MS resin adhesive composition, antistatic protective film, and preparation method and application thereof
Through the use of MS resin adhesive composition, the problems of complex structure and lack of anti-static function in the existing protective film technology are solved, and simple construction and efficient anti-static protection are achieved. It is suitable for aerospace and marine engineering fields and provides a more comprehensive Protective effect.
Patent Information
- Application Number
- CN202411005962.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-15
AI Technical Summary
Existing protective film technology has problems such as complex structure, cumbersome preparation process, lack of anti-static function or complicated procedures for introducing anti-static function. Traditional resin materials also have deficiencies in weather resistance, cost and protective performance.
Use MS resin adhesive composition, including component A and component B, through plasticizer, thixotropic agent, silica-immobilized antistatic agent, ultraviolet light absorber, light stabilizer, MS resin and coupling agent A combination of these materials can be used to prepare an anti-static protective film with simple construction and permanent anti-static function.
A protective film with simple construction, simple structure and efficient anti-static function is realized. It is suitable for aerospace and marine engineering fields, provides a more comprehensive protection effect, reduces costs, and has excellent mechanical properties and protective properties.
Smart Images

Figure CN118772822A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of protective films, and in particular relates to an MS resin (silane-modified polyether polymer) adhesive composition, an antistatic protective film, and a preparation method and application thereof. Background Art
[0002] In the fields of aerospace and marine engineering, heat-resistant coatings and heavy-duty anti-corrosion coatings face challenges from a variety of harsh environmental factors such as light, electricity, water, dust, acid and alkali, as well as the bumps and friction they may suffer during transportation. In order to enhance the protective effect of these coatings, a protective film is usually added to their surface. These protective films can be made of a variety of materials, including plastic films such as polyethylene (PE), polypropylene (PE), polytetrafluoroethylene (PTFE), or foam films with elastic and shock-absorbing functions. In addition, there are spray-molded film materials such as silicone, polyurethane, alkyd resin, etc. These materials need to have simple processes, fast curing, good toughness and wear resistance, impact resistance, corrosion resistance and anti-static properties, easy peeling, etc., and the cost should be as low as possible.
[0003] The patent "A polyurethane adhesive composition, protective film and its application" (authorization announcement number CN 113444484B) discloses a polyurethane adhesive composition, a protective film and its application, which is composed of a fluorine coating, an adhesive layer and a release adhesive layer to protect the substrate layer. The curing temperature of the adhesive layer is 115-125°C.
[0004] The patent, "Resin Composition and Surface Protective Film" (Granted Publication No. CN 109422952B), discloses a resin composition that can impart excellent peelability, storage stability, antifouling properties, damage resistance, and water repellency to a surface protective film. The composition comprises a thermoplastic resin, a fluorinated copolymer, and solid particles. The surface protective film comprises an adhesive layer, an intermediate layer, and a backing layer, and is prepared using a mixing and heating process.
[0005] The patent, "Resin Composition for Protective Film" (Granted Publication No. 100387652C), discloses a resin composition that provides excellent heat resistance, water resistance, and visible light transmittance without the need for a double-layer protective film. In particular, when used as a protective film for a colored resin used in liquid crystal display color filters, the composition can form a protective film with high surface smoothness and excellent resistance to ITO vapor deposition. The resin composition also exhibits good storage stability. The base resin of the resin composition is an epoxy resin, and no antistatic function is introduced.
[0006] The patent application "Antistatic Silicone Protective Film" (application publication number CN 115418181A) discloses an antistatic silicone protective film, which includes: a substrate layer; and a first antistatic layer formed on one side of the substrate layer.
[0007] The patent, "Semi-interpenetrating polymer network polyurethane-polyurea protective film" (authorization publication number CN 101939395 B), discloses an outer layer of a film, strip, or composite component comprising: a) at least one layer comprising a cross-linked polymer selected from polyurethane, polyurea, and optionally an acrylate, and b) an adhesive layer. The protective film requires mold production and does not mention antistatic properties.
[0008] The aforementioned patented protective film technologies present several challenges, including complex construction, cumbersome preparation and application processes, a lack of anti-static functionality, or a relatively complex process for implementing this functionality. Traditional plastic films or foam films, while simple, offer limited protection and lack a tight fit on irregularly shaped parts.
[0009] Traditional resin materials, such as alkyd, epoxy, and polyurethane, each have their limitations. For example, alkyds have long drying times and poor water and alkali resistance. Epoxy resins are expensive, have high viscosity, require large amounts of diluent, and some curing agents are toxic. They are also brittle and have poor release and anti-static properties. Polyurethanes offer excellent wear resistance and strength, but suffer from poor weather resistance, poor release properties, and a long curing time. Silicone resins offer excellent thermal stability and weather resistance, but poor anti-static properties, average corrosion resistance, weak film-forming properties, and mechanical strength, leading to high costs. Summary of the Invention
[0010] Based on the above technical background, the main purpose of the present invention is to provide a MS resin adhesive composition, an antistatic protective film, and a preparation method and application thereof to overcome the deficiencies in the prior art.
[0011] To achieve the aforementioned object of the invention, the technical solutions adopted by the present invention include:
[0012] The first aspect of the present invention is to provide a MS resin adhesive composition, which comprises a component A and a component B, wherein the mass ratio of the component A to the component B is 100:(3-4), wherein:
[0013] Component A is prepared from plasticizer, thixotropic agent, silica solid-supported antistatic agent, ultraviolet light absorber, light stabilizer, MS resin, coupling agent and dehydrating agent;
[0014] Component B is made from a catalyst and a plasticizer.
