Method for preparing high-wear-resistance and corrosion-resistance film on surface of die steel and corresponding film
By using the thermal reaction diffusion method to prepare a highly wear-resistant and corrosion-resistant (V, Cr, Nb, Ta) C quaternary medium-entropy alloy carbide film on the surface of the mold steel, the oxidation resistance and corrosion resistance of the low-entropy film in the existing technology are solved. The problem of insufficient performance is eliminated and the service life of the mold is significantly improved.
Patent Information
- Application Number
- CN202410802145.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-15
AI Technical Summary
The existing low-entropy film prepared by the thermal reaction diffusion method (TD method) on the surface of the mold steel has problems with low oxidation resistance and corrosion resistance, resulting in insufficient mold service life.
Thermal reaction diffusion method (TD method) is used to prepare highly wear-resistant and corrosion-resistant (V, Cr, Nb, Ta) C quaternary medium-entropy alloy carbide films by introducing V, Cr, Nb, Ta elements and C on the surface of the mold steel. The elements form alloy carbides, improving the film's hardness, oxidation resistance and corrosion resistance.
It significantly improves the hardness, wear resistance and oxidation resistance of the mold surface, prolongs the service life of the auto parts mold, and increases the service life by more than 3 times.
Smart Images

Figure BDA0004903679090000071
Abstract
Description
Technical Field
[0001] The invention relates to the field of metal materials and heat treatment, and in particular to preparing a highly wear-resistant and corrosion-resistant (V, Cr, Nb, Ta)C quaternary medium-entropy alloy carbide film on a die steel surface by a TD method. Background Art
[0002] In the fields of transportation and other fields, the mass production of auto parts has an increasing demand for high-performance molds. According to relevant national data, the production capacity of my country's auto parts industry chain ranks first in the world. From the perspective of my country's demand for low-carbon energy transformation, there is huge room for the development of the new energy vehicle industry in the future. Therefore, the high-performance mold industry has broad application prospects and development space. In general, the main development direction is to develop highly wear-resistant and corrosion-resistant coating film materials on the mold surface to increase the service life of the mold.
[0003] The two major factors of the mold's wear resistance and corrosion resistance basically determine its service life. In order to meet the mold's wear resistance index, high strength and hardness can ensure that the mold has high wear resistance. The preparation of high-hardness and corrosion-resistant films on the mold surface is the development direction. At present, various high-hardness films can be prepared by physical vapor deposition (PVD) and chemical vapor deposition (CVD), but the bonding force between the film and the mold steel substrate is low, which makes the film easy to peel off when the mold is working. The film prepared by the thermal reaction diffusion method (TD) has a significantly higher interface bonding force with the mold steel substrate than the film prepared by PVD and CVD, and the TD method has a low production cost and can produce large-sized and complex-shaped molds, which is conducive to production and application. However, the existing low-entropy films prepared by the TD method have low oxidation resistance and corrosion resistance.
[0004] At present, molds have been widely used in various fields of manufacturing, including transportation, but the service life of molds needs to be further improved. Based on the above situation, a TD method was developed to prepare a highly wear-resistant and corrosion-resistant (V, Cr, Nb, Ta)C quaternary medium-entropy alloy carbide film on the mold steel surface. Summary of the invention
[0005] The technical problem solved by the present invention is to provide a method for preparing a highly wear-resistant and corrosion-resistant (V, Cr, Nb, Ta)C quaternary medium-entropy alloy carbide film on the surface of mold steel by TD method, and develop a corresponding treatment process to solve the problem that the low-entropy film prepared by the existing TD method has low oxidation resistance and corrosion resistance.
[0006] The present invention discloses a method for preparing a highly wear-resistant and corrosion-resistant film on the surface of a mold steel. The film is prepared by a thermal reaction diffusion method (TD). The mass percentage of the raw material components of the formula is:
[0007] 3.0wt%~7.0wt%V2O5;
[0008] 2.0wt%~6.0wt%Cr2O3;
[0009] 4.5wt%~8.5wt%Nb2O5;
[0010] 11.0wt%~13.0wt%Ta2O5;
[0011] 8.0 wt% to 12.0 wt% Al;
[0012] The balance is Na2B4O7.
