] In some embodiments, the carboxyl activating agent includes at least one of 1-ethyl-(3-dimethylaminopropyl)carbodiimide, carbodiimide, and 2-(7-azabenzotriazole)-N,N,N',N'-tetramethyluronium hexafluorophosphate.
[0021] Preferably, the carboxyl activator is 1-ethyl-(3-dimethylaminopropyl)carbodiimide, CAS: 1892-57-5.
[0022] In some embodiments, the amidation catalyst includes at least one of N-hydroxysuccinimide, triethylamine, and pyridine.
[0023] Preferably, the amidation catalyst is N-hydroxysuccinimide, CAS: 6066-82-6.
[0024] In some embodiments, the graphene oxide dispersion consists of graphene oxide, 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC), and N-hydroxysuccinimide (NHS) in a mass ratio of 1:(0.001-0.1):(0.001-0.1).
[0025] Preferably, the graphene oxide has a purity of 99.9 wt %, a diameter of 0.3-3 μm, a thickness of 0.55-12 nm, a number of layers of 1-5 layers, and amber color, and is purchased from Zhongke Leiming (Beijing) Technology Co., Ltd.
[0026] In some embodiments, the mass ratio of the carboxyl activator, the amidation catalyst, and the graphene oxide is 1:1:(10-1000); the mass ratio of the f-SiC particles in the f-SiC dispersion to the graphene oxide is 1:(1-16).
[0027] Preferably, the mass ratio of f-SiC particles to graphene oxide in the f-SiC dispersion is 1:4.
[0028] In some embodiments, the sulfur-containing solution includes at least one of a Na2S2O3 solution, a CaS2O3 solution, a (NH4)2S2O3 solution, and a K2S2O3 solution.
[0029] Preferably, the sulfur-containing solution is a Na2S2O3 aqueous solution with a concentration of 0.625 mmol / mL.
[0030] In some embodiments, the reducing agent includes at least one of hydrochloric acid, sodium borohydride, hydrazine hydrate, hydrogen peroxide, and potassium permanganate.
[0031] Preferably, the reducing agent is hydrochloric acid with a mass concentration of 30wt%.
[0032] In some embodiments, the mass ratio of the SG composite filler, the sulfur-containing solution, and the reducing agent is (1-10): (1-10): (1-10).
[0033] Preferably, the mass ratio of the SG composite filler, the sulfur-containing solution and the reducing agent is 2:1:2.
[0034] In some embodiments, the addition amount of SG-S filler is 1-10 phr, preferably 4 phr.
[0035] The phr represents the number of parts added per 100 parts (by weight) of natural latex; that is, the number of grams of SG-S filler added per 100 grams of natural latex.
[0036] Furthermore, the mass ratio of the solid content in the natural latex and the CaCl2 solution is 1:1-5, preferably 1:1.
[0037] Furthermore, the natural latex is a 60wt% aqueous solution of natural latex; and the CaCl2 is a 10wt% aqueous solution of calcium chloride.
[0038] In some embodiments, the rubber additive includes at least one of zinc oxide, stearic acid, N-tert-butylbenzothiazole-2-sulfenamide, poly(1,2-dihydro-2,2,4-trimethylquinoline), 1,4-phenylenediamine, N-(1-(methylethyl)-N'-phenyl) and insoluble sulfur.
[0039] In some embodiments, the rubber additives are added in an amount of: 1-10 phr zinc oxide, 1-10 phr stearic acid, 1-10 phr N-tert-butylbenzothiazole-2-sulfonamide, 0.5-1.5 phr poly (1,2-dihydro-2,2,4-trimethylquinoline), 1-10 phr 1,4-phenylenediamine, 1-10 phr N-(1-(methylethyl)-N'-phenyl).
[0040] Preferably, the rubber additives are added in the following amounts: 5 phr zinc oxide, 2 phr stearic acid, 2 phr N-tert-butylbenzothiazole-2-sulfonamide, 1 phr poly(1,2-dihydro-2,2,4-trimethylquinoline), 1 phr 1,4-phenylenediamine, and 1 phr N-(1-(methylethyl)-N'-phenyl).
[0041] The second aspect of the present invention provides a nano-sulfur modified silicon carbide and graphene composite rubber obtained by the above-mentioned preparation method.
[0042] The third aspect of the present invention provides an application of nano-sulfur modified silicon carbide and graphene composite rubber in the preparation of automotive parts.
