A high temperature resistant polyester adhesive for flexible printed circuit board and preparation method thereof
By modifying the polyester adhesive with naphthalene ring multifunctional epoxy prepolymer of the flexible printed circuit board, the problem of insufficient heat resistance at high temperatures is solved, the welding and fire drop performance is improved, and more stable adhesive layer.
Patent Information
- Application Number
- CN202411246439.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-06
AI Technical Summary
The polyester adhesive of flexible printed circuit boards lacks heat resistance and welding performance at high temperatures, making it difficult to meet the requirements during the circuit board welding process.
The polyfunctional epoxy prepolymer is formed by pretreating the monomer with naphthalene rings, and the polyester resin is modified using the prepolymer to introduce a rigid ring structure to improve the temperature resistance of the adhesive. The specific method includes the use of neopentyl glycol, hyperbranched epoxy naphthalene ring prepolymer, 1,6-hexanediol, isophthalic acid, trimellitic anhydride, catalyst and antioxidant, etc., to synthesize high-temperature resistant poly through specific process steps. Ester adhesive.
It significantly improves the soldering resistance and fire-dripping performance of polyester adhesives, reduces color aging at high temperatures, and enhances its stability and heat resistance during circuit board welding.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesive resin synthesis, and in particular to a high temperature resistant polyester adhesive for a flexible printed circuit board and a preparation method thereof. Background Art
[0002] Flexible printed circuit (FPC) has become the fastest growing product in the printed circuit industry due to its lightness, thinness, small size, flexibility and three-dimensional wiring. With the rapid development of the electrical and electronic industries, there are more and more requirements for miniaturization, lightweight, high reliability and simplified assembly process of instruments and equipment. The flexible printed circuit substrate is made of insulating plastic film and copper foil bonded with adhesive. There are generally two types of insulating plastic films, polyimide (PI) and polyester (PET) films. Among them, polyester copper clad laminate (CCL) has been increasingly widely used due to its excellent performance and low price, especially in automotive instruments, household appliances, audio-visual equipment, high-end toys, computers and auxiliary equipment. It has currently occupied more than 30% of the FPC substrate market.
[0003] FPC adhesives are required to have good insulation, adhesion, chemical resistance, heat resistance, etc., and can be used as adhesives for flexible printed circuit boards. The main varieties include polyester, polyurethane, epoxy, phenolic, polyimide, etc. Among them, polyester has good electrical properties and chemical resistance, and the lowest cost, but it has the disadvantage of poor heat resistance. At the same time, it has some shortcomings in welding resistance and fire-resistant dripping performance during circuit board welding. It is necessary to add epoxy resin, melamine resin and other resins with good temperature resistance to modify it. In addition, phenol, naphthalene, etc. are also often used to improve the heat resistance of resins. In patent 202410544445.X, phenol, naphthol, formaldehyde solution and catalyst are mixed to carry out condensation polymerization reaction to obtain naphthol aldehyde oligomers to modify bismaleimide resin. Summary of the invention
[0004] To this end, the technical problem to be solved by the present invention is to provide a high-temperature resistant polyester adhesive for flexible printed circuit boards and a preparation method thereof, by pretreating a monomer with a naphthalene ring to form a multifunctional epoxy prepolymer with a naphthalene ring, and using the multifunctional epoxy prepolymer with a naphthalene ring to modify a polyester resin, thereby utilizing a rigid cyclic structure to improve the temperature resistance of the polyester adhesive.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A high temperature resistant polyester adhesive for a flexible printed circuit board comprises the following components: 100 parts by weight of neopentyl glycol, 10 to 50 parts by weight of a hyperbranched epoxy naphthalene ring prepolymer, 20 to 40 parts by weight of 1,6-hexanediol, 120 parts by weight of isophthalic acid, 2 to 5 parts by weight of trimellitic anhydride, 0.3 parts by weight of catalyst A, 0.3 parts by weight of antioxidant 1010 and 200 parts by weight of a solvent, wherein the molar ratio of hydroxyl to carboxyl in the raw materials is 1.05 to 0.95 / 1; wherein the hyperbranched epoxy naphthalene ring prepolymer is prepared from 100 parts by weight of a naphthalene compound, 5 to 10 parts by weight of maleic anhydride, 20 to 60 parts by weight of a modified monomer, 1 to 3 parts by weight of a catalyst B and 100 to 200 parts by weight of toluene through the following steps:
[0007] (1) Add naphthalene compound, maleic anhydride and toluene into a reaction kettle, stir and heat to 80°C to melt, add catalyst B and react for 2 to 4 hours;
[0008] (2) Slowly add the modified monomer to the reaction kettle dropwise for 0.5 to 1 hour, raise the temperature to 100°C and keep the temperature for 2 to 4 hours;
[0009] (3) Add activated carbon for decolorization, and use a thin film evaporator to remove toluene in vacuo to obtain a hyperbranched naphthalene oxide ring prepolymer.