[0013] Preferably, the method for preparing a highly wear-resistant and corrosion-resistant film on the surface of mold steel comprises the following steps:
[0014] a: Put the Na2B4O7 raw material in the formula into the equipment reactor, heat it to 400°C, and keep it warm for 1 hour to dehydrate; then heat it to 900°C to obtain a molten borax bath;
[0015] b: continuing to heat the molten borax bath to 940°C - 1020°C;
[0016] c: then add the V2O5 powder raw material in the formula and stir evenly;
[0017] d: Continue to add the Cr2O3 powder raw material in the formula and stir evenly;
[0018] e: Continue to add the Nb2O5 powder raw material in the formula and stir evenly;
[0019] f: Continue to add the Ta2O5 powder raw material in the formula and stir evenly;
[0020] g: Finally, add Al in the formula and stir evenly;
[0021] h: Put the Cr12 and Cr12MoV die steels into the borax molten bath in step g and keep them warm for 4-6 hours, then take them out and directly oil-quench them, and then temper them twice at 180°C.
[0022] Preferably, steps c to g require uniform stirring of the molten borax bath to avoid as much as possible the segregation of chemical components in the borax bath from adversely affecting the quaternary medium entropy carbide layer prepared later.
[0023] Preferably, the mold steel described in step h is Cr12, Cr12MoV high carbon steel.
[0024] Preferably, the die steel described in step h is subjected to forging, spheroidizing annealing and machining treatment, the forging heating temperature is 1180°C to 1250°C, the forging temperature is 1000°C to 1200°C, and the dynamic recrystallization is fully utilized to refine the grain size of the Cr12 and Cr12MoV die steel forging billets during the forging process.
[0025] Preferably, the spheroidizing annealing heating temperature in step h is 850°C to 900°C. After being kept at the above temperature for 2 hours, the steel is cooled to 730°C to 760°C with the furnace and kept for 4 hours. Then, the steel is cooled to below 450°C in the furnace and air-cooled. Spheroidizing annealing can eliminate forging stress, refine grains, and obtain granular pearlite structure, thus preparing the structure for subsequent mold machining and heat treatment.
[0026] The present invention also includes a film, which is prepared by adopting the above method for preparing a highly wear-resistant and corrosion-resistant film on the surface of mold steel.
[0027] The present invention provides a method for preparing a highly wear-resistant and corrosion-resistant (V, Cr, Nb, Ta)C quaternary medium-entropy alloy carbide film on a mold steel surface by a TD method, namely a thermal reaction diffusion method (TD method). The raw material components include: 3.0wt% to 7.0wt% V2O5; 2.0wt% to 6.0wt% Cr2O3; 4.5wt% to 8.5wt% Nb2O5; 11.0wt% to 13.0wt% Ta2O5; 8.0wt% to 12.0wt% Al; and the balance is Na2B4O7. The V, Cr, Nb, and Ta elements in the raw materials diffuse to the surfaces of mold steels such as Cr12 and Cr12MoV in a molten borax bath, and form a (V, Cr, Nb, Ta) C quaternary medium-entropy alloy carbide film on the mold steel surface with the C element in the steel, which has high hardness, high wear resistance and high corrosion resistance. The (V, Cr, Nb, Ta) C quaternary medium-entropy alloy carbide film is well combined with the mold steel matrix. The V and Nb elements ensure the high hardness of the film, while the Cr element ensures the oxidation resistance and corrosion resistance. The introduction of the Ta element can significantly improve the surface roughness and quality of the carbide film. The four elements are added simultaneously to form a medium-entropy alloy, which comprehensively improves various properties. The method for preparing a highly wear-resistant and corrosion-resistant (V, Cr, Nb, Ta) C quaternary medium-entropy alloy carbide film on the mold steel surface by the TD method disclosed by the present invention can be applied to the fields of mold manufacturing, and exhibits good comprehensive performance during use, significantly improving the service life of molds such as automotive parts. Experiments have shown that the TD method for preparing a highly wear-resistant and corrosion-resistant (V, Cr, Nb, Ta)C quaternary medium-entropy alloy carbide film on the surface of the mold steel involved in the present invention has a mold surface hardness of 2000-2700 HV after surface treatment with the (V, Cr, Nb, Ta)C quaternary medium-entropy alloy carbide film, and the wear resistance, oxidation resistance and corrosion resistance are significantly improved, and the service life of the automotive parts mold is increased by more than 3 times.
[0028] Specific implementation method
[0029] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0030] The introduction of V and Nb elements into carbide films is conducive to obtaining high-hardness films. The introduction of Cr elements can effectively improve the film's oxidation resistance and corrosion resistance, and the introduction of Ta elements can significantly improve the surface roughness and quality of carbide films. The four elements are added simultaneously to form medium-entropy alloy carbides, which comprehensively improves various properties. Therefore, the preparation of (V, Cr, Nb, Ta) C quaternary medium-entropy carbide films can obtain high wear resistance and corrosion resistance. In recent years, research on high-entropy alloys and medium-entropy alloys has shown that multi-chemical composition films have better performance than single films. Therefore, developing high-wear-resistant and corrosion-resistant (V, Cr, Nb, Ta) C quaternary medium-entropy alloy carbide films with independent intellectual property rights, high quality, and long life on the surface of mold steel can significantly improve the service life of the mold, have significant economic and social benefits, and have important significance in theory and engineering.