[0043] Compared with the prior art, the present invention has the following beneficial effects:
[0044] 1. Compared with the prior art, in the preparation method of the nano-sulfur modified silicon carbide / graphene composite rubber of the present invention, the method of preparing the masterbatch by latex blending and then mechanically mixing is innovatively used to prepare the composite rubber, so that the product not only has the good dispersibility and performance improvement brought by the latex blending method, but also has the possibility of large-scale generation by the mechanical mixing method. Therefore, the present invention uses an innovative process to achieve the purpose of large-scale generation, and the composite rubber prepared at the same time is uniformly dispersed and has good mechanical properties. This method breaks the shortcomings of traditional rubber production, that the latex blending method has superior performance but is difficult to mass produce, and the mechanical mixing method is simple to mass produce, but has poor performance.
[0045] 2. In the present invention, by combining silicon carbide with graphene of specific parameters, the structural degree of filler is increased, thereby improving the dispersibility of composite filler in natural rubber latex. Further, silicon carbide and graphene can produce coordination effect, significantly improving the mechanical properties of natural rubber latex. Through nano-sulfur modification, composite filler can be involved in the vulcanization process of natural rubber latex, and composite filler is evenly dispersed in the cross-linked network of natural rubber latex while improving the cross-linking degree of natural rubber latex, thereby effectively playing the role of composite filler in improving the mechanical properties of natural rubber latex.
[0046] 3. In the present invention, GO and SiC are compounded by amidation reaction to prepare SG filler with high structure and high thermal conductivity. Sulfur is further grown on the SG surface by chemical deposition and π-π interaction to prepare SG-S particles with both reinforcement and vulcanization functions. The covalent bond between GO and SiC weakens the interfacial thermal resistance between the fillers and promotes the effective transmission of phonons. The highly structured filler increases the probability of contact and entanglement with the rubber molecular chain, anchoring the NR molecular chain more firmly on the SG surface, thereby enhancing the interfacial interaction between the filler and the rubber molecular chain. In addition, this allows the SG-S particles to be more evenly dispersed in the rubber composite material. The abundant sulfur on the surface of the evenly dispersed SG-S particles also effectively promotes the scope of action of the vulcanizer, making the cross-linking network in the rubber composite material richer. At low filler dosage, this unique filler-rubber interface structure gives the composite rubber better mechanical properties. DETAILED DESCRIPTION
[0047] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0048] The natural latex in the present invention is purchased from Shandong Xinzexiang Chemical Co., Ltd., THR natural latex, with a solid content of 60%.
[0049] Example 1
[0050] This embodiment provides a nano-sulfur-modified silicon carbide and graphene composite rubber, and the preparation method includes the following steps:
[0051] S1. Preparation of f-SiC dispersion: dispersing silicon carbide powder in a 5 mol / L alkaline solution and soaking for 30 min, adding an amination agent, reacting at 70°C for 8 h, washing and drying to obtain f-SiC particles, and dispersing the f-SiC particles in water to obtain a f-SiC dispersion;
[0052] The particle size of the silicon carbide powder is 3 μm; the alkaline solution is a sodium hydroxide aqueous solution with a concentration of 1 mol / L; the amination reagent is 3-aminopropyltriethoxysilane; and the mass ratio of the silicon carbide powder to the amination reagent is 1:7.
[0053] S2. Preparation of SG composite filler: adding carboxyl activator, amidation catalyst, f-SiC dispersion to graphene oxide dispersion, stirring at 200 r / min for 1 h at 40°C to obtain a mixed solution, and vacuum freezing and drying the mixed solution to obtain SG composite filler;
[0054] The carboxyl activator is 1-ethyl-(3-dimethylaminopropyl)carbodiimide; the amidation catalyst is N-hydroxysuccinimide; the graphene oxide dispersion is composed of graphene oxide, EDC, and NHS in a mass ratio of 1:0.05:0.05; the graphene oxide has a purity of 99.9wt%, a diameter of 0.3-3μm, a thickness of 0.55-12nm, a number of layers of 1-5 layers, and a color of amber, and is purchased from Zhongke Leiming (Beijing) Technology Co., Ltd.; the mass ratio of the carboxyl activator, the amidation catalyst, and the graphene oxide is 1:0.01:0.01; the mass ratio of f-SiC particles and graphene oxide in the f-SiC dispersion is 1:4.