[0015] Preferably, the A component is prepared by the following steps:
[0016] Step 1: mixing a plasticizer, a thixotropic agent, a silica-supported antistatic agent, an ultraviolet light absorber, and a light stabilizer, stirring and dispersing the mixture, then heating the mixture and continuing to stir and disperse the mixture;
[0017] Step 2: After cooling, add MS resin under nitrogen protection, stir and disperse, then add coupling agent and desiccant, stir evenly to obtain component A.
[0018] More preferably, in step 1,
[0019] The plasticizer is selected from one or more of 2000D (polyether polyol), DOTP (dioctyl terephthalate), DINP (diisononyl phthalate), DOP (dioctyl phthalate), and DINCH (diisononyl cyclohexane-1,2-dicarboxylate); and / or,
[0020] The thixotropic agent is selected from one or more of silicon powder, white carbon black, and wollastonite; and / or,
[0021] The silicon dioxide solid-supported antistatic agent is AA@SiO2; and / or,
[0022] The ultraviolet light absorber is selected from 2'-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole (UV-326), 2-(2H-benzotriazole-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol (UV-928), 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole (UV-329), 2-(2-hydroxy-3'-tert-butyl-5'-methylphenyl)benzotriazole (UV-326), 2-(2H-benzotriazole-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol (UV-928), One or more of: -3,5-bis(a,a-dimethylbenzyl)phenyl)benzotriazole (UV-234), 2-[2-hydroxy-3,5-bis(1,1-dimethylpropylphenyl)]-2H-benzotriazole (UV-328), 2,2'-methylenebis(4-tert-octyl-6-benzotriazolephenol) (UV-360), and 2-(2'-hydroxy-5'-methylphenyl)benzotriazole (UV-P); and / or,
[0023] The light stabilizer is selected from bis-2,2,6,6-tetramethylpiperidinol sebacate (770), polymer of succinic acid and (4-hydroxy-2,2,6,6-tetramethyl-1-piperidinol) (622), poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-[(2,2,6,6,-tetramethyl-piperidinyl)imino]-1,6-hexanediol[(2,2,6,6-tetramethyl-4-piperidinyl)imino]}(UV-944), 2,2,6,6-tetramethyl-4-piperidinyl stearyl One or more of the following: ester (UV-3853), 1,5,8,12-tetrakis[4,6-di(N-butyl-N-1,2,2,6,6-pentamethyl-4-piperidinylamino)-1,3,5-triazin-2-yl]-1,5 (UV-119), and the polymer of the reaction product of N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine with 2,4,6-trichloro-1,3,5-triazine and N-butyl-1-butylamine and N-butyl-2,2,6,6-tetramethyl-4-piperidinamine (UV-2020).
[0024] Further preferably, the silica-supported antistatic agent AA@SiO2 is prepared by the following steps: heating nano-silica to 350-450°C for activation treatment for 4-6 hours to obtain activated nano-silica, placing the activated nano-silica in toluene for ultrasonic dispersion, then heating for reaction, cooling and centrifuging after the reaction, washing and drying the precipitate to obtain the product.
[0025] Preferably, in step 1,
[0026] Mix 40-80 parts of plasticizer, 5-10 parts of thixotropic agent, 3-5 parts of silica-supported antistatic agent, 0.5-1.0 parts of ultraviolet light absorber, and 0.1-0.5 parts of light stabilizer, stir and disperse at normal pressure for 5-15 minutes, then evacuate, heat to 100-130°C, and stir and disperse for 1-3 hours.
[0027] Preferably, in step 2, the MS resin comprises a first MS resin (silane-modified polyether polymer) and a second MS resin (silane-modified polyether polymer), wherein the first MS resin has a high modulus and low viscosity, a tensile modulus of 1.5 to 3.0 MPa, and a viscosity of 400 to 15,000 mPa.s, and the second MS resin has a medium-high modulus and high viscosity, a tensile modulus of 0.8 to 1.5 MPa, and a viscosity of 15,000 to 200,000 mPa.s; and / or,
[0028] The coupling agent is an amino coupling agent, selected from one or more of γ-aminopropyltriethoxysilane (KH-550), γ-aminopropyltrimethoxysilane (KH-540), N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane (KH-792), N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane (KH-602), N-(β-aminoethyl)-γ-aminopropyltriethoxysilane (KH-791), N-β-(aminoethyl)γ-aminopropylmethyldiethoxysilane, phenylaminomethyltriethoxysilane (ND-42), and phenylaminomethyltrimethoxysilane (ND-73); and / or,
[0029] The dehydrating agent is a vinyl silane coupling agent, selected from one or more of vinyl trichlorosilane (KH-150), vinyl triethoxysilane (KH-151), vinyl trimethoxysilane (KH-171), and vinyl tris-(2-methoxyethoxy) silane (KH-172).
[0030] Preferably, in step 2,
[0031] After the reaction is completed, the temperature is lowered to below 50° C., 0 to 100 parts of filler are added under nitrogen protection, and the mixture is stirred and dispersed for 5 to 15 minutes. Subsequently, 1 to 1.5 parts of coupling agent and 6 to 10 parts of dehydrating agent are added, and the mixture is stirred and dispersed for 5 to 15 minutes to obtain component A.
[0032] Preferably, the B component is prepared by the following steps: adding a plasticizer to the catalyst for dilution;
[0033] Preferably, the catalyst is selected from one or more of an amine catalyst and an organic metal catalyst, the amine catalyst is selected from one or more of N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl) ether, N,N,N',N'-tetramethylalkylenediamine, triethylamine, N,N-dimethylbenzylamine, triethanolamine, and N,N'-dimethylpyridine, and the organic metal catalyst is an organic tin compound selected from dimethyltin di-2-ethylhexanoate, dimethyltin dilaurate, di-n-butyltin diacetate, di- One or more of di-n-butyltin-2-ethylhexanoate, di-n-butyltin dioctanoate, di-n-butyltin di-2,2-dimethyloctanoate, di-n-butyltin dilaurate, di-n-butyltin distearate, di-n-butyltin dimaleate, di-n-butyltin dioleate, di-n-octyltin di-2-ethylhexanoate, di-n-octyltin di-2,2-dimethyloctanoate, di-n-octyltin dimaleate, di-n-octyltin dilaurate, di-n-butyltin oxide, di-n-octyltin oxide, tetrabutyl titanate, or tetraisopropyl titanate; and / or,
[0034] Preferably, the plasticizer is selected from one or more of 2000D (polyether polyol), DOTP (dioctyl terephthalate), DINP (diisononyl phthalate), DOP (dioctyl phthalate), and DINCH (diisononyl cyclohexane-1,2-dicarboxylate).
