Thin-gauge low-yield-ratio quenched and tempered L450QS steel plate used in acid environment and manufacturing method thereof
Through specific chemical composition and manufacturing process, the problem of high yield ratio of thin-specification high-strength steel plates in acidic environments in the existing technology has been solved, and the production of high-strength steel plates with low cost, low yield ratio and excellent acid resistance has been realized to meet the needs of Demand for high-grade steel oil and gas pipelines.
Patent Information
- Application Number
- CN202411037042.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-15
AI Technical Summary
It is difficult to produce thin-sized, low-yield-ratio modified high-strength steel plates suitable for use in sour environments, especially in the field of high-grade oil and gas pipelines. The existing solutions have high costs, high hydrogen-induced cracking susceptibility to elements, and The problem that ultra-thin gauge steel plates are not suitable.
Adopting a specific chemical composition combination and manufacturing process, including C: 0.05-0.065%, Si: 0.2-0.3%, Mn: 1.25-1.30%, P≤0.010%, S≤0.002%, Cr: 0.35-0.40%, Cu :0.15-0.25%, Nb: 0.03-0.05 %, V: 0.01-0.02%, Ti: 0.008-0.015%, Al: 0.015-0.035%, B: ≤5ppm, Ca: 8-16ppm steel plate, through converter-outside furnace refining-slab casting-rolling -Quenching treatment-tempering treatment process, controlling the relationship between Ca, S, and O to optimize acid resistance.
The production yield strength in acidic environment is ≥485MPa, the tensile strength is 583-635MPa, the yield ratio is ≤0.85, the transverse impact energy at -30℃ is ≥220J, and the DWTT shear area at -15℃ is ≥90%. High-strength steel plate has both low cost and excellent resistance to HIC and SSCC, meeting the needs of high-grade steel-grade acid-resistant pipelines.
Smart Images

Figure CN118773513A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal material production, and particularly relates to a thin-gauge low-yield ratio quenched and tempered L450QS high-strength steel plate suitable for use in an acidic environment produced by using a continuous casting billet and a manufacturing method thereof. Background Art
[0002] Used to transport acidic H 2 At present, the high-grade oil and gas pipelines with S components are mainly made of TMCP (thermomechanical rolling) steel plates for the manufacture of straight seam submerged arc welded pipes. However, due to the inevitable uneven cooling problem of TMCP steel plates during the strong cooling process, local hard spots exist on the surface of the steel plates, causing the high-grade welded pipes produced with TMCP steel plates to frequently crack due to acid corrosion during operation. Quenched and tempered steel, due to its better performance uniformity, is considered to be able to replace TMCP high-grade steel plates and solve the problem of local acid corrosion cracking of steel pipes. However, for the currently common commercially available ultra-thin high-grade pipeline steel with a size of ≤12.5mm, the use of quenching and tempering process is very likely to lead to a high yield strength ratio (≥0.90), which cannot meet the actual needs of the project. Therefore, it is urgent to develop a quenched and tempered high-grade acid-resistant pipeline steel plate suitable for use in acidic environments and with a low yield strength ratio.
[0003] At present, the quenched and tempered high-grade acid-resistant steel pipes are mainly small-diameter seamless pipes, such as the disclosed CN101921964B X70QS seamless steel pipe with HIC resistance, CN101892432A manufacturing method of X70QS seamless pipeline pipe for acidic environment, CN103205648A a rare earth-containing seamless steel pipe for L450QS pipeline resistant to wet H2S corrosion and its production method, CN103215517A a rare earth-containing seamless steel pipe for L485QS pipeline resistant to wet H2S corrosion and its production method. On the one hand, these schemes are not suitable for steel plate production due to the special production method of seamless pipes; on the other hand, there are also problems such as high cost of design alloys, high hydrogen-induced cracking sensitive elements such as C and Mo. The processes described are not suitable for the production of thin-gauge high-strength steel plates used in quenched and tempered acidic environments with low yield ratio.