[0031] The embodiment of the present invention discloses a method for preparing a highly wear-resistant and corrosion-resistant film on the surface of a mold steel, and more specifically, a method for preparing a highly wear-resistant and corrosion-resistant (V, Cr, Nb, Ta)C quaternary medium-entropy alloy carbide film on the surface of a mold steel by a TD method, namely, a thermal reaction diffusion method (TD method), and the mass percentage of the raw materials in the formula is: 3.0wt%~7.0wt% V2O5; 2.0wt%~6.0wt% Cr2O3; 4.5wt%~8.5wt% Nb2O5; 11.0wt%~13.0wt% Ta2O5; 8.0wt%~12.0wt% Al; the balance is Na2B4O7.
[0032] In the method for preparing a highly wear-resistant and corrosion-resistant film on the surface of a mold steel, the temperature of the molten borax bath is 940°C-1020°C, and the temperature is kept for 4-6 hours. In order to further understand the present invention, the following is a detailed introduction to the preparation of a (V, Cr, Nb, Ta) C quaternary medium entropy alloy carbide film on the surface of a mold steel of high carbon steel such as Cr12 and Cr12MoV provided by the present invention in combination with the embodiments. If the carbon content in the mold steel is low, it may affect the hardness and other properties of the carbide film. The protection scope of the present invention is not limited by the following embodiments.
[0033] Example 1.
[0034] (1) The raw material formula is as follows: 4.0wt% V2O5; 4.0wt% Cr2O3; 5.0wt% Nb2O5; 11.0wt% Ta; 9.0wt% Al; the balance is Na2B4O7.
[0035] (2) placing the Na2B4O7 raw material in the formula into the equipment reactor, heating it to 400°C, and keeping it warm for 1 hour to dehydrate it; then heating it to 900°C to obtain a molten borax bath;
[0036] (3) continuing to heat the molten borax bath to 940° C.;
[0037] (4) Add the V2O5 powder raw material in the formula and stir evenly;
[0038] (5) Add the Cr2O3 powder raw material in the formula and stir evenly;
[0039] (6) Add the Nb2O5 powder raw material in the formula and stir evenly;
[0040] (7) Add the Ta2O5 powder raw material in the formula and stir evenly;
[0041] (8) Finally, add Al in the formula and stir evenly;
[0042] (9) The Cr12MoV die steel was placed in the borax molten bath and kept warm for 4 h, then taken out and directly oil-quenched, and then tempered twice at 180°C.
[0043] The surface of the Cr12MoV mold steel prepared according to the above method was tested for microhardness. The results are shown in Table 1.
[0044] Preferably, the die steel in (9) is forged, spheroidized annealed and machined, the forging heating temperature is 1180°C to 1250°C, the forging temperature is 1000°C to 1200°C, and the dynamic recrystallization is fully utilized to refine the grain size of the Cr12 and Cr12MoV die steel forging billets during the forging process.
[0045] Among them, the spheroidizing annealing heating temperature is 850℃~900℃. After being kept at the above temperature for 2h, it is cooled to 730℃~760℃ with the furnace and kept for 4h, and then continued to be furnace cooled to below 450℃ before being air-cooled. Spheroidizing annealing can eliminate forging stress, refine grains, and obtain granular pearlite structure, so as to prepare the structure for subsequent mold machining and heat treatment.
[0046] Example 2
[0047] (1) The raw material formula is as follows: 5.0wt% V2O5; 4.0wt% Cr2O3; 6.0wt% Nb2O5; 12.0wt% Ta; 10.0wt% Al; the balance is Na2B4O7.
[0048] (2) placing the Na2B4O7 raw material in the formula into the equipment reactor, heating it to 400°C, and keeping it warm for 1 hour to dehydrate it; then heating it to 900°C to obtain a molten borax bath;
[0049] (3) continuing to heat the molten borax bath to 960° C.;
[0050] (4) Add the V2O5 powder raw material in the formula and stir evenly;
[0051] (5) Add the Cr2O3 powder raw material in the formula and stir evenly;
[0052] (6) Add the Nb2O5 powder raw material in the formula and stir evenly;
[0053] (7) Add the Ta2O5 powder raw material in the formula and stir evenly;
[0054] (8) Finally, add Al in the formula and stir evenly;
[0055] (9) The Cr12MoV die steel was placed in the borax molten bath described in (8) and kept warm for 5 h. It was then taken out and directly oil-quenched and then tempered twice at 180 °C.