[0035] A second aspect of the present invention is to provide a method for preparing an antistatic protective film, wherein the antistatic protective film is prepared using the MS resin adhesive composition described in the first aspect of the present invention, and the preparation method comprises the following steps:
[0036] Step a, dispersing component A in a diluent to obtain a mixed solution A, and dispersing component B in a diluent to obtain a mixed solution B;
[0037] Step b: Mixing the mixed solution A and the mixed solution B to obtain a mixed solution C, and applying the mixed solution C on a substrate to solidify the mixed solution.
[0038] The third aspect of the present invention is to provide a protective film produced by the preparation method described in the second aspect of the present invention.
[0039] The fourth aspect of the present invention is to provide an application of the antistatic protective film described in the third aspect of the present invention in the fields of aerospace and marine engineering to protect heat-resistant coatings and heavy-duty anti-corrosion coatings during storage and transportation.
[0040] The beneficial effects of the present invention are:
[0041] (1) The present invention addresses the shortcomings of existing protective film technology, such as insufficient protection provided by conventional films, poor adhesion to irregularly shaped parts, and the complex structure, cumbersome preparation and construction, lack of anti-static function, or complex introduction process of non-traditional protective films. The present invention utilizes an adhesive composition based on MS resin and introduces a solid-supported anti-static agent, achieving the advantages of simple construction, simple structure, and permanent anti-static function, as well as high adhesion to irregularly shaped parts. Furthermore, the adhesive composition is low-cost.
[0042] The MS resin adhesive composition described in this invention comprises two types of MS resins: medium modulus and high modulus. Through precise proportioning, the mechanical strength of the protective film can be customized to meet diverse requirements. This adhesive composition has a wide range of applications, including the production and processing of protective films for various elastomers, including polyurethanes, epoxies, and silicones, providing a more flexible and efficient option for related industries.
[0043] (2) The antistatic protective film made from the MS resin has both excellent mechanical and antistatic properties and is particularly suitable for external heat-resistant coatings and anti-corrosion coatings in the fields of aviation and marine engineering. The protective film provided by the present invention eliminates the traditional release film, greatly simplifying the film structure and making the construction process simpler and faster. The protective film is easy to tear off without causing any damage to the resin after tearing off. At the same time, the protective film inherits the traditional advantages of release films, such as excellent heat resistance, moisture resistance, and mildew resistance, as well as excellent protective properties and release effect.
[0044] In addition, the anti-static protective film is cost-effective and has a simple molding process. Users can choose transparent or colored products by adding fillers as needed, and efficient release can be achieved without the need for additional coating of fluorine release agents.
[0045] (3) The adhesive composition of the MS resin of the present invention also includes a silica-supported antistatic agent, which is integrated into the MS resin adhesive system, not only giving the protective film a long-lasting antistatic effect, but also making the antistatic surface resistivity of the protective film reach 10 6 (Ω·m), which significantly improves the static control ability of the product and ensures that the antistatic agent can be well integrated into the system without affecting the transparency of the protective film.
[0046] (4) The present invention provides an effective anti-static protective film by simplifying the structure and construction process of the protective film, and provides an efficient, convenient and fully functional protective film product for external heat protection coatings and anti-corrosion coatings in the fields of aviation and marine engineering. It is particularly suitable for special-shaped parts and can provide more comprehensive protection. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 Shown is a simplified synthetic route for MS resin;
[0048] Figure 2 A photograph of the antistatic protective film obtained by coating in Example 4 is shown;
[0049] Figure 3 A photograph showing the peeling of the antistatic protective film of Example 4 is shown. DETAILED DESCRIPTION
[0050] The present invention will be described in detail below, and the characteristics and advantages of the present invention will become clearer and more distinct with the following description.
[0051] To address these issues, this patent proposes a sprayable / brushable antistatic protective film based on an MS resin adhesive composition. This film is particularly suitable for special-shaped parts, providing comprehensive protection. The MS resin production process includes three typical routes. Among them, the SiPU1 route, which serves as the base adhesive for sprayable / brushable protective films, specifically addresses the aforementioned issues.
[0052] The first aspect of the present invention is to provide a MS resin adhesive composition, which comprises a component A and a component B, wherein the mass ratio of the component A to the component B is 100:(3-4), wherein:
[0053] Component A is prepared from plasticizer, thixotropic agent, silica solid-supported antistatic agent, ultraviolet light absorber, light stabilizer, MS resin, coupling agent and dehydrating agent;
[0054] Component B is made from a catalyst and a plasticizer.
[0055] Preferably, the mass ratio of component A to component B is 100:3.65.
[0056] The A component is prepared by the following steps:
[0057] Step 1: mixing a plasticizer, a thixotropic agent, a silica-supported antistatic agent, an ultraviolet light absorber, and a light stabilizer, stirring and dispersing the mixture, then heating the mixture and continuing to stir and disperse the mixture;
[0058] Step 2: After cooling, add MS resin under nitrogen protection, stir and disperse, then add coupling agent and desiccant, stir evenly to obtain component A.
[0059] The above steps are described in detail below.