[0010] In the high temperature resistant polyester adhesive for flexible printed circuit boards, the naphthalene compound is one or more of 2-naphthol, 2-naphthoic acid, naphthalenediol and naphthalenediamine.
[0011] In the above-mentioned high temperature resistant polyester adhesive for flexible printed circuit boards, the modified monomer is one of resorcinol diglycidyl ether, bisphenol A diglycidyl ether, hexahydrophthalic acid diglycidyl ether and tetrahydrophthalic acid diglycidyl ether.
[0012] In the above-mentioned high temperature resistant polyester adhesive for flexible printed circuit boards, the catalyst B is one of benzyltriethylammonium chloride, tetrabutylammonium bromide and tetrabutylammonium chloride.
[0013] In the above-mentioned high temperature resistant polyester adhesive for flexible printed circuit boards, the catalyst A is one of organic tin, organic bismuth and organic zinc.
[0014] The solvent of the high temperature resistant polyester adhesive for flexible printed circuit boards is one or more of No. 150 solvent oil, No. 200 solvent oil, xylene and trimethylbenzene.
[0015] The high temperature resistant polyester adhesive for flexible printed circuit boards is composed of the following components: 100 parts by weight of neopentyl glycol, 30 parts by weight of hyperbranched epoxy naphthalene ring prepolymer, 20 parts by weight of 1,6-hexanediol, 120 parts by weight of isophthalic acid, 2 parts by weight of trimellitic anhydride, 0.3 parts by weight of catalyst A, 0.3 parts by weight of antioxidant 1010 and 200 parts by weight of solvent No. 150 solvent oil.
[0016] The high temperature resistant polyester adhesive for flexible printed circuit boards comprises 100 parts by weight of neopentyl glycol, 50 parts by weight of hyperbranched epoxy naphthalene ring prepolymer, 20 parts by weight of 1,6-hexanediol, 120 parts by weight of isophthalic acid, 2 parts by weight of trimellitic anhydride, 0.3 parts by weight of catalyst A, 0.3 parts by weight of antioxidant 1010 and 200 parts by weight of solvent No. 150 solvent oil.
[0017] The above-mentioned high temperature resistant polyester adhesive for flexible printed circuit boards, the hyperbranched epoxy naphthalene ring prepolymer is prepared from 100 parts by weight of naphthalene compounds, 5 parts by weight of maleic anhydride, 60 parts by weight of modified monomer resorcinol diglycidyl ether, 1 part by weight of catalyst B benzyltriethylammonium chloride and 100 parts by weight of solvent toluene.
[0018] A method for preparing the above-mentioned high temperature resistant polyester adhesive for flexible printed circuit boards comprises the following steps:
[0019] (I) Add neopentyl glycol, 1,6-hexanediol, isophthalic acid and trimellitic anhydride into a reaction kettle, then add catalyst A and antioxidant 1010, start heating and stirring;
[0020] (II) Heating to 240°C, dehydrating and keeping warm for 8-10 hours, until the material becomes transparent, and the acid value is 30-50 mgKOH / g;
[0021] (III) adding 100 to 150 parts by weight of solvent to dilute and cooling to 120° C., and then adding hyperbranched naphthalene oxide prepolymer to react for 2 to 4 hours until the test acid value reaches 5 to 10 mgKOH / g;
[0022] (IV) Add the remaining solvent to dilute the mixture, cool it down and filter out the material.