[0055] S3. Preparation of SG-S filler: The SG composite filler was dispersed in water to obtain a SG dispersion, and the sulfur-containing solution and the reducing agent were added and stirred for 2 h, washed and filtered, and the solid material was vacuum frozen and dried to obtain a SG-S filler;
[0056] The sulfur-containing solution is a 0.625 mmol / mL Na2S2O3 aqueous solution; the reducing agent is hydrochloric acid with a mass concentration of 30 wt%; the mass ratio of the SG composite filler, the sulfur-containing solution, and the reducing agent is 2:1:2.
[0057] S4. Preparation of SG-S / natural latex composite materials: Add SG-S filler to natural latex (the mass ratio of the two is 1:1) and add CaCl2 solution for flocculation, filter and wash to obtain SG-S / natural latex masterbatch, further add natural latex and rubber additives and stir and mix for 5 hours, and after vulcanization, nano-sulfur modified silicon carbide and graphene composite rubber is obtained.
[0058] The amount of the SG-S filler added is 4 phr; the mass ratio of the solid content in the natural rubber latex and the CaCl2 solution is 1:1; the rubber additives and their addition amounts are: 5 phr zinc oxide, 2 phr stearic acid, 2 phr N-tert-butylbenzothiazole-2-sulfonamide, 1 phr poly (1,2-dihydro-2,2,4-trimethylquinoline), 1 phr 1,4-phenylenediamine, and 1 phr N-(1-(methylethyl)-N'-phenyl).
[0059] Comparative Example 1
[0060] The specific implementation of this comparative example is the same as that of Example 1, except that the graphene oxide dispersion consists of graphene oxide, carbodiimide and triethylamine in a mass ratio of 1:0.1:0.1.
[0061] Comparative Example 2
[0062] The specific implementation of this comparative example is the same as that of Example 1, except that the sulfur-containing solution is a CaS2O3 solution; and the reducing agent is hydrogen peroxide with a mass concentration of 1 mol / L.
[0063] Comparative Example 3
[0064] The specific implementation manner of this comparative example is the same as that of Example 1, except that the amination reagent is an aqueous solution of ammonium bicarbonate with a concentration of 1 mol / L; the graphene oxide dispersion is composed of graphene oxide, 2-(7-azabenzotriazole)-N,N,N',N'-tetramethyluronium hexafluorophosphate (HATU) and pyridine in a mass ratio of 1:0.1:0.1.
[0065] Comparative Example 4
[0066] The specific implementation of this comparative example is the same as that of Example 1, except that the nano-sulfur modification in step S3 is not performed, and the SG composite filler is directly added to the natural rubber latex in step S4.
[0067] Comparative Example 5
[0068] The specific implementation of this comparative example is the same as that of Example 1, except that the preparation method comprises the following steps:
[0069] Silicon carbide is added to natural latex and CaCl2 solution is added for flocculation, filtered and washed to obtain silicon carbide / natural latex masterbatch, natural latex and rubber additives are further added and stirred for 5 hours, and silicon carbide composite rubber is obtained after vulcanization.
[0070] The particle size of the silicon carbide powder is 3 μm.
[0071] Comparative Example 6
[0072] The specific implementation of this comparative example is the same as that of Example 1, except that the preparation method comprises the following steps:
[0073] Graphene oxide is added to natural latex and CaCl2 solution is added for flocculation, and the graphene oxide / natural latex masterbatch is obtained by filtration and washing. Natural latex and rubber additives are further added and stirred for 5 hours, and the graphene oxide composite rubber is obtained after vulcanization.
[0074] The graphene oxide has a purity of 99.9 wt %, a diameter of 0.3-3 μm, a thickness of 0.55-12 nm, a number of layers of 1-5 layers, and a color of amber. The manufacturer is Zhongke Leiming (Beijing) Technology Co., Ltd.
[0075] Performance Testing
[0076] The composite rubbers prepared in the above examples and comparative examples were subjected to the following tests, and the experimental results are recorded in Table 1.
[0077] The control group is pure natural latex, which is obtained by mixing natural latex and rubber additives for 5 hours and then vulcanizing. The type and addition amount of the rubber additives are the same as those in Example 1.
[0078] Thermal conductivity: Refer to MIL-I-49456A.
[0079] Energy loss Tanδ: refer to GB / T 1687-93.