[0060] Step 1: The plasticizer is selected from one or more of 2000D (polyether polyol), DOTP (dioctyl terephthalate), DINP (diisononyl phthalate), DOP (dioctyl phthalate), and DINCH (diisononyl cyclohexane-1,2-dicarboxylate), preferably 2000D or DINP, more preferably DINP.
[0061] The thixotropic agent is selected from one or more of silica powder, white carbon black, and wollastonite, preferably silica powder.
[0062] The silica-supported antistatic agent is AA@SiO2. Preferably, the antistatic agent is prepared by the following steps: heating nano-silica to 350-450°C for activation treatment for 4-6 hours to obtain activated nano-silica; placing the activated nano-silica in toluene for ultrasonic dispersion; then heating for reaction; cooling and centrifuging after the reaction; washing and drying the precipitate to obtain the solid-supported antistatic agent.
[0063] More preferably, the antistatic agent is prepared by heating nano-silica to 400°C for activation for 5 hours to obtain activated nano-silica. The activated nano-silica is an amorphous white powder with a particle size between 20 and 100 nanometers and a variety of morphologies, including spheres, rods, or flakes. The surface remains pristine and has not undergone any chemical modification. The activated nano-silica and substance X are dispersed in 3000 ml of toluene dehydrated with 3A molecular sieves and ultrasonically dispersed for 10 minutes to ensure uniform mixing. The mixture is then heated to reflux and allowed to react under these conditions for 4 hours. After the reaction is complete, heating is stopped and the mixture is allowed to cool. Next, the mixture is centrifuged at 13,000 rpm, the precipitate is collected, and repeatedly washed with anhydrous ethanol to remove impurities. Finally, the washed precipitate is dried in an oven at 105°C for 5 hours. The resulting product is the desired solid-supported antistatic agent, labeled AA@SiO2. The nano-silicon dioxide has a particle size of 20 to 40 nanometers and a spherical shape.
[0064] The substance X is preferably bis(methoxyethyl)-3-trimethoxysilylpropylammonium chloride, as shown in formula (1):
[0065]
[0066] The ultraviolet light absorber is selected from 2'-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole (UV-326), 2-(2H-benzotriazole-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol (UV-928), 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole (UV-329), 2-(2-hydroxy-3,5-bis(a,a-dimethylbenzyl)phenyl)benzotriazole (UV-234), 2-[2-hydroxy-3,5-bis(1,1-dimethylpropylphenyl)]-2H-benzotriazole (UV-32 8), one or more of 2,2'-methylenebis(4-tert-octyl-6-benzotriazolephenol) (UV-360), 2-(2'-hydroxy-5'-methylphenyl)benzotriazole (UV-P), preferably 2'-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole (UV-326) or 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol (UV-928), more preferably 2'-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole (UV-326).
[0067] The light stabilizer is selected from bis-2,2,6,6-tetramethylpiperidinol sebacate (770), polymer of succinic acid and (4-hydroxy-2,2,6,6-tetramethyl-1-piperidinol) (622), poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-[(2,2,6,6,-tetramethyl-piperidinyl)imino]-1,6-hexanediol[(2,2,6,6-tetramethyl-4-piperidinyl)imino]} (UV-944), 2,2,6,6-tetramethyl-4-piperidinyl stearate (UV-3853), 1,5 ,8,12-tetrakis[4,6-di(N-butyl-N-1,2,2,6,6-pentamethyl-4-piperidinylamino)-1,3,5-triazine-2-yl]-1,5 (UV-119), a polymer of the reaction product of N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine with 2,4,6-trichloro-1,3,5-triazine and N-butyl-1-butylamine and N-butyl-2,2,6,6-tetramethyl-4-piperidinamine (UV-2020), preferably bis-2,2,6,6-tetramethylpiperidinol sebacate (770).
[0068] Mix 40-80 parts of plasticizer, 5-10 parts of thixotropic agent, 3-5 parts of silica-supported antistatic agent, 0.5-1.0 parts of ultraviolet light absorber, and 0.1-0.5 parts of light stabilizer, stir and disperse at normal pressure for 5-15 minutes, then evacuate, heat to 100-130°C, and stir and disperse for 1-3 hours.
[0069] Preferably, 50 parts of plasticizer, 8 parts of thixotropic agent, 3 parts of silica-supported antistatic agent, 0.9 parts of ultraviolet light absorber, and 0.3 parts of light stabilizer are mixed, stirred and dispersed at normal pressure for 10 minutes, then vacuumed, heated to 120° C., and stirred and dispersed for 2 hours.
[0070] In step 2, the MS resin includes a first MS resin (silane-modified polyether polymer) and a second MS resin (silane-modified polyether polymer), both of which are synthesized by the Zhonghua MS route, SiPU1 route or SiPU2 route (see Figure 1 ), the first MS resin and the second MS resin are both synthesized from the SiPU2 route, the first MS resin has a high modulus and low viscosity, a tensile modulus of 1.5 to 3.0 MPa, and a viscosity of 400 to 15000 mPa.s, and the second MS resin has a medium-high modulus and high viscosity, a tensile modulus of 0.8 to 1.5 MPa, and a viscosity of 15000 to 200000 mPa.s.
[0071] Preferably, the viscosity of the first MS resin is 500-10,000 mPa.s, providing high modulus; the viscosity of the second MS resin is 15,000-100,000 mPa.s, providing medium-high modulus.
[0072] The addition mass ratio of the first MS resin to the second MS resin is (8-12):1, and the preferred addition ratio is 10:1.
[0073] MS resin is healthy and environmentally friendly, containing no formaldehyde or free isocyanates, and will not contaminate substrates. It also offers excellent paintability and is easily colorable. Its unique "molecule-free structure" imparts superior mildew resistance. MS resin also offers excellent mechanical properties, excellent release properties, and adjustable cure speeds. It is also a more affordable alternative to silicone 107 adhesive.