[0023] The technical solution of the present invention achieves the following beneficial technical effects:
[0024] The active groups of conventional naphthalene compounds are generally hydroxyl groups, and the esterification reaction temperature with carboxyl groups is very high, which will result in a very dark color of the polyester product. The present invention synthesizes a multifunctional epoxy prepolymer with a naphthalene ring and introduces it into the main structure of the polyester resin at a relatively low temperature, thereby reducing color aging at high temperatures, and the rigid ring structure improves the temperature resistance of the polyester adhesive, and the multifunctional reactive groups improve the crosslinking degree and molecular weight of the resin, thereby improving the welding resistance and fire-resistant dripping performance of the adhesive layer during the circuit board welding process. DETAILED DESCRIPTION
[0025] Example 1
[0026] In this embodiment, the high temperature resistant polyester adhesive for flexible printed circuit boards is composed of the following components: 100 parts by weight of neopentyl glycol, 10 parts by weight of hyperbranched epoxy naphthalene ring prepolymer, 20 parts by weight of 1,6-hexanediol, 120 parts by weight of isophthalic acid, 2 parts by weight of trimellitic anhydride, 0.3 parts by weight of catalyst A, 0.3 parts by weight of antioxidant 1010 and 200 parts by weight of solvent No. 150 solvent oil. It is synthesized according to the following process:
[0027] (I) Add neopentyl glycol, 1,6-hexanediol, isophthalic acid and trimellitic anhydride into a reaction kettle, then add catalyst A, organotin and antioxidant 1010, start heating and stirring;
[0028] (II) Heating to 240°C, dehydrating and heat-keeping for 8 hours, until the material becomes transparent, and the acid value is 50 mgKOH / g;
[0029] (III) adding 100 parts by weight of solvent to dilute and cooling to 120 degrees, and then adding hyperbranched naphthalene oxide ring prepolymer to react for 2 hours until the test acid value reaches 10 mgKOH / g;
[0030] (IV) Add the remaining solvent to dilute the mixture, cool it down and filter out the material.
[0031] The hyperbranched epoxy naphthalene ring prepolymer is prepared from 100 parts by weight of 2-naphthol, 5 parts by weight of maleic anhydride, 20 parts by weight of modified monomer resorcinol diglycidyl ether, 1 part by weight of catalyst B benzyltriethylammonium chloride, and 100 parts by weight of solvent toluene by the following steps:
[0032] (1) Add 2-naphthol, maleic anhydride and solvent into a reaction kettle, stir and heat to 80°C to melt, add catalyst B and react for 2 hours;
[0033] (2) Slowly add the modified monomer into the reactor dropwise for 0.5 hours, raise the temperature to 100°C and keep the reaction for 2 hours;
[0034] (3) A small amount of activated carbon is added for decolorization, and the solvent is removed by vacuum using a thin film evaporator to obtain a hyperbranched naphthalene oxide ring prepolymer.
[0035] Example 2
[0036] The high temperature resistant polyester adhesive for flexible printed circuit boards in this embodiment is different from that in Embodiment 1 in that the added amount of the hyperbranched naphthalene oxide ring prepolymer in this embodiment is 30 parts by weight.
[0037] Example 3
[0038] The high temperature resistant polyester adhesive for flexible printed circuit boards in this embodiment is different from that in Embodiment 1 in that the added amount of the hyperbranched naphthalene oxide ring prepolymer in this embodiment is 50 parts by weight.
[0039] Example 4
[0040] The high temperature resistant polyester adhesive for flexible printed circuit boards in this embodiment is different from that in Embodiment 1 in that the amount of trimellitic anhydride added in this embodiment is 3 parts by weight.
[0041] Example 5
[0042] The high temperature resistant polyester adhesive for flexible printed circuit boards in this embodiment is different from that in Embodiment 1 in that the amount of trimellitic anhydride added in this embodiment is 5 parts by weight.
[0043] Example 6
[0044] The high temperature resistant polyester adhesive for flexible printed circuit boards in this embodiment is different from that in Embodiment 1 in that the dehydration and heat preservation reaction time in step (II) in this embodiment is 10 h, and the tested acid value is 30 mgKOH / g.
[0045] Example 7
[0046] The high temperature resistant polyester adhesive for flexible printed circuit boards in this embodiment is different from that in embodiment 1 in that in this embodiment, the hyperbranched naphthalene oxide prepolymer is added in step (III) and reacted for 4 hours until the test acid value reaches 5 mgKOH / g.
