Preparation method of silicon carbide-based metal ceramic material

Through the modification treatment of titanate, ultrafine carbon black and silicon carbide and vacuum sintering technology, the problem of poor wettability between silicon carbide and metal and element interdiffusion in the coating method has been solved, and the efficient preparation of silicon carbide-based cermet materials has been achieved And the stability of electrical and thermal conductivity, suitable for high-voltage electrical contact fields.

CN118773467APending Publication Date: 2024-10-15ZHEJIANG JIANMO TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410741649.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In the process of preparing cermets from the composite of silicon carbide and metal, there are poor wettability and complex reactive interfaces, which makes it difficult to achieve high density with liquid metal infiltration, which limits the production and preparation of silicon carbide cermets. In addition, the existing coating method has complex operations and High cost, uneven coating and interdiffusion of elements affect electrical and thermal conductivity.

Method used

Modified silicon carbide is prepared using titanate, ultrafine carbon black and silicon carbide in a molar ratio of 1:1:10 to 25. It is stirred magnetically to form a gel. After vacuum sintering, the titanium carbide is coated and then mixed with copper or aluminum powder. It is sintered under vacuum conditions to form a porous silicon carbide-based cermet material, which avoids the problems of element interdiffusion and uneven coating.

Benefits of technology

It achieves good wetting of silicon carbide and metal, avoids element diffusion, improves the stability of the material's electrical and thermal conductivity, reduces production costs and environmental impact, is suitable for mass production, and is suitable for high-voltage electrical contact fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773467A_ABST
    Figure CN118773467A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a silicon carbide-based metal ceramic material, which is characterized by comprising the following steps: A, weighing titanate, superfine carbon black and silicon carbide according to a molar ratio of 1: 1: (10-25), putting into a beaker, slowly dropwise adding deionized water under magnetic stirring until the mixture is gel-shaped to obtain modified silicon carbide, and putting into a drying oven for later use; b, transferring the modified silicon carbide to a sintering furnace, heating to 1350 DEG C under a vacuum condition, preserving heat for 2 hours, and then cooling to room temperature along with the furnace to obtain a porous silicon carbide preform coated with titanium carbide; c, weighing a proper amount of copper powder, briquetting the copper powder, and placing the briquetted copper powder on the prefabricated body; and then transferring into a sintering furnace, heating to 1150 DEG C under a vacuum condition, preserving heat for 2 hours, and then cooling to room temperature along with the furnace to obtain the silicon carbide-based metal ceramic material. The obtained silicon carbide-based metal ceramic material does not have the problem of mutual diffusion of elements, does not increase electron and phonon scattering, and has the advantages of being stable in electric conduction and heat conduction performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal ceramics, and in particular to a method for preparing a silicon carbide-based metal ceramic material. Background Art

[0002] Cermet is a composite material composed of ceramics and metals. It has the excellent physical properties of metals such as electrical conductivity and thermal conductivity, and mechanical properties such as toughness and flexural strength. In addition, it also has the high hardness, high temperature resistance and oxidation resistance of ceramics.

[0003] Silicon carbide has become an ideal ceramic phase material for metal-ceramic composites due to its low density, high hardness (second only to diamond), excellent acid and alkali corrosion resistance, thermal shock resistance, and oxidation resistance. Silicon carbide-copper cermets and silicon carbide-aluminum cermets prepared by powder metallurgy have been widely used in aerospace, high-speed railways, etc. as lightweight materials and high-speed friction brake materials.

[0004] However, in the process of preparing metal ceramics by combining silicon carbide with metals such as copper and aluminum, poor wettability and the formation of complex reactive interfaces make it difficult to achieve high density and thus ideal performance in the preparation of silicon carbide-based metal ceramics by liquid metal infiltration, which limits and constrains the production and preparation of silicon carbide metal ceramics.