[0074] During the preparation process, a filler may be added. The filler is selected from one or more of calcium carbonate, barium sulfate, kaolin, diatomaceous earth, talc, graphite, aluminum oxide powder, glass powder, asbestos powder, mica powder, quartz powder, powdered cork, and corundum. It is possible to choose to completely omit the filler to avoid affecting transparency or coloring, or to carefully select fillers that do not significantly affect the desired properties based on actual needs. Preferably, the filler is calcium carbonate.
[0075] The coupling agent is an amino coupling agent, selected from one or more of γ-aminopropyltriethoxysilane (KH-550), γ-aminopropyltrimethoxysilane (KH-540), N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane (KH-792), N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane (KH-602), N-(β-aminoethyl)-γ-aminopropyltriethoxysilane (KH-791), N-β-(aminoethyl)γ-aminopropylmethyldiethoxysilane, phenylaminomethyltriethoxysilane (ND-42), and phenylaminomethyltrimethoxysilane (ND-73).
[0076] Preferably, the coupling agent is γ-aminopropyltriethoxysilane (KH-550) or N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane (KH-792).
[0077] More preferably, the coupling agent is γ-aminopropyltriethoxysilane (KH-550).
[0078] The dehydrating agent is a vinyl silane coupling agent, selected from one or more of vinyl trichlorosilane (KH-150), vinyl triethoxysilane (KH-151), vinyl trimethoxysilane (KH-171), and vinyl tris-(2-methoxyethoxy) silane (KH-172).
[0079] Preferably, the desiccant is vinyltrimethoxysilane (KH-171).
[0080] The dehydrating agent and coupling agent used in the present invention not only have the main functions of dehydrating and connecting the MS resin (silane-modified polyether polymer) base glue and filler, but also play a certain role in the curing speed of the entire MS resin adhesive composition.
[0081] After the reaction is completed, the temperature is lowered to below 50° C., 0 to 100 parts of filler are added under nitrogen protection, and the mixture is stirred and dispersed for 5 to 15 minutes. Subsequently, 1 to 1.5 parts of coupling agent and 6 to 10 parts of dehydrating agent are added, and the mixture is stirred and dispersed for 5 to 15 minutes to obtain component A.
[0082] Preferably, after the reaction is completed, the temperature is lowered to below 50° C., 100 parts of filler are added under nitrogen protection, and the mixture is stirred and dispersed for 10 minutes. Subsequently, 1.2 parts of coupling agent and 6.5 parts of dehydrating agent are added, and the mixture is stirred and dispersed for 10 minutes to obtain component A.
[0083] The B component is prepared by the following steps: adding a plasticizer to the catalyst and diluting the mixture.
[0084] Preferably, the catalyst is selected from one or more of an amine catalyst and an organometallic catalyst, the amine catalyst is selected from one or more of N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl) ether, N,N,N',N'-tetramethylalkylenediamine, triethylamine, N,N-dimethylbenzylamine, triethanolamine, and N,N'-lutidine, and the organometallic catalyst is an organotin compound selected from dimethyltin di-2-ethylhexanoate, dimethyltin dilaurate, di-n-butyltin diacetate, and dimethyltin diacetate. , di-n-butyltin di-2-ethylhexanoate, di-n-butyltin dioctanoate, di-n-butyltin di-2,2-dimethyloctanoate, di-n-butyltin dilaurate, di-n-butyltin distearate, di-n-butyltin dimaleate, di-n-butyltin dioleate, di-n-octyltin di-2-ethylhexanoate, di-n-octyltin di-2,2-dimethyloctanoate, di-n-octyltin dimaleate, di-n-octyltin dilaurate, di-n-butyltin oxide and di-n-octyltin oxide, tetrabutyl titanate or tetraisopropyl titanate.
[0085] More preferably, the catalyst is di-n-butyltin dilaurate.
[0086] The plasticizer is selected from one or more of 2000D, (polyether polyol), DOTP (dioctyl terephthalate), DINP (diisononyl phthalate), DOP (dioctyl phthalate), and DINCH (diisononyl cyclohexane-1,2-dicarboxylate), preferably 2000D or DINP, and more preferably DINP.
[0087] Preferably, 40 to 80 parts of plasticizer are added to 3 to 7 parts of catalyst for dilution.
[0088] More preferably, 50 parts of plasticizer are added to 5 parts of catalyst and diluted.
[0089] A second aspect of the present invention is to provide a method for preparing an antistatic protective film, wherein the antistatic protective film is prepared using the MS resin adhesive composition described in the first aspect of the present invention, and the preparation method comprises the following steps:
[0090] Step a, dispersing component A in a diluent to obtain a mixed solution A, and dispersing component B in a diluent to obtain a mixed solution B;
[0091] Step b: Mixing the mixed solution A and the mixed solution B to obtain a mixed solution C, and applying the mixed solution C on a substrate to solidify the mixed solution.
[0092] The above steps are described in detail below.
[0093] In step a, the diluent is selected from one of 120# solvent oil, petroleum ether, ethyl acetate, and butyl acetate, preferably 120# solvent oil.
[0094] 100 parts by weight of component A are dispersed in 60 to 80 parts of diluent to obtain a mixed solution A, and 3.65 parts of component B are dispersed in 20 to 40 parts of diluent to obtain a mixed solution B.
[0095] Preferably, 100 parts by weight of component A are dispersed in 70 parts of diluent to obtain a mixed solution A, and 3.65 parts of component B are dispersed in 30 parts of diluent to obtain a mixed solution B.
[0096] In step b, the mixed solution C is coated on the substrate and cured at 20-35°C for 2-8 hours. The coating amount is 200-400 g / cm 2 The thickness of the protective layer is 350 to 400 μm.