[0004] In terms of tempering to produce high-strength steel plates, CN115198194A discloses a method for producing low-yield ratio tempered container steel plates. Although this solution can achieve the effect of low yield ratio, the C content in the chemical composition is relatively high, and it is generally not applicable to the field of oil and gas pipelines, and it does not reflect the performance of acid resistance service; CN109112394A discloses a quenched and tempered low-yield ratio X60Q pipeline steel and a preparation method. Although this solution achieves a good low yield ratio effect, it does not reflect the applicable steel plate thickness and acid resistance. From the control requirements of hydrogen-induced crack sensitive elements such as C, Mn, P, and S in this solution, it is difficult to meet the requirements of high-strength pipeline steel for hydrogen-induced crack resistance; CN104674114A discloses a A quenched and tempered low yield ratio pipeline steel and a preparation method thereof. In this solution, C: 0.08-0.12% and Mo element are added. It is produced by a two-phase zone quenching process. Austenite stabilizing elements such as C, Mo, and Mn are easily enriched in the core of the steel plate, resulting in abnormal structure in the core of the steel plate, affecting the HIC resistance. Whether the process is applicable to thin-gauge steel plates remains to be verified; CN105441799A discloses a high-strength and low-yield ratio quenched and tempered steel plate for low-temperature environments and a manufacturing method thereof. In this solution, the Mn content reaches 1.55-1.74% and 0.18-0.25% Ni element is added. The segregation caused by high Mn and the abnormal structure in the core are likely to lead to inconsistent acid resistance of thin-gauge steel plates. In addition, the economic efficiency of this solution is not good.
[0005] In summary, among the currently disclosed schemes for thin-gauge quenched and tempered steel plates and steel pipes, on the one hand, the schemes related to seamless pipes cannot be applied to steel plate production. On the other hand, the design schemes for related low-yield ratio quenched and tempered steel plates generally have problems such as high cost, high content of hydrogen-induced cracking sensitive elements such as C and Mo, and unsuitability for extremely thin-gauge steel plates. Summary of the invention
[0006] The object of the present invention is to provide a thin-gauge low-yield ratio quenched and tempered L450QS high-strength steel plate suitable for use in an acidic environment and a manufacturing method thereof, so as to solve the problems in the prior art.
[0007] The present invention is realized by the following technical scheme: a thin-gauge low-yield ratio quenched and tempered L450QS high-strength steel plate suitable for use in an acidic environment and a manufacturing method thereof, characterized in that: the chemical composition mass percentage is: C: 0.05-0.065%, Si: 0.2-0.3%, Mn: 1.25-1.30%, P≤0.010%, S≤0.002%, Cr: 0.35-0.40%, Cu: 0.15-0.25%, Nb: 0.03-0.05%, V: 0.01-0.02%, Ti: 0.008-0.015%, Als: 0.015-0.035%, B: ≤5ppm, Ca: 8-16ppm, and (1.28*Ca-0.17*O+0.32) / S >0.6, N: ≤40ppm, H: ≤1.5ppm, O: ≤25ppm, the rest are Fe and unavoidable impurities.
[0008] The above composition range is mainly based on the following considerations: C: Carbon plays a major role in solid solution strengthening in quenched and tempered steel and has the effect of reducing the yield ratio. However, carbon is easy to segregate in steel and is also an element sensitive to hydrogen-induced cracking. Adding too much carbon is not good for acid resistance. Therefore, control C: 0.05-0.065%.
[0009] Si: Silicon is a deoxidizing element in steel and has a certain solid solution strengthening effect, which is beneficial to ensure the strength level of quenched and tempered steel plates under conditions of low carbon and low manganese. However, for high-toughness pipeline steel, too high silicon content is easy to obtain hard phase structures such as MA, which is not conducive to low-temperature toughness. Therefore, the present invention limits Si to 0.2-0.3%.
[0010] Mn: Manganese is an austenite stabilizing element that can improve the hardenability of steel. If the content is too low, it cannot meet the strength requirements of quenched and tempered high-strength steel. However, under continuous casting conditions, excessively high manganese content can easily aggravate the central segregation of the continuous casting billet and cannot be completely diffused and eliminated at high temperatures. After quenching, it is easy to form a high-hardness banded structure in the core of the steel plate, affecting the acid resistance. Therefore, this plan limits Mn to 1.25-1.30%.