[0005] The methods used to improve the wetting of ceramics and metals in the prior art mainly adopt methods such as electroplating, chemical plating and molten salt plating, that is, a metal transition layer such as chromium, nickel, titanium, tungsten, etc. is plated on the surface of the ceramic powder to achieve the wetting of the ceramic and the metal. The coating method is currently widely used in the modification of silicon carbide powder. The modification of silicon carbide by metal coating has problems such as complex operating procedures, high cost of plating solution treatment, uneven coating, and difficulty in large-scale production. In addition, the coating metal will have elemental mutual diffusion and other phenomena in the process of compounding with metals such as copper and aluminum, which is easy to increase electron and phonon scattering, resulting in a decrease in the electrical and thermal conductivity of the metal ceramic. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a method for preparing a silicon carbide-based metal ceramic material. The method has simple process steps and can well solve the wetting problem between silicon carbide and metal. The obtained silicon carbide-based metal ceramic material does not have the problem of element mutual diffusion, does not increase electron and phonon scattering, and the obtained material has stable electrical and thermal conductivity.

[0007] In order to solve the above technical problems, the present invention adopts the following technical solution: a method for preparing a silicon carbide-based metal ceramic material, characterized by adopting the following steps:

[0008] A. Weigh titanate, ultrafine carbon black and silicon carbide in a molar ratio of 1:1:10-25, put them into a beaker, slowly add deionized water under magnetic stirring until it is in a gel state to obtain modified silicon carbide, and put it into an oven for later use;

[0009] B. Transfer the modified silicon carbide obtained in step A to a sintering furnace, and under vacuum conditions, first heat it to 1000° C. at a rate of 15° C. / min, then continue to heat it to 1350° C. at a rate of 5° C. / min, keep it warm for 2 hours, and then cool it to room temperature with the furnace, and take it out to obtain a porous silicon carbide preform coated with titanium carbide;

[0010] C. Weigh an appropriate amount of copper powder and the porous silicon carbide preform coated with titanium carbide obtained in step B, press the weighed copper powder into a block and place it on the porous silicon carbide preform coated with titanium carbide; then transfer it to a sintering furnace, and under vacuum conditions, heat it to 1150° C. at a rate of 5° C. / min, keep it warm for 2 hours, and then cool it to room temperature with the furnace, and take it out to obtain a silicon carbide-based copper metal ceramic material.

[0011] The amount of the copper powder can be calculated according to the size and porosity of the porous silicon carbide preform coated with titanium carbide. After calculating the required volume of copper, the appropriate mass of copper powder is weighed according to the volume of copper multiplied by the density of copper. The mass ratio of the copper powder to the porous silicon carbide preform coated with titanium carbide is preferably 0.58 to 2.2:1. The copper powder can be replaced by aluminum powder.

[0012] Furthermore, the titanate is one of tetra-n-butyl titanate, tetra-propyl titanate, tetra-propyl titanate, tetra-ethyl titanate, or a mixture thereof in any mass ratio.

[0013] The average particle size of the ultrafine carbon black is ≤300nm.

[0014] As further preferred, the average particle size of the ultrafine carbon black is 50 nm.

[0015] As a further improvement of the present invention, the step A is: weigh titanate, ultrafine carbon black and silicon carbide in a molar ratio of 1:1:10-25, put them into a beaker, add an appropriate amount of anhydrous ethanol under magnetic stirring, stir for 15 minutes to obtain modified silicon carbide, and put it into an oven for standby use;

[0016] The vacuum condition is a pressure of less than 13.3 Pa.

[0017] The copper powder in step C can be replaced by aluminum powder, and the material obtained after sintering is a silicon carbide-based aluminum metal ceramic material.

[0018] The present invention first adds titanate, ultrafine carbon black and silicon carbide into a beaker and stirs to obtain gel, then performs vacuum sintering, vacuum infiltration and finally sintering to obtain silicon carbide-based metal ceramic material. The obtained silicon carbide-based metal ceramic material has no element diffusion problem and has stable electrical and thermal conductivity.

[0019] The silicon carbide is porous silicon carbide, such as α-SiC porous ceramics or porous silicon carbide powder.

[0020] The silicon carbide-based copper metal ceramic material prepared by the present invention can be used as a high-voltage resistant metal conductor and can be applied to a 30kV-110kV high voltage environment for a long time.