[0097] Preferably, the mixed solution C is coated on the substrate and cured at 30°C for 4 hours, and the coating amount is 300-320 g / cm 2 The thickness of the protective layer is 350 to 400 μm.
[0098] The third aspect of the present invention is to provide an antistatic protective film prepared by the preparation method described in the second aspect of the present invention.
[0099] The fourth aspect of the present invention is to provide an application of the antistatic protective film described in the third aspect of the present invention in the fields of aerospace and marine engineering to protect heat-resistant coatings and heavy-duty anti-corrosion coatings during storage and transportation.
[0100] Preferably, the heat-resistant coating and heavy-duty anti-corrosion coating include one or more of an epoxy system, a phenolic resin system, a silicone system, and a polyurea system.
[0101] The MS resin adhesive composition described in this invention offers significant advantages as a protective film material for applications in aerospace and marine engineering, providing a more efficient, comprehensive, and environmentally friendly protective solution. It is also highly suitable for special-shaped parts. This MS resin adhesive composition exhibits excellent flexibility, cure speed, environmental performance, cost-effectiveness, and overall protective properties, making it suitable for use as a base adhesive for spray-on protective films.
[0102] Example
[0103] The present invention is further described below by using specific examples. These examples are only for illustration and are not intended to limit the scope of the present invention. All raw materials used in the examples of the present invention except AA@SiO2 were purchased.
[0104] MS resin is commercially available 200D, Taking 3623T (Jiangsu Ruiyang Antai) as an example, both polymers have polyether polymer as the main chain segment. The solvents used are 120# solvent oil, petroleum ether, ethyl acetate, butyl acetate, etc., all of which are industrial grade.
[0105] The AA@SiO2 is prepared by the following steps:
[0106] Nano-silica was activated by heating it to 400°C for 5 hours to obtain activated nano-silica. This activated nano-silica is an amorphous white powder with a particle size ranging from 20 to 100 nanometers and a variety of morphologies, including spheres, rods, or flakes. Its surface remains pristine, unmodified. The activated nano-silica and substance X (bis(methoxyethyl)-3-trimethoxysilylpropylammonium chloride) were co-dispersed in 3000 ml of toluene dehydrated with 3A molecular sieves and ultrasonically dispersed for 10 minutes to ensure uniform mixing. The mixture was then heated to reflux and allowed to react for 4 hours. After the reaction, heating was stopped and the mixture was allowed to cool. The mixture was then centrifuged at 13,000 rpm, and the precipitate was collected and repeatedly washed with anhydrous ethanol to remove impurities. Finally, the washed precipitate was dried in an oven at 105°C for 5 hours. The resulting product is the desired solid-supported antistatic agent, labeled AA@SiO2.
[0107] Example 1
[0108] The preparation method of component A of the MS resin adhesive of this embodiment comprises the following steps:
[0109] 500 parts of DINP (diisononyl phthalate), 80 parts of silicon powder, 30 parts of AA@SiO2, 9 parts of UV-326, and 3 parts of 770 were added to the double planetary reactor in sequence, and stirred and dispersed at low speed for 10 minutes under normal pressure; then the vacuum was turned on, the temperature was raised to 120°C, and after high-speed dispersion stirring for 2 hours, the system was cooled to below 50°C; then nitrogen was introduced and 1000 parts of 200D (first MS resin, with a viscosity of 4000-6000 mPa.s and a tensile modulus of 1.8 MPa), 100 parts After 3623T (the second MS resin, with a viscosity of 20,000-30,000 mPa.s and a tensile modulus of 1.2 MPa), disperse and stir at low speed for 10 minutes, then add 65 parts of vinyltrimethoxysilane (KH-171) and 12 parts of γ-aminopropyltriethoxysilane (KH-550) in sequence, stir at medium speed for 10 minutes, and then discharge and seal for storage.
[0110] The preparation method of component B of the MS resin adhesive of this embodiment comprises the following steps:
[0111] 50 parts of di-n-butyltin dilaurate are diluted with 500 parts of DINP.
[0112] The method for using the MS resin adhesive composition of this embodiment to prepare the antistatic protective film is as follows:
[0113] (a) Dispersing 100 parts of the MS resin adhesive component A in 70 parts of 120# solvent oil to obtain a mixed solution A;
[0114] (b) dispersing 3.65 parts of the MS resin adhesive component B in 30 parts of 120# solvent oil to obtain a mixed solution B;
[0115] (c) Mixed solution A and mixed solution B are dispersed to obtain mixed solution C.
[0116] (d) coating the mixed solution C on the substrate layer with a coating amount of 300 to 320 g / cm 2 The protective film was obtained by curing at 30°C for 4 hours. The thickness of the protective layer was 350-400 μm.
[0117] Example 2
[0118] The preparation was carried out in a similar manner to Example 1, except that: The dosage of 3623T is increased to 150 parts.
[0119] Example 3
[0120] The preparation was carried out in a manner similar to Example 1, except that the amount of AA@SiO2 was adjusted to 50 parts.
[0121] Example 4
[0122] This embodiment uses the MS resin adhesive composition in Example 1 to protect the outer heat-resistant coating of the epoxy resin system. The specific operation is to evenly apply the MS resin adhesive on the surface of the outer heat-resistant coating to form a 350-400 μm protective film thereon. Figure 2 As shown in the figure, the overall protection effect is improved. Figure 3 As shown. Figure 2 It can be seen that the protective film has extremely high transparency. Figure 3 It can be seen that the protective film is easy to tear off and will not cause any damage to the resin after tearing off.
[0123] Example 5
[0124] This example uses the MS resin adhesive composition of Example 1 to protect a polyurea-based heavy-duty anti-corrosion coating. Specifically, the MS resin adhesive is evenly applied to the surface of the heavy-duty anti-corrosion coating, forming a 350-400 μm thick protective film thereon, enhancing the overall protective effect.