[0056] The surface of the Cr12MoV mold steel prepared according to the above method was tested for microhardness. The results are shown in Table 1.
[0057] Example 3
[0058] (1) The raw material formula is as follows: 6.0wt% V2O5; 4.0wt% Cr2O3; 7.0wt% Nb2O5; 12.0wt% Ta; 10.0wt% Al; the balance is Na2B4O7.
[0059] (2) placing the Na2B4O7 raw material in the formula into the equipment reactor, heating it to 400°C, and keeping it warm for 1 hour to dehydrate it; then heating it to 900°C to obtain a molten borax bath;
[0060] (3) continuing to heat the molten borax bath to 960° C.;
[0061] (4) Add the V2O5 powder raw material in the formula and stir evenly;
[0062] (5) Add the Cr2O3 powder raw material in the formula and stir evenly;
[0063] (6) Add the Nb2O5 powder raw material in the formula and stir evenly;
[0064] (7) Add the Ta2O5 powder raw material in the formula and stir evenly;
[0065] (8) Finally, add Al in the formula and stir evenly;
[0066] (9) The Cr12MoV die steel was placed in the borax molten bath and kept warm for 5 hours, then taken out and directly oil-quenched, and then tempered twice at 180°C.
[0067] The surface of the Cr12MoV mold steel prepared according to the above method was tested for microhardness. The results are shown in Table 1.
[0068] Example 4
[0069] (1) The raw material formula is as follows: 6.5wt% V2O5; 3.0wt% Cr2O3; 7.5wt% Nb2O5; 11.0wt% Ta; 10.0wt% Al; the balance is Na2B4O7.
[0070] (2) placing the Na2B4O7 raw material in the formula into the equipment reactor, heating it to 400°C, and keeping it warm for 1 hour to dehydrate it; then heating it to 900°C to obtain a molten borax bath;
[0071] (3) continuing to heat the molten borax bath to 970° C.;
[0072] (4) Add the V2O5 powder raw material in the formula and stir evenly;
[0073] (5) Add the Cr2O3 powder raw material in the formula and stir evenly;
[0074] (6) Add the Nb2O5 powder raw material in the formula and stir evenly;
[0075] (7) Add the Ta2O5 powder raw material in the formula and stir evenly;
[0076] (8) Finally, add Al in the formula and stir evenly;
[0077] (9) The Cr12MoV die steel was placed in the borax molten bath and kept warm for 6 hours, then taken out and directly oil-quenched, and then tempered twice at 180°C.
[0078] The surface of the Cr12MoV mold steel prepared according to the above method was tested for microhardness. The results are shown in Table 1.
[0079] Example 5
[0080] (1) The raw material formula is as follows: 5.0wt% V2O5; 3.0wt% Cr2O3; 6.5wt% Nb2O5; 11.0wt% Ta; 10.0wt% Al; the balance is Na2B4O7.
[0081] (2) placing the Na2B4O7 raw material in the formula into the equipment reactor, heating it to 400°C, and keeping it warm for 1 hour to dehydrate it; then heating it to 900°C to obtain a molten borax bath;
[0082] (3) continuing to heat the molten borax bath to 980° C.;
[0083] (4) Add the V2O5 powder raw material in the formula and stir evenly;
[0084] (5) Add the Cr2O3 powder raw material in the formula and stir evenly;
[0085] (6) Add the Nb2O5 powder raw material in the formula and stir evenly;
[0086] (7) Add the Ta2O5 powder raw material in the formula and stir evenly;
[0087] (8) Finally, add Al in the formula and stir evenly;
[0088] (9) The Cr12MoV die steel was placed in the borax molten bath and kept warm for 4 h, then taken out and directly oil-quenched, and then tempered twice at 180°C.
[0089] The surface of the Cr12MoV mold steel prepared according to the above method was tested for microhardness. The results are shown in Table 1.
[0090] Example 6
[0091] (1) The raw material formula is as follows: 4.0wt% V2O5; 4.0wt% Cr2O3; 6.0wt% Nb2O5; 11.0wt% Ta; 10.0wt% Al; the balance is Na2B4O7.