[0021] The preparation method of the present invention has the following advantages:

[0022] 1. Cheap and safe raw materials, low manufacturing cost. Titanate, carbon black, deionized water or alcohol are all conventional raw materials, with a wide range of sources and are safe. Compared with metal plating processes, there is no need to use strong acid, alkali reagents or precious metal raw materials such as hydrochloric acid, nitric acid, sodium hydroxide, tin, palladium, etc.

[0023] Second, the process is simple and efficient. Compared with the metal plating method, the present invention does not require complex processes such as degreasing, roughening, activation, and coating. It only needs one pot of material to prepare gel or solution, and then dry and sinter to achieve titanium carbide coating silicon carbide. The production cycle is much shorter than that of the metal plating method, and the efficiency is high.

[0024] 3. Environmentally friendly: Compared with the metal plating method, the present invention does not need to deal with waste acid, waste alkali, metal salts and other wastes, and only emits carbon dioxide during the sintering process, so it is environmentally friendly.

[0025] Fourth, it can be scaled up for production. The metal coating process is difficult to scale up in equal proportions, and the scale-up process will result in uneven coating. However, the preparation of titanium carbide coating by the present invention only requires uniform dispersion of silicon carbide, which can be scaled up in equal proportions and is suitable for scale-up production.

[0026] 5. No element diffusion problem. The titanium carbide formed in the preparation process of the present invention has good stability. The titanium element therein, due to its unique electronegativity and binding energy, does not react and wet the titanium carbide with most molten metals, thereby achieving a continuous and smooth interface of silicon carbide / titanium carbide / metal. The coating metal in the metal coating method is easily dissolved in the molten copper or aluminum liquid, and after solidification, it is dissolved or precipitated in the metal matrix phase, increasing electron and phonon scattering and the interface. The titanium carbide in the present invention can reduce the electron and phonon scattering problems caused by interface reactions and interface discontinuities, and avoid affecting the electrical and thermal conductivity of metal ceramics.

[0027] 6. The invention has a wide range of applications. Compared with metal coating, the invention can be evenly attached to the surface of powder, film (porous body), block, and obtain uniform titanium carbide coated silicon carbide through sintering. Metal coating method can only achieve uniform coating of powder.

[0028] 7. The present invention can be extended to the preparation process of metal ceramics where the wettability between ceramics and metals is poor or there is a reaction between ceramics and metals that will affect the performance, and has wide adaptability.

[0029] 8. The silicon carbide-based copper cermet obtained by the present invention has both the hardness of silicon carbide and the excellent electrical conductivity of copper, and has great application potential in the field of high-voltage electrical contact.

[0030] In summary, the present invention has the advantages of simple process steps, being able to solve the wetting problem between silicon carbide and metal well, and the obtained silicon carbide-based metal ceramic material does not have the problem of element mutual diffusion, does not increase electron and phonon scattering, and the obtained material has stable electrical and thermal conductivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is the XRD pattern of silicon carbide based copper metal ceramic material;

[0032] Figure 2 This is a photo of silicon carbide-based copper cermet material;

[0033] Figure 3 Photo of silicon carbide-based aluminum cermet material for implementation case 3;

[0034] Figure 4 This is a comparison chart of the mechanical and electrical properties of silicon carbide-based copper metal ceramic materials with different porosities.

[0035] Description of reference numerals: Figure 1 a is the XRD curve of the silicon carbide-based aluminum metal ceramic SiC-55AI-2TiC obtained in Example 3, b is the XRD curve of the silicon carbide-based copper metal ceramic Sic-60Cu-2TiC obtained in Example 1, and c is the XRD curve of the silicon carbide-based copper metal ceramic SiC-55AI-2TiC obtained in Example 2; Figure 2 A is the silicon carbide-based copper metal ceramic material of Example 1, Figure 2 B is the silicon carbide-based copper metal ceramic material of Example 2. Figure 4 The SIC-55Cu-2TiC is Example 2, the SIC-60Cu-2TiC is Example 1, and the SIC-60Cu-3TiC is Example 4. DETAILED DESCRIPTION