[0011] P, S: Phosphorus and sulfur are harmful elements in steel. Their inclusions will become irreversible hydrogen traps to capture hydrogen entering the steel, significantly reducing the acid resistance of the steel. Theoretically, the lower the better. Considering production operability, the present invention limits P≤0.010%, S≤0.002%.
[0012] Cr: Chromium is a relatively economical strengthening element in steel. Under the premise that carbon and manganese are at a relatively low level in this scheme, increasing the chromium content can significantly improve the hardenability of the steel plate and make up for the strength loss caused by low carbon and manganese. In addition, chromium is mainly used for solid solution strengthening in steel, and high chromium also has a certain effect on improving the yield strength ratio of quenched and tempered steel. Therefore, Cr is set to 0.35-0.40%.
[0013] Cu: Copper is also an austenite stabilizing element and can also improve the hardenability of steel plates. In addition, copper can form a passivation film on the surface of steel, which to a certain extent prevents the diffusion of hydrogen into the steel and has a positive effect on improving the acid resistance of steel. In this scheme, a certain amount of copper is added, and through appropriate quenching and tempering heat treatment, the solid solution copper is precipitated during the tempering process, which has a significant effect on improving the strength of the steel plate. However, too much copper can easily lead to surface defects of continuous casting billets, especially under the condition of not using the combination of nickel elements. Therefore, the present invention limits Cu: 0.15-0.25%.
[0014] Ni, Mo: Both nickel and molybdenum are precious alloy elements. Adding large amounts of them is not economical. In this scheme, nickel and molybdenum alloys are not actively added.
[0015] Nb: Niobium is the main microalloying element added when the steel plate is produced by the controlled rolling process in the non-recrystallization zone. Since this solution is mainly for thin-gauge steel plates, the temperature reduction in the controlled rolling stage is extremely large, and the water entry temperature of the steel plate must be guaranteed. Therefore, it is necessary to expand the non-recrystallization zone of the steel by adding niobium to ensure that the second-stage rolling reduction is carried out in the non-recrystallization zone as much as possible, laying the foundation for obtaining a refined original structure before quenching and tempering. At the same time, since the steel plate of this solution adopts quenching and tempering heat treatment as the final delivery state, niobium has a certain effect of improving hardenability, but it also has a certain precipitation strengthening effect during the tempering process, resulting in an increase in the yield strength ratio, and excessive addition will also result in poor economy. Therefore, the present invention sets Nb: 0.03-0.04%.
[0016] Als, Ti: Aluminum is the main deoxidizing element in steel. Under the premise of meeting the deoxidation requirements in steel, in order to avoid the formation of large aluminum inclusions, the target is to control Als: 0.015-0.035%; Titanium in this solution mainly plays the role of grain refinement. Through micro-titanium treatment, a certain amount of fine TiN particles are formed in the steel to inhibit the growth of austenite during the heating process of the steel. However, excessive addition is prone to form large TiN inclusions, which affects the flaw detection and acid resistance of the steel plate. Therefore, the present invention sets Ti: 0.008-0.015%.
[0017] V: The addition of V in this solution mainly utilizes the effect of V combining with C, N, etc. to form precipitates to strengthen the matrix during the tempering process, which can make up for the overall strength deficiency caused by low solid solution strengthening elements in the steel to a certain extent. However, if too much is added, the significant precipitation strengthening effect will lead to a significant increase in yield strength, affecting the yield strength ratio index of the steel plate. Therefore, the present invention sets V: 0.01-0.02%.
[0018] Ca: Ca treatment is performed on inclusions to change the morphology of inclusions, producing dispersed spherical high-melting-point CaS, thereby improving acid resistance. However, through practice, if the amount of calcium wire fed into the steel is too large, that is, the Ca content is too high, large-particle calcium aluminate inclusions are easily produced in the steel, which is extremely unfavorable for acid resistance. At the same time, the yield of Ca is related to the morphology and distribution of Ca-containing inclusions and the oxygen content in the steel. Therefore, in this scheme, Ca is controlled at 8-16ppm, and Ca, S, and O in the steel satisfy the following relationship (1.28*Ca-0.17*O+0.32) / S >0.6, where the units of Ca, S, and O are ppm.