[0092] (2) placing the Na2B4O7 raw material in the formula into the equipment reactor, heating it to 400°C, and keeping it warm for 1 hour to dehydrate it; then heating it to 900°C to obtain a molten borax bath;
[0093] (3) continuing to heat the molten borax bath to 1000° C.;
[0094] (4) Add the V2O5 powder raw material in the formula and stir evenly;
[0095] (5) Add the Cr2O3 powder raw material in the formula and stir evenly;
[0096] (6) Add the Nb2O5 powder raw material in the formula and stir evenly;
[0097] (7) Add the Ta2O5 powder raw material in the formula and stir evenly;
[0098] (8) Finally, add Al in the formula and stir evenly;
[0099] (9) The Cr12MoV die steel was placed in the borax molten bath and kept warm for 4 h, then taken out and directly oil-quenched, and then tempered twice at 180°C.
[0100] The surface of the Cr12MoV mold steel prepared according to the above method was tested for microhardness. The results are shown in Table 1.
[0101] Table 1 Hardness test results of quaternary medium entropy alloy carbide film prepared on the surface of Cr12MoV die steel in Example
[0102]
[0103] It can be seen from Table 1 that the (V, Cr, Nb, Ta)C quaternary medium entropy alloy carbide film prepared on the surface of Cr12MoV mold steel by the thermal reaction diffusion method (TD) provided by the present invention has high hardness and wear resistance, and is suitable for thin film formation treatment on the surface of high carbon mold steel.
[0104] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0105] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a highly wear-resistant and corrosion-resistant film on the surface of mold steel, characterized in that: The film was prepared by thermal reaction diffusion method (TD), and the mass percentage of the raw material components of the formula was: 3.0wt%~7.0wt%V2O5; 2.0wt%~6.0wt%Cr2O3; 4.5wt%~8.5wt%Nb2O5; 11.0wt%~13.0wt%Ta2O5; 8.0 wt% to 12.0 wt% Al; The balance is Na2B4O7.
2. The method for preparing a highly wear-resistant and corrosion-resistant film on the surface of mold steel according to claim 1, characterized in that: The following steps are involved: a: Put the Na2B4O7 raw material in the formula into the equipment reactor, heat it to 400°C, and keep it warm for 1 hour to dehydrate; then heat it to 900°C to obtain a molten borax bath; b: continuing to heat the molten borax bath to 940°C - 1020°C; c: then add the V2O5 powder raw material in the formula and stir evenly; d: Continue to add the Cr2O3 powder raw material in the formula and stir evenly; e: Continue to add the Nb2O5 powder raw material in the formula and stir evenly; f: Continue to add the Ta2O5 powder raw material in the formula and stir evenly; g: Finally, add Al in the formula and stir evenly; h: Put the Cr12 and Cr12MoV die steels into the borax molten bath in step g and keep them warm for 4-6 hours, then take them out and directly oil-quench them, and then temper them twice at 180°C.
3. The method for preparing a highly wear-resistant and corrosion-resistant film on the surface of mold steel according to claim 2, characterized in that: Steps c to g require uniform stirring of the molten borax bath to avoid the segregation of chemical components in the borax bath from adversely affecting the quaternary medium-entropy carbide layer prepared later.
4. The method for preparing a highly wear-resistant and corrosion-resistant film on the surface of mold steel according to claim 2, characterized in that: The mold steel described in step h is Cr12, Cr12MoV high carbon steel.
5. The method for preparing a highly wear-resistant and corrosion-resistant film on the surface of mold steel according to claim 2, characterized in that: The die steel described in step h is forged, spheroidized annealed and machined, the forging heating temperature is 1180°C to 1250°C, the forging temperature is 1000°C to 1200°C, and the dynamic recrystallization is fully utilized to refine the grain size of the Cr12 and Cr12MoV die steel forging billets during the forging process.
6. The method for preparing a highly wear-resistant and corrosion-resistant film on the surface of mold steel according to claim 2, characterized in that: The spheroidizing annealing heating temperature described in step h is 850°C to 900°C. After being kept at the above temperature for 2 hours, it is cooled to 730°C to 760°C with the furnace and kept for 4 hours. Then it is continued to be furnace cooled to below 450°C before being air-cooled. Spheroidizing annealing can eliminate forging stress, refine grains, and obtain granular pearlite structure, which prepares the structure for subsequent mold machining and heat treatment.
7. A film, characterized in that: The film is prepared by the method for preparing a highly wear-resistant and corrosion-resistant film on the surface of mold steel as described in any one of claims 1 to 6.
Citation Information
Patent Citations
Surface strengthening treatment method for car friction plate hot-press forming die
CN108359930A
Metal workpiece with vanadium-niobium impregnated surface using borax molten salt as carrier and production method thereof
CN1876887A