[0036] Embodiment 1:

[0037] A method for preparing a silicon carbide-based copper metal ceramic material comprises the following steps: weighing 3.45 g of n-butyl titanate and 1.2 g of ultrafine carbon black with an average particle size of 25 nm respectively and adding them into a beaker; slowly adding deionized water at 50° C. and 300 rpm / min to form a homogeneous gel; adding 32.2 g of α-SiC porous ceramic with a porosity of 49%, wherein the molar ratio of n-butyl titanate: ultrafine carbon black: α-SiC porous ceramic is 1:1:10; ultrasonically treating the material for 15 min, transferring the material into an oven, and drying the material at 105° C. to obtain a gel-modified porous silicon carbide ceramic membrane;

[0038] The gel-modified porous silicon carbide ceramic membrane was transferred to a sintering furnace, and heated to 1000°C at a rate of 15°C / min under a vacuum pressure of 10Pa, and then heated from 1000°C to 1350°C at a rate of 5°C / min, and kept warm for 2h;

[0039] After cooling to room temperature, TiC0.8 modified porous silicon carbide ceramic membrane was obtained with a porosity of 45.2;

[0040] According to the size and porosity of the TiC0.8 modified porous silicon carbide ceramic membrane, the required volume of copper is calculated, and the appropriate mass of copper powder is determined by multiplying the volume of copper by the density of copper. In this embodiment, 60g of copper powder tablets and the above-mentioned TiC0.8 modified porous silicon carbide ceramic membrane are weighed and placed in a graphite crucible in sequence, and the graphite crucible is transferred to a vacuum sintering furnace. Under a vacuum pressure of 1Pa, the temperature is raised to 1150°C at a rate of 5°C / min, kept warm for 2h, and then cooled with the furnace to obtain a silicon carbide-based copper metal ceramic material.

[0041] Embodiment 2:

[0042] A method for preparing a silicon carbide-based copper metal ceramic material, comprising weighing 3.1 g of tetraisopropyl titanate, 1.5 g of ultrafine carbon black with an average particle size of 25 nm, and 35.5 g of a porous silicon carbide preform with a porosity of 64.5, respectively, and adding them into a beaker, slowly adding deionized water at 50° C. and 300 rpm / min to form a homogeneous gel, wherein the molar ratio of the tetraisopropyl titanate: the ultrafine carbon black: the silicon carbide is 1:1:12, and after ultrasonic treatment for 15 minutes, transferring the mixture into an oven, and drying the mixture at 105° C. to obtain a gel-modified porous silicon carbide preform;

[0043] The gel-modified porous silicon carbide preform was transferred to a sintering furnace, and heated to 1000°C at a rate of 15°C / min under a vacuum pressure of 10Pa, and then heated from 1000°C to 1350°C at a rate of 5°C / min, and kept warm for 2h; and cooled to room temperature in the furnace to obtain 37.4g of TiC0.7 modified silicon carbide preform with a porosity of 60;

[0044] Take the above-mentioned TiC0.7 modified silicon carbide porous preform, weigh 55g of copper powder pressed tablets and the above-mentioned porous preform and place them in a graphite crucible in sequence, transfer the above-mentioned graphite crucible to a vacuum sintering furnace, and under a vacuum pressure of 1Pa, heat up to 1150℃ at 5℃ / min, keep warm for 2h, and then cool with the furnace to obtain a silicon carbide-based copper metal ceramic material.