[0019] The present invention relates to a method for manufacturing a low yield ratio, thin gauge quenched and tempered L450QS high-strength steel plate suitable for use in an acidic environment. The process flow is mainly converter-external refining-slab continuous casting-rolling-quenching treatment-tempering treatment, and the main features include: 1) During the whole RH vacuum treatment, argon is used as the lifting gas. The net circulation time is ≥20 minutes at a vacuum degree of ≤40Pa. After breaking the air, the steel is taken out for sampling and chemical composition measurement. According to the S and O contents in the steel, pure calcium wire is fed in an amount of (7.5*(S+O)±30) meters. The S and O contents are brought in in ppm. The feeding speed is 150-200m / min, and Ca is controlled at 8-16ppm. The Ca, S, and O in the steel satisfy the following relationship (1.28*Ca-0.17*O+0.32) / S >0.6. After feeding the wire, the molten steel is blown clean for ≥15 minutes before being put into casting. This part is one of the core control points of the smelting process of the present invention, which is crucial to ensure the stability of the acid resistance of the steel plate. The key point is that the net cycle time under high vacuum and the net blowing time after wire feeding must meet the requirements, otherwise the large particle inclusions that have not been removed in the steel will cause a large fluctuation in the test results of hydrogen crack resistance; in addition, blindly pursuing the Ca / S requirement when the sulfur content in the steel is already at a low level can easily lead to excessive feeding of calcium wire, but not using large particle inclusion control. This scheme adopts (1.28*Ca-0.17*O+0.32) / S>0.6 instead of the traditional Ca / S requirement, which is conducive to the control of the calcium wire feeding amount and the effective calcium content in the steel, and can avoid the problem of fluctuations in acid resistance caused by insufficient or excessive calcium treatment to a certain extent.
[0020] 2) Continuous casting uses a 250*1500mm slab section, controls the superheat between 20±3℃, and a constant pulling speed of 0.95m / min. The electromagnetic stirring in the secondary cooling zone adopts a single-roll stirring mode, a stirring current of 400A, and a current frequency of 6Hz to ensure that the center segregation of the slab is ≤C1.5. The main purpose of this part is to obtain continuous casting slabs with excellent internal quality. Low superheat, constant pulling speed, relatively low current density, and high-frequency electromagnetic stirring are all beneficial to reducing the center segregation of the continuous casting slab.
[0021] 3) The billet is heated by a walking beam heating furnace, and the billet is cold loaded into the furnace. The temperature of the three heating sections is 1250-1280℃, the temperature of the soaking section is 1230-1250℃, and the total time of the billet in the furnace is ≥1.1min / mm*T (T is the thickness of the billet, in mm). The heating time of the three heating sections is controlled by (0.2-0.25)min / mm*T, and the heating time of the soaking section is controlled by (0.30-0.35)min / mm*T. The core purpose of this part is to further improve the internal quality of the billet through high-temperature heating. The cold charging furnace can refine the original austenite grains through recrystallization during the heating process; the heating temperature is set high and the total time of the billet in the furnace meets the requirements in order to ensure that the alloy elements in the steel, especially the segregation elements in the core of the continuous casting billet, can be diffused to a certain extent, and the internal chemical elements are better homogenized; the three heating and soaking time are limited in order to avoid the billet staying at high temperature for too long, resulting in excessive growth of the original austenite.