[0047] Example 8
[0048] The high temperature resistant polyester adhesive for flexible printed circuit boards in this embodiment is different from that in Embodiment 1 in that the amount of maleic anhydride added during the preparation of the hyperbranched naphthalene oxide prepolymer in this embodiment is 10 parts by weight.
[0049] Example 9
[0050] The high temperature resistant polyester adhesive for flexible printed circuit boards in this embodiment is different from that in Embodiment 1 in that the amount of the modified monomer added during the preparation of the hyperbranched naphthalene oxide ring prepolymer in this embodiment is 40 parts by weight.
[0051] Example 10
[0052] The high temperature resistant polyester adhesive for flexible printed circuit boards in this embodiment is different from that in Embodiment 1 in that the amount of the modified monomer added during the preparation of the hyperbranched naphthalene oxide ring prepolymer in this embodiment is 60 parts by weight.
[0053] Embodiment 11
[0054] The high temperature resistant polyester adhesive for flexible printed circuit boards in this embodiment is different from that in Embodiment 1 in that the modified monomer in the preparation process of the hyperbranched naphthalene oxide ring prepolymer in this embodiment is bisphenol A diglycidyl ether.
[0055] Example 12
[0056] The high temperature resistant polyester adhesive for flexible printed circuit boards in this embodiment is different from that in Embodiment 1 in that in the preparation process of the hyperbranched naphthalene oxide prepolymer in this embodiment, the reaction time after adding the catalyst B in step (1) is 4 hours.
[0057] Embodiment 13
[0058] The high temperature resistant polyester adhesive for flexible printed circuit boards in this embodiment is different from that in embodiment 1 in that in the preparation process of the hyperbranched naphthalene oxide prepolymer in this embodiment, the temperature is raised to 100° C. and kept for 4 hours in step (2).
[0059] Comparative Example 1
[0060] The high temperature resistant polyester adhesive for flexible printed circuit boards in this comparative example is different from that in Example 1 in that no hyperbranched naphthalene oxide ring prepolymer is added during the synthesis of the polyester adhesive.
[0061] Performance Testing
[0062] The polyester adhesives prepared in Examples 1 to 13 and Comparative Example 1 were tested for relevant properties according to the following conditions:
[0063] 1. Solid content is tested by taking 1±0.05g of material in a tin foil box and baking it at 105℃ for 2h;
[0064] 2. Viscosity is measured with a rotational viscometer when the material temperature is controlled at 25°C;
[0065] 3. Peel strength: Coat the polyester adhesive on a 100 μm thick polyester film, control the adhesive thickness to 20 μm, dry it, and compound it with a 35 μm roughened copper foil. Curing it in a hot press at 120°C for 120 minutes, and discharging it after cooling to obtain a polyester copper clad laminate for flexible printed circuits. Test it according to the requirements of GB / T 13556-2017.
[0066] The 4.5% thermal decomposition temperature was tested by TGA from room temperature to 500 °C in a nitrogen atmosphere at a heating rate of 10 °C / min.
[0067] The relevant performance test results of the polyester adhesives prepared in Examples 1 to 13 and Comparative Example 1 are shown in Table 1.
[0068] Table 1 Comparison of resin properties
[0069]
[0070] It can be seen from the data recorded in Table 1 that the addition of the hyperbranched naphthalene oxide ring prepolymer significantly improves the peel strength of the polyester adhesive while keeping the solid content almost unchanged, and improves the peel strength of the polyester adhesive. At the same time, the heat resistance of the polyester adhesive is significantly improved.
[0071] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the claims of this patent application.