[0045] Embodiment 3:

[0046] A method for preparing a silicon carbide-based copper metal ceramic material, 3.5g of tetrabutyl titanate, 1.2g of ultrafine carbon black with an average particle size of 25nm and 35.5g of a silicon carbide ceramic membrane with a porosity of 62 are weighed and added into a beaker, 150ml of deionized water is slowly added dropwise at 50°C and 500rpm / min, stirred for 120min, then ultrasonically treated for 15min, and finally transferred to an oven and dried at 105°C to obtain a gel-modified silicon carbide ceramic membrane. The molar ratio of tetrabutyl titanate: ultrafine carbon black: silicon carbide is 1:1:10;

[0047] The gel-modified silicon carbide ceramic membrane was transferred to a sintering furnace, and under a vacuum pressure of 10 Pa, the temperature was increased to 1000°C at a rate of 15°C / min, and then increased from 1000°C to 1350°C at a rate of 5°C / min, and kept warm for 2 hours; the furnace was cooled to room temperature to obtain 37.4 g of TiC0.7 modified silicon carbide porous preform with a porosity of 55.2.

[0048] Take the above-mentioned TiC0.7 modified silicon carbide porous preform, weigh 35g of aluminum powder pressed tablets and the porous preform and place them in a graphite crucible in sequence, transfer the above-mentioned graphite crucible to a vacuum sintering furnace, and under a vacuum pressure of 1Pa, heat to 950℃ at a rate of 5℃ / min, keep warm for 2h, and then cool with the furnace to obtain a silicon carbide-based aluminum metal ceramic material.

[0049] Embodiment 4:

[0050] A method for preparing a silicon carbide-based copper metal ceramic material, 2.3g of tert-butyl titanate and 0.75g of ultrafine carbon black with an average particle size of 25nm are weighed and added to a beaker, deionized water is slowly added at 50°C and 300rpm / min to form a homogeneous gel, and 21.5g of α-SiC porous ceramic with a porosity of 59.5% is added, and the molar ratio of tert-butyl titanate: ultrafine carbon black: α-SiC porous ceramic is 1:1:10. The homogeneous gel is ultrasonically treated for 15 minutes and then transferred to an oven, and dried at 105°C to obtain a gel-modified porous silicon carbide ceramic membrane;

[0051] The gel-modified porous silicon carbide ceramic membrane was transferred to a sintering furnace, and heated to 1000°C at a rate of 15°C / min under a vacuum pressure of 5 Pa, and then heated from 1000°C to 1350°C at a rate of 5°C / min, and kept at this temperature for 2 hours, and then cooled to room temperature with the furnace to obtain a TiC0.8-modified porous silicon carbide ceramic membrane with a porosity of 45.2.

[0052] According to the size and porosity of the TiC0.8 modified porous silicon carbide ceramic membrane, the required volume of aluminum is calculated, and the appropriate mass of aluminum powder is determined by multiplying the volume of aluminum by the density of aluminum. In this embodiment, 30g of aluminum powder tablets and the above-mentioned TiC0.8 modified porous silicon carbide ceramic membrane are weighed and placed in a graphite crucible in sequence, and the graphite crucible is transferred to a vacuum sintering furnace. Under a vacuum pressure of 1Pa, the temperature is raised to 1000°C at a rate of 5°C / min, kept warm for 2h, and then cooled with the furnace to obtain a silicon carbide-based aluminum metal ceramic material.

[0053] Embodiment 5:

[0054] A method for preparing a silicon carbide-based copper metal ceramic material, 1.1g of n-butyl titanate and 0.28g of ultrafine carbon black with an average particle size of 25nm are weighed and added to a beaker, deionized water is slowly added at 50°C and 300rpm / min to form a homogeneous gel, and 26.8g of α-SiC porous ceramic with a porosity of 36.5% is added, and the molar ratio of n-butyl titanate: ultrafine carbon black: α-SiC porous ceramic is 1:1:25. The homogeneous gel is ultrasonically treated for 15 minutes and then transferred to an oven, and dried at 105°C to obtain a gel-modified porous silicon carbide ceramic membrane;

[0055] The gel-modified porous silicon carbide ceramic membrane was transferred to a sintering furnace, and heated to 1000°C at a rate of 15°C / min under a vacuum pressure of 5 Pa, and then heated from 1000°C to 1350°C at a rate of 5°C / min, and kept at this temperature for 2 hours. Then, the membrane was cooled to room temperature with the furnace, and a TiC0.5-modified porous silicon carbide ceramic membrane was obtained, 27.4 g, with a porosity of 34.8.