[0022] 4) In the rough rolling stage, high temperature and large reduction rolling is adopted to ensure that the reduction rate of at least 3 passes in the rough rolling is ≥20%, and the intermediate billet is 55-60mm; in the finishing rolling stage, the final rolling temperature is controlled to be 860-880℃, the ACC water inlet temperature is ≥770℃, the ACC water supply pressure is 0.2MPa, the water group adopts the front-end continuous opening mode, the number of water groups is 3-5, the upper surface water volume is 80m3 / h, the upper and lower water volume ratio is 1.5, and the final cooling temperature is 630±20℃. The rolling process focuses on microstructure refinement to prepare the steel plate for tempering. The rough rolling reduction rate of at least 3 passes with a reduction rate ≥ 20% can ensure the acquisition of finer recrystallized austenite grains. The combined control of the finishing temperature, water entry temperature, cooling water group start-up mode, and final cooling temperature of the finishing rolling process can avoid the formation of large proeutectoid ferrite in thin-gauge steel plates during the phase transformation process, and promote the rolled steel plates to obtain a uniform and fine quasi-polygonal ferrite + poor pearlite-based microstructure, laying the foundation for the uniform nucleation of austenite in the subsequent quenching and heating process.
[0023] 5) The steel plate is subjected to offline quenching + tempering treatment, in which the quenching temperature is controlled at 890-900℃, the time in the furnace is 25-30 min, and the holding time is required to be ≥5min. The steel plate is water quenched by a roller quenching machine, the water pressure in the high-pressure section of quenching is ≥0.7MPa, and the nozzle in the low-pressure section is not opened. The surface temperature of the steel plate reaches room temperature after quenching; the tempering temperature of the steel plate is 630-650℃, the time in the furnace is 35-40 min, and the holding time is required to be ≥8 min. Compared with the common two-phase zone quenching to control the yield strength ratio, this scheme adopts complete austenitization quenching and uses a high-pressure nozzle with a high cooling rate to directly quench to room temperature, which matches the chemical composition design and can obtain a quenched structure dominated by bainite, avoiding the banded structure formed by two-phase zone quenching, which is beneficial to the stability of acid resistance; the tempering process adopts a high-temperature and short-time tempering process, and obtains a relatively coarse precipitate size through high temperature, which reduces the influence of precipitation strengthening on the yield strength improvement to a certain extent. On the other hand, through short-time heat preservation, the degree of merging and coarsening of bainite lath structure is reduced, avoiding a significant reduction in matrix strength. Finally, it is ensured that the thin-gauge high-strength steel plate in the quenched and tempered state obtains a better yield strength ratio index under the premise of meeting the strength requirements.
[0024] The advantages of the present invention are as follows: the steel plate is produced by continuous casting, the thickness range is 8.8-10.2mm, and the steel plate is delivered by quenching + tempering. The yield strength of the steel plate is ≥485MPa, the tensile strength is 583-635MPa, the yield strength ratio is ≤0.85, and the transverse impact energy at -30℃ is ≥220J, and the DWTT shear area at -15℃ is ≥90%. The steel plate does not actively add precious alloy elements such as Mo and Ni, and has low cost, low yield strength ratio and excellent HIC and SSCC resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is the appearance of the continuous casting billet; Figure 2 It is the structure of 10.2mm rolled steel plate (200X); Figure 3 It is the 10.2mm quenched and tempered steel plate structure (200X). DETAILED DESCRIPTION
[0026] The invention discloses a thin-gauge low-yield ratio quenched and tempered L450QS high-strength steel plate suitable for use in an acidic environment. The steel plate comprises the following components in percentage by mass: C: 0.05-0.065%, Si: 0.2-0.3%, Mn: 1.25-1.30%, P≤0.010%, S≤0.002%, Cr: 0.35-0.40%, Cu: 0.15-0.25%, Nb: 0.03-0.05%, V: 0.01-0.02%, Ti: 0.008-0.015%, Als: 0.015-0.035%, B: ≤5ppm, Ca: 8-16ppm, N: ≤40ppm, H: ≤1.5ppm, O: ≤25ppm, and the rest are Fe and unavoidable impurities; wherein, (1.28*Ca-0.17*O+0.32) / S>0.6.