[0080] Tensile strength: refer to GB / T 1688-2008.
[0081] Elongation at break: Refer to GB / T 13934-2006.
[0082] Tear strength: refer to GB / T 529-2008.
[0083] Hardness: Refer to GB / T 6031-1998.
[0084] Wear rate: refer to GB / T 9867-2008.
[0085] Table 1
[0086]
[0087]
[0088] From the above data analysis, it can be seen that compared with pure natural latex, the thermal conductivity of the nano-sulfur modified silicon carbide / graphene composite rubber prepared in Example 1 reached 0.377W / mK, an increase of 149.7%, and the energy loss Tanδ was also reduced from 23.2 to 4.4, which greatly reduced the service life loss of the composite rubber due to self-heating during use. Compared with Example 1, the composite rubber prepared in Comparative Examples 1-6 has various properties that have decreased to varying degrees due to the change of the technical scheme defined in the present invention, but compared with natural latex, the tensile strength, elongation at break, tear strength, and hardness of the composite rubber prepared in Comparative Examples 1-10 are still significantly improved, so that the nano-sulfur modified silicon carbide / graphene composite rubber can be more widely used in many scenarios.
[0089] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a nano-sulfur-modified silicon carbide and graphene composite rubber, characterized in that: The preparation method comprises the following steps: S1. Preparation of f-SiC dispersion: dispersing silicon carbide powder in an alkaline solution, adding an amination agent, reacting at 60-100°C for 6-24h, washing and drying to obtain f-SiC particles, and dispersing the f-SiC particles in water to obtain f-SiC dispersion; S2. Preparation of SG composite filler: adding carboxyl activator, amidation catalyst, f-SiC dispersion to graphene oxide dispersion, stirring at 100-1000r / min for 1-24h at 20-90°C to obtain a mixed solution, and the mixed solution was vacuum frozen and dried to obtain SG composite filler; S3. Preparation of SG-S filler: The SG composite filler was dispersed in water to obtain a SG dispersion, and the sulfur-containing solution and the reducing agent were added and stirred for 2-24h, washed and filtered, and the solid material was vacuum frozen and dried to obtain a SG-S filler; S4. Preparation of SG-S / natural latex composite materials: Add SG-S filler to natural latex and add CaCl2 solution for flocculation, filter and wash to obtain SG-S / natural latex masterbatch, further add natural latex and rubber additives and stir and mix for 1-10 hours, and after vulcanization, obtain nano-sulfur modified silicon carbide and graphene composite rubber.
2. The preparation method according to claim 1, characterized in that: The amination agent includes at least one of 3-aminopropyltriethoxysilane, ammonia water, ammonium bicarbonate, hydroxylamine and urea.
3. The preparation method according to claim 2, characterized in that: The mass ratio of the silicon carbide powder to the amination reagent is 1:(1-15).
4. The preparation method according to claim 3, characterized in that: The carboxyl activator includes at least one of 1-ethyl-(3-dimethylaminopropyl)carbodiimide, carbodiimide, and 2-(7-azabenzotriazole)-N,N,N',N'-tetramethyluronium hexafluorophosphate.
5. The preparation method according to claim 4, characterized in that: The graphene oxide dispersion consists of graphene oxide, EDC and NHS in a mass ratio of 1:(0.001-0.1):(0.001-0.1).
6. The preparation method according to claim 5, characterized in that: The mass ratio of the carboxyl activator, the amidation catalyst and the graphene oxide is 1:1:(10-1000); the mass ratio of the f-SiC particles and the graphene oxide in the f-SiC dispersion is 1:(1-16).
7. The preparation method according to claim 6, characterized in that: The amidation catalyst includes at least one of N-hydroxysuccinimide, triethylamine and pyridine.
8. The preparation method according to claim 7, characterized in that: The sulfur-containing solution includes at least one of a Na2S2O3 solution, a CaS2O3 solution, a (NH4)2S2O3 solution, and a K2S2O3 solution.
9. A nano-sulfur modified silicon carbide and graphene composite rubber, characterized in that: Obtained by the preparation method according to any one of claims 1 to 8.
10. Application of nano-sulfur modified silicon carbide and graphene composite rubber in the preparation of automotive parts.
Citation Information
Cited By
Flame-retardant silicon carbide ceramic rubber material and preparation method thereof
CN119552514A