[0056] According to the size and porosity of the TiC0.5 modified porous silicon carbide ceramic membrane, the required volume of aluminum is calculated, and the appropriate mass of aluminum powder is determined by multiplying the volume of aluminum by the density of aluminum. In this embodiment, 16g of aluminum powder tablets and the above-mentioned TiC0.5 modified porous silicon carbide ceramic membrane are weighed and placed in a graphite crucible in sequence, and the graphite crucible is transferred to a vacuum sintering furnace. Under a vacuum pressure of 1Pa, the temperature is raised to 1000°C at a rate of 5°C / min, kept warm for 2h, and then cooled with the furnace to obtain a silicon carbide-based aluminum metal ceramic material.

Claims

1. A method for preparing a silicon carbide-based metal ceramic material, characterized in that Use the following steps: A. Weigh titanate, ultrafine carbon black and silicon carbide in a molar ratio of 1:1:10-25, put them into a beaker, slowly add deionized water under magnetic stirring until it is in a gel state to obtain modified silicon carbide, and put it into an oven for later use; B. Transfer the modified silicon carbide obtained in step A to a sintering furnace, and under vacuum conditions, first heat it to 1000° C. at a rate of 15° C. / min, then continue to heat it to 1350° C. at a rate of 5° C. / min, keep it warm for 2 hours, and then cool it to room temperature with the furnace, and take it out to obtain a porous silicon carbide preform coated with titanium carbide; C. Weigh an appropriate amount of copper powder and the porous silicon carbide preform coated with titanium carbide obtained in step B, press the weighed copper powder into a block and place it on the porous silicon carbide preform coated with titanium carbide; then transfer it to a sintering furnace, and under vacuum conditions, heat it to 1150° C. at a rate of 5° C. / min, keep it warm for 2 hours, and then cool it to room temperature with the furnace, and take it out to obtain a silicon carbide-based copper metal ceramic material.

2. The method for preparing the silicon carbide-based metal ceramic material according to claim 1, characterized in that: The titanate is one of tetra-n-butyl titanate, tetra-propyl titanate, tetra-propyl titanate, tetra-ethyl titanate, or a mixture thereof in any mass ratio.

3. The method for preparing the silicon carbide-based metal ceramic material according to claim 1, characterized in that: The average particle size of the ultrafine carbon black is ≤300nm.

4. The method for preparing the silicon carbide-based metal ceramic material according to claim 3, characterized in that: The average particle size of the ultrafine carbon black is 25 nm.

5. The method for preparing the silicon carbide-based cermet material according to claim 1, characterized in that: The vacuum condition is a pressure of less than 13.3 Pa.

6. The method for preparing the silicon carbide-based cermet material according to claim 1, characterized in that: The mass ratio of the copper powder or aluminum powder to the porous silicon carbide preform coated with titanium carbide is 0.58-2.2:

1.

7. The method for preparing the silicon carbide-based cermet material according to claim 1 or 2 or 3 or 4 or 5 or 6, characterized in that: The copper powder in step C can be replaced by aluminum powder, and the material obtained after sintering is a silicon carbide-based aluminum metal ceramic material.

8. The method for preparing the silicon carbide-based cermet material according to claim 1 or 2 or 3 or 4 or 5 or 6, characterized in that: The step A comprises: weighing titanate, ultrafine carbon black and silicon carbide in a molar ratio of 1:1:10-25, putting them into a beaker, adding a proper amount of anhydrous ethanol under magnetic stirring, stirring for 15 minutes to obtain modified silicon carbide, and putting it into an oven for standby use.

9. The method for preparing the silicon carbide-based metal ceramic material according to claim 8, characterized in that: The copper powder in step C can be replaced by aluminum powder, and the material obtained after sintering is a silicon carbide-based aluminum metal ceramic material.

10. Use of the silicon carbide-based copper metal ceramic material prepared by the method for preparing the silicon carbide-based metal ceramic material according to claims 1-9 as a high-voltage resistant metal conductor.