[0027] The present invention also discloses a method for manufacturing the above-mentioned low yield ratio, thin gauge quenched and tempered L450QS high-strength steel plate suitable for use in an acidic environment, comprising the steps of converter-external refining-slab continuous casting-rolling-quenching treatment-tempering treatment, wherein: 1) During the whole RH vacuum treatment, argon is used as the lifting gas. The net cycle time is ≥20 minutes at a vacuum degree of ≤40Pa. Samples are taken to measure the chemical composition. According to the S and O contents in the steel, pure calcium wire is fed in an amount of (7.5*(S+O)±30) meters. The S and O contents are brought in in ppm. The feeding speed is 150-200m / min, and Ca is controlled to be 8-16ppm, and (1.28*Ca-0.17*O+0.32) / S>0.6. After feeding the wire, the molten steel is cleanly blown for ≥15 minutes before casting on the machine; 2) Continuous casting uses a 250*1500mm slab section, controls the superheat between 20±3℃, and a constant pulling speed of 0.95m / min. The electromagnetic stirring in the secondary cooling zone adopts a single-roll stirring mode, a stirring current of 400A, and a current frequency of 6Hz to ensure that the center segregation of the slab is ≤C1.5 level; 3) The walking beam heating furnace is used for heating, and the billet is cold loaded into the furnace. The temperature of the three heating sections is 1250-1280℃, the temperature of the soaking section is 1230-1250℃, and the total time of the billet in the furnace is ≥1.1min / mm*T, of which the heating time of the three heating sections is controlled at (0.2-0.25)min / mm*T, and the heating time of the soaking section is controlled at (0.30-0.35)min / mm*T; T is the thickness of the billet, in mm; 4) In the rough rolling stage, high temperature and high pressure rolling are adopted to ensure that the reduction rate of at least 3 passes of rough rolling is ≥20%, and the intermediate billet is 55-60mm; in the finishing rolling stage, the final rolling temperature is controlled to be 860-880℃, the ACC water inlet temperature is ≥770℃, the ACC water supply pressure is 0.2MPa, the water group adopts the front-end continuous opening mode, the number of water groups is 3-5, and the upper surface water volume is 80m3 / h, upper and lower water volume ratio 1.5, final cooling temperature 630±20℃; 5) The steel plate is subjected to offline quenching + tempering treatment, wherein the quenching temperature is controlled at 890-900°C, the furnace time is 25-30 min, and the holding time is ≥5 min. The steel plate is water quenched by a roller quenching machine, the water pressure in the high-pressure section of the quenching is ≥0.7 MPa, and the nozzle in the low-pressure section is not opened. After quenching, the surface temperature of the steel plate reaches room temperature; the tempering temperature of the steel plate is 630-650°C, the furnace time is 35-40 min, and the holding time is ≥8 min.
[0028] The steel plate described in the present invention is produced by continuous casting billet, has a thickness range of 8.8-10.2mm, is delivered by quenching + tempering, has a yield strength of ≥485MPa, a tensile strength of 583-635MPa, a yield strength ratio of ≤0.85, and a transverse impact energy of ≥220J at -30°C, and a DWTT shear area of ≥90% at -15°C.
[0029] The present invention is further described below by way of examples. Example
[0030] According to the method of the present invention, 3 furnaces of 250*1500mm cross-section continuous casting billets are produced. The chemical composition of the molten steel basically meets the design requirements through converter and LF furnace treatment. Ar gas is used as circulating lifting gas in the RH treatment process. The actual RH high vacuum degree is 32-35Pa. The net cycle time under high vacuum conditions is 20-22min. After breaking the air, component samples and gas samples are taken. The amount of pure Ca wire fed is determined in combination with the S and O contents, and fine-tuned according to the actual Ca recovery and the empirical relationship between Ca, O, and S. In the actual production process, the amount of Ca wire fed is 220-250m, and the net blowing time after wire feeding is 15-17min. The specific data of the production process are as follows: Table 1 Actual smelting process of the embodiment
[0031] The continuous casting machine was used, and the superheat was controlled at 22℃, 18℃, and 21℃ respectively. The constant pulling speed was 0.95m / min. The electromagnetic stirring in the secondary cooling zone adopted a single-roll stirring mode. The stirring current was 400A, the current frequency was 6Hz, and the actual sampling slab center segregation was C1.5 level, without other internal defects. Figure 1 This is a low-magnification photograph of a continuous casting slab.