Claims
1. A high temperature resistant polyester adhesive for a flexible printed circuit board, characterized in that: The invention comprises the following components: 100 parts by weight of neopentyl glycol, 10 to 50 parts by weight of hyperbranched epoxy naphthalene ring prepolymer, 20 to 40 parts by weight of 1,6-hexanediol, 120 parts by weight of isophthalic acid, 2 to 5 parts by weight of trimellitic anhydride, 0.3 parts by weight of catalyst A, 0.3 parts by weight of antioxidant 1010 and 200 parts by weight of solvent; wherein the hyperbranched epoxy naphthalene ring prepolymer is prepared from 100 parts by weight of 2-naphthol, 5 to 10 parts by weight of maleic anhydride, 20 to 60 parts by weight of modified monomer, 1 to 3 parts by weight of catalyst B and 100 to 200 parts by weight of toluene through the following steps: (1) Add 2-naphthol, maleic anhydride and toluene into a reaction kettle, stir and heat to 80°C to melt, add catalyst B and react for 2 to 4 hours; (2) Slowly add the modified monomer to the reaction kettle dropwise for 0.5 to 1 hour, raise the temperature to 100°C and keep the temperature for 2 to 4 hours; (3) adding activated carbon for decolorization, and removing toluene by vacuum using a thin film evaporator to obtain a hyperbranched naphthalene oxide ring prepolymer; The modified monomer is one of resorcinol diglycidyl ether, bisphenol A diglycidyl ether, hexahydrophthalic acid diglycidyl ether and tetrahydrophthalic acid diglycidyl ether.
2. The high temperature resistant polyester adhesive for flexible printed circuit boards according to claim 1, characterized in that: The catalyst B is one of benzyltriethylammonium chloride, tetrabutylammonium bromide and tetrabutylammonium chloride.
3. The high temperature resistant polyester adhesive for flexible printed circuit boards according to claim 1, characterized in that: The catalyst A is one of organic tin, organic bismuth and organic zinc.
4. The high temperature resistant polyester adhesive for flexible printed circuit boards according to claim 1, characterized in that: The solvent is one or more of No. 150 solvent oil, No. 200 solvent oil, xylene and trimethylbenzene.
5. The high temperature resistant polyester adhesive for flexible printed circuit boards according to claim 1, characterized in that: The invention is composed of the following components: 100 parts by weight of neopentyl glycol, 30 parts by weight of hyperbranched epoxy naphthalene ring prepolymer, 20 parts by weight of 1,6-hexanediol, 120 parts by weight of isophthalic acid, 2 parts by weight of trimellitic anhydride, 0.3 parts by weight of catalyst A, 0.3 parts by weight of antioxidant 1010 and 200 parts by weight of solvent No. 150 solvent oil.
6. The high temperature resistant polyester adhesive for flexible printed circuit boards according to claim 1, characterized in that: 100 parts by weight of neopentyl glycol, 50 parts by weight of hyperbranched epoxy naphthalene ring prepolymer, 20 parts by weight of 1,6-hexanediol, 120 parts by weight of isophthalic acid, 2 parts by weight of trimellitic anhydride, 0.3 parts by weight of catalyst A, 0.3 parts by weight of antioxidant 1010 and 200 parts by weight of solvent No. 150 solvent oil.
7. The high temperature resistant polyester adhesive for flexible printed circuit boards according to claim 1, characterized in that: The hyperbranched epoxy naphthalene ring prepolymer is prepared from 100 parts by weight of a naphthalene compound, 5 parts by weight of maleic anhydride, 60 parts by weight of a modified monomer resorcinol diglycidyl ether, 1 part by weight of a catalyst B benzyltriethylammonium chloride and 100 parts by weight of a solvent toluene.
8. A method for preparing a high temperature resistant polyester adhesive for a flexible printed circuit board according to claim 1, characterized in that: The steps include: (I) Add neopentyl glycol, 1,6-hexanediol, isophthalic acid and trimellitic anhydride into a reaction kettle, then add catalyst A and antioxidant 1010, start heating and stirring; (II) Heating to 240°C, dehydrating and keeping warm for 8-10 hours, until the material becomes transparent and the acid value is 30-50 mgKOH / g; (III) adding 100 to 150 parts by weight of solvent to dilute and cooling to 120° C., and then adding hyperbranched naphthalene oxide prepolymer to react for 2 to 4 hours until the test acid value reaches 5 to 10 mgKOH / g; (IV) Add the remaining solvent to dilute the mixture, cool it down and filter out the material.
Citation Information
Patent Citations
Room-temperature-cured high-temperature-resistant anticorrosive epoxy structural adhesive, and preparation method thereof
CN105440999A
Hot-melt pressure-sensitive adhesive for alkaline dry cell label and preparing method thereof
CN105907352A
Naphthalenediol hyperbranched epoxy resin as well as preparation method and application thereof
CN110078894A
Ultralow-temperature epoxy cured polyester resin and preparation method thereof
CN111423565A
Epoxy resin molding material for sealing electric part
JP1992173829A