[0125] Example 6:
[0126] This example uses the MS resin adhesive composition of Example 2 to protect the epoxy resin system's external heat-resistant coating. Specifically, the MS resin adhesive is evenly applied to the surface of the external heat-resistant coating, forming a 350-400 μm thick protective film thereon, enhancing the overall protective effect.
[0127] Example 7:
[0128] This example uses the MS resin adhesive composition of Example 2 to protect a polyurea-based heavy-duty anti-corrosion coating. Specifically, the MS resin adhesive is evenly applied to the surface of the heavy-duty anti-corrosion coating, forming a 350-400 μm thick protective film thereon, thereby enhancing the overall protective effect.
[0129] Example 8:
[0130] This example uses the MS resin adhesive composition of Example 3 to protect the epoxy resin system's external heat-resistant coating. Specifically, the MS resin adhesive is evenly applied to the surface of the external heat-resistant coating, forming a 350-400 μm thick protective film thereon, enhancing the overall protective effect.
[0131] Example 9:
[0132] This example uses the MS resin adhesive composition of Example 3 to protect a polyurea-based heavy-duty anti-corrosion coating. Specifically, the MS resin adhesive is evenly applied to the surface of the heavy-duty anti-corrosion coating, forming a 350-400 μm thick protective film thereon, thereby enhancing the overall protective effect.
[0133] Comparative Example
[0134] Comparative Example 1
[0135] The preparation was carried out in a manner similar to Example 1, except that AA@SiO2 was not added.
[0136] Comparative Example 2
[0137] The preparation was carried out in a similar manner to Example 1 except that: 3623T.
[0138] Comparative Example 3
[0139] The coating was carried out in a manner similar to that of Example 4, except that before applying the MS resin adhesive composition, an additional layer of fluorine release agent was applied on the same outer heat-resistant coating.
[0140] Comparative Example 4
[0141] The coating was carried out in a manner similar to that of Example 5, except that before applying the MS resin adhesive composition, an additional layer of fluorine release agent was applied on the same outer heavy anti-corrosion coating.
[0142] Comparative Example 5
[0143] The coating was carried out in a manner similar to that of Example 6, except that before applying the MS resin adhesive composition, an additional layer of fluorine release agent was applied on the same outer heat-resistant coating.
[0144] Comparative Example 6
[0145] The coating was carried out in a manner similar to that of Example 7, except that before applying the MS resin adhesive composition, an additional layer of fluorine release agent was applied on the same outer heavy anti-corrosion coating.
[0146] Comparative Example 7
[0147] The coating was carried out in a manner similar to that of Example 8, except that before applying the MS resin adhesive composition, an additional layer of fluorine release agent was applied on the same outer heat-resistant coating.
[0148] Comparative Example 8
[0149] The coating was performed in a manner similar to that of Example 9, except that before applying the MS resin adhesive composition, an additional layer of fluorine release agent was applied on the same outer heavy anti-corrosion coating.
[0150] Experimental example
[0151] Experimental Example 1 Mechanical Properties Test
[0152] The adhesives prepared in Examples 1-3 and Comparative Examples 1-2 were tested for tensile strength and tensile elongation, and the protective films prepared in Examples 4-9 and Comparative Examples 3-8 were tested for physical properties such as impedance performance and room-temperature peel strength. The testing instruments and methods are mainly as follows. The test results are shown in Table 1:
[0153] (1) Tensile strength test: in accordance with GB / T 528 (Type I);
[0154] Elongation at break test: in accordance with GB / T 528 (Type I);
[0155] Hardness: According to GB / T 531.
[0156] (2) Surface resistivity test: Use SL-030 surface resistivity tester, place it directly on the surface of the protective film product to be tested, and take the average of three tests;
[0157] (3) Room temperature peeling strength test: The peeling strength of the protective film was tested using a CMT4104 microcomputer-controlled electronic universal testing machine. The test standard was in accordance with ASTM D3330.
[0158] Table 1 Test results
[0159]
[0160] As can be seen from Table 1, the tensile strength and elongation at break of the protective films prepared from the MS resin adhesive compositions of Examples 1 to 3 are higher than those of the protective film prepared from the composition of Comparative Example 2, and the antistatic surface resistivity of the protective films of Examples 1 to 3 can reach 10 6 (Ω·m). The room-temperature peel strength of the protective films prepared in Examples 4-9 was higher than that of the protective films prepared in Comparative Examples 3-8. This indicates that the protective films formed from the adhesive composition of the present invention have good tensile strength, elongation at break, room-temperature peel strength, and antistatic properties.
[0161] The present invention has been described in detail above with reference to specific embodiments and exemplary examples. However, these descriptions should not be construed as limiting the present invention. Those skilled in the art will appreciate that various equivalent substitutions, modifications, or improvements may be made to the technical solutions and implementations of the present invention without departing from the spirit and scope of the present invention, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be determined by the appended claims.
Claims
1. A MS resin adhesive composition, characterized in that: The MS resin adhesive composition comprises component A and component B, wherein the mass ratio of component A to component B is 100:(3-4), wherein: Component A is prepared from a plasticizer, a thixotropic agent, a silica-supported antistatic agent, an ultraviolet light absorber, a light stabilizer, an MS resin, a coupling agent, and a dehydrating agent; Component B is made from a catalyst and a plasticizer.
2. The MS resin adhesive composition according to claim 1, characterized in that The A component is prepared by the following steps: Step 1, mixing a plasticizer, a thixotropic agent, a silica-supported antistatic agent, an ultraviolet light absorber, and a light stabilizer, stirring and dispersing the mixture, then heating the mixture, and continuing to stir and disperse the mixture; Step 2: After cooling, add MS resin under nitrogen protection, stir and disperse, then add coupling agent and dehydrating agent, stir evenly, and obtain component A.