[0032] The actual chemical composition of smelting is as follows: Table 2 Actual chemical composition of the embodiment (weight percentage, wt / %)
[0033] After inspection and cleaning, the smelted billet is cold-sent to a 3.5m medium and thick plate mill for steel plate rolling. The thicknesses of the rolled steel plates are 8.8mm, 9.53mm, and 10.2mm respectively. The steel plate rolling information is as follows: Table 3 Steel plate rolling information
[0034] In order to avoid ferrite phase transformation before entering the water, the front water nozzle is continuously opened during the actual cooling process, the ACC water supply pressure is set to 0.2MPa, the number of water groups opened for 8.8, 9.53, and 10.2mm steel plates are 3, 4, and 5 respectively, the upper water volume is set to 80m3 / h, and the upper and lower water ratios are both 1.5. The rolled steel plates are subjected to quenching + tempering treatment, and the actual process execution of each steel plate is as follows: Table 4 Steel plate heat treatment information
[0035] After quenching and tempering, the steel plates were sampled and subjected to conventional performance tests such as tensile, low temperature impact, and DWTT according to API 5L standard. The specific results are as follows: Table 5 Physical properties of steel plates
[0036] As can be seen from the above, the 8.8-10.2mm thick L450QS steel plate delivered in the quenched and tempered state is produced by using 250mm thick continuous casting billet, and the yield strength of the delivered steel plate is ≥495MPa, the tensile strength is ≥583MPa, the elongation is ≥37%, the yield strength ratio is ≤0.85, the average transverse impact energy at -30℃ is ≥300J, and the DWTT shear area at -15℃ is ≥90%. It meets the requirements of L450 grade pipeline steel, especially the yield strength ratio is ≤0.93 required by API 5L standard, which has a large margin. The samples of the embodiment were subjected to HIC and SSCC tests according to NACE 0284 and NACE 0177 standards, respectively. In the HIC test, three samples were tested in each group, and three test surfaces were tested for each sample. The test crack length rate (CLR) was 0, the crack thickness rate (CTR) was 0, and the crack sensitivity rate (CSR) was 0. The SSCC test adopted the four-point bending method, and the loading stress was 80% of the actual yield strength. After 720 hours of testing, it was observed that there was no hydrogen-induced crack on the surface of the sample. The specific results are as follows: Table 6 Acid resistance of steel plates
[0037] Example 3 was sampled and tested, and the attached Figure 1-3 As shown. Among them, Figure 1The appearance photo of the continuous casting billet is a sample of Example 3. Through the implementation of the above-mentioned steelmaking and continuous casting process, a continuous casting slab with a center segregation C1.5 level and no other defects is obtained, laying the foundation for obtaining ideal organization, mechanical properties and acid resistance in the downstream rolling and heat treatment processes. Figure 2 This is Example 3, the microstructure of the 10.2 mm rolled steel plate. Through the implementation of the above rolling and cooling process, the rolled steel plate obtains a uniform and fine quasi-polygonal ferrite + poor pearlite type structure, which is prepared for the uniform nucleation of austenite during the quenching and heating process of the subsequent heat treatment process of the steel plate. Figure 3 This is Example 3, the final state of the heat-treated steel plate with a thickness of 10.2 mm, the steel plate obtains a typical tempered bainite structure, the steel plate structure is uniform and fine, and there is no obvious banded structure formed after quenching in the two-phase region, which is conducive to obtaining better acid resistance and mechanical properties.
[0038] In summary, the thickness range of the steel produced by this solution is 8.8-10.2mm, and the steel is delivered by quenching + tempering. The yield strength of the steel plate is ≥485MPa, the tensile strength is 583-635MPa, the yield strength ratio is ≤0.85, and the transverse impact energy at -30℃ is ≥220J, and the DWTT shear area at -15℃ is ≥90%. The steel plate has low cost, low yield strength ratio and excellent HIC and SSCC resistance, meeting the construction requirements of high-grade acid-resistant pipelines.