3. The MS resin adhesive composition according to claim 2, characterized in that: In step 1, The plasticizer is selected from one or more of 2000D, DOTP, DINP, DOP, and DINCH; and / or, The thixotropic agent is selected from one or more of silicon powder, white carbon black and wollastonite; and / or, The silicon dioxide solid-supported antistatic agent is AA@SiO2; and / or, The ultraviolet light absorber is selected from one or more of 2'-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol, 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-3,5-bis(a,a-dimethylbenzyl)phenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(1,1-dimethylpropylphenyl)]-2H-benzotriazole, 2,2'-methylenebis(4-tert-octyl-6-benzotriazolephenol), and 2-(2'-hydroxy-5'-methylphenyl)benzotriazole; and / or, The light stabilizer is selected from the group consisting of bis-2,2,6,6-tetramethylpiperidinol sebacate, a polymer of succinic acid and (4-hydroxy-2,2,6,6-tetramethyl-1-piperidinol), poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-[(2,2,6,6,-tetramethyl-piperidinyl)imino]-1,6-hexanediol[(2,2,6,6-tetramethyl-4-piperidinyl)imino]}, 2,2,6,6-tetramethyl-4- One or more of the polymers of piperidine stearate, 1,5,8,12-tetrakis[4,6-di(N-butyl-N-1,2,2,6,6-pentamethyl-4-piperidinylamino)-1,3,5-triazine-2-yl]-1,5, N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine and the reaction product of 2,4,6-trichloro-1,3,5-triazine and N-butyl-1-butylamine and N-butyl-2,2,6,6-tetramethyl-4-piperidinamine.
4. The MS resin adhesive composition according to claim 3, characterized in that: The silica-supported antistatic agent AA@SiO2 is prepared by the following steps: heating nano-silicon dioxide to 350-450° C. for activation treatment for 4-6 hours to obtain activated nano-silicon dioxide, placing the activated nano-silicon dioxide in toluene for ultrasonic dispersion, then heating for reaction, cooling and centrifuging after the reaction, washing and drying the precipitate to obtain the antistatic agent.
5. The MS resin adhesive composition according to claim 2, characterized in that: In step 1, Mix 40-80 parts of plasticizer, 5-10 parts of thixotropic agent, 3-5 parts of silica solid antistatic agent, 0.5-1.0 parts of ultraviolet light absorber and 0.1-0.5 parts of light stabilizer, stir and disperse for 5-15 minutes at normal pressure, then evacuate, heat to 100-130°C and stir and disperse for 1-3 hours.
6. The MS resin adhesive composition according to claim 2, characterized in that: In step 2, The MS resin comprises a first MS resin and a second MS resin, wherein the first MS resin has a tensile modulus of 1.5 to 3.0 MPa and a viscosity of 400 to 15000 mPa.s, and the second MS resin has a tensile modulus of 0.8 to 1.5 MPa and a viscosity of 15000 to 200000 mPa.s; and / or, The coupling agent is an amino coupling agent, selected from one or more of γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, N-β-(aminoethyl)γ-aminopropylmethyldiethoxysilane, anilinomethyltriethoxysilane, and anilinomethyltrimethoxysilane; and / or, The dewatering agent is a vinyl silane coupling agent selected from one or more of vinyl trichlorosilane, vinyl triethoxysilane, vinyl trimethoxysilane, and vinyl tri-(2-methoxyethoxy) silane; and / or, After the reaction is completed, the temperature is lowered to below 50°C, 0 to 100 parts of filler are added under nitrogen protection, stirred and dispersed for 5 to 15 minutes, and then 1 to 1.5 parts of coupling agent and 6 to 10 parts of dehydrating agent are added, stirred and dispersed for 5 to 15 minutes to obtain component A.
7. The MS resin adhesive composition according to claim 1, characterized in that: The B component is prepared by the following steps: adding a plasticizer to the catalyst for dilution; The catalyst is selected from one or more of an amine catalyst and an organic metal catalyst. The amine catalyst is selected from one or more of N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl) ether, N,N,N',N'-tetramethylalkylenediamine, triethylamine, N,N-dimethylbenzylamine, triethanolamine, and N,N'-dimethylpyridine. The organic metal catalyst is an organic tin compound selected from dimethyltin di-2-ethylhexanoate, dimethyltin dilaurate, di-n-butyltin diacetate, di-2 - one or more of di-n-butyltin ethylhexanoate, di-n-butyltin dioctanoate, di-n-butyltin di-2,2-dimethyloctanoate, di-n-butyltin dilaurate, di-n-butyltin distearate, di-n-butyltin dimaleate, di-n-butyltin dioleate, di-n-octyltin di-2-ethylhexanoate, di-n-octyltin di-2,2-dimethyloctanoate, di-n-octyltin dimaleate, di-n-octyltin dilaurate, di-n-butyltin oxide, di-n-octyltin oxide, tetrabutyl titanate or tetraisopropyl titanate; and / or, The plasticizer is selected from one or more of 2000D, DOTP, DINP, DOP, and DINCH.
8. A method for preparing an antistatic protective film, wherein the antistatic protective film is prepared using the MS resin adhesive composition according to any one of claims 1 to 7, and the preparation method comprises the following steps: Step a, dispersing component A in a diluent to obtain a mixed solution A, and dispersing component B in a diluent to obtain a mixed solution B; Step b, mixing the mixed solution A and the mixed solution B to obtain a mixed solution C, and applying the mixed solution C on a substrate for curing.
9. An antistatic protective film obtained by the preparation method according to claim 8.
10. An application of the antistatic protective film according to claim 9 in the fields of aerospace and marine engineering to protect heat-resistant coatings and heavy-duty anti-corrosion coatings during storage and transportation.