Claims
1. A thin gauge low yield ratio quenched and tempered L450QS high strength steel plate suitable for use in acidic environments, characterized by: The invention comprises the following components in mass percentage: C: 0.05-0.065%, Si: 0.2-0.3%, Mn: 1.25-1.30%, P≤0.010%, S≤0.002%, Cr: 0.35-0.40%, Cu: 0.15-0.25%, Nb: 0.03-0.05%, V: 0.01-0.02%, Ti: 0.008-0.015%, Als: 0.015-0.035%, B: ≤5ppm, Ca: 8-16ppm, N: ≤40ppm, H: ≤1.5ppm, O: ≤25ppm, and the rest are Fe and unavoidable impurities; wherein, (1.28*Ca-0.17*O+0.32) / S >0.
6.
2. The method for manufacturing a low yield ratio, thin gauge quenched and tempered L450QS high-strength steel plate suitable for use in an acidic environment according to claim 1, comprising the steps of converter - refining outside the furnace - slab continuous casting - rolling - quenching treatment - tempering treatment, characterized in that: 1) During the whole RH vacuum treatment, argon is used as the lifting gas. The net cycle time is ≥20 minutes at a vacuum degree of ≤40Pa. Samples are taken to measure the chemical composition. According to the S and O contents in the steel, pure calcium wire is fed in an amount of (7.5*(S+O)±30) meters. The S and O contents are brought in in ppm. The feeding speed is 150-200m / min, and Ca is controlled to be 8-16ppm, and (1.28*Ca-0.17*O+0.32) / S>0.
6. After feeding the wire, the molten steel is cleanly blown for ≥15 minutes before casting on the machine; 2) Continuous casting uses a 250*1500mm slab section, controls the superheat between 20±3℃, and a constant pulling speed of 0.95m / min. The electromagnetic stirring in the secondary cooling zone adopts a single-roll stirring mode, a stirring current of 400A, and a current frequency of 6Hz to ensure that the center segregation of the slab is ≤C1.5 level; 3) The walking beam heating furnace is used for heating, and the billet is cold loaded into the furnace. The temperature of the three heating sections is 1250-1280℃, the temperature of the soaking section is 1230-1250℃, and the total time of the billet in the furnace is ≥1.1min / mm*T, of which the heating time of the three heating sections is controlled at (0.2-0.25)min / mm*T, and the heating time of the soaking section is controlled at (0.30-0.35)min / mm*T; T is the thickness of the billet, in mm; 4) In the rough rolling stage, high temperature and high pressure rolling are adopted to ensure that the reduction rate of at least 3 passes of rough rolling is ≥20%, and the intermediate billet is 55-60mm; in the finishing rolling stage, the final rolling temperature is controlled to be 860-880℃, the ACC water inlet temperature is ≥770℃, the ACC water supply pressure is 0.2MPa, the water group adopts the front-end continuous opening mode, the number of water groups is 3-5, and the upper surface water volume is 80m 3 / h, upper and lower water volume ratio 1.5, final cooling temperature 630±20℃; 5) The steel plate is subjected to offline quenching + tempering treatment, wherein the quenching temperature is controlled at 890-900°C, the furnace time is 25-30 min, and the holding time is ≥5 min. The steel plate is water quenched by a roller quenching machine, the water pressure in the high-pressure section of the quenching is ≥0.7 MPa, and the nozzle in the low-pressure section is not opened. After quenching, the surface temperature of the steel plate reaches room temperature; the tempering temperature of the steel plate is 630-650°C, the furnace time is 35-40 min, and the holding time is ≥8 min.
3. The thin-gauge low-yield ratio quenched and tempered L450QS high-strength steel plate suitable for use in an acidic environment according to claim 1, characterized in that: The steel plate is produced by continuous casting billet, with a thickness range of 8.8-10.2mm and is delivered by quenching + tempering. The yield strength of the steel plate is ≥485MPa, the tensile strength is 583-635MPa, the yield strength ratio is ≤0.85, and the transverse impact energy at -30℃ is ≥220J, and the DWTT shear area at -15℃ is ≥90%.