Mo film and preparation method and application thereof
By using a butterfly valve in the deposition chamber to adjust the sputtering deposition pressure, low-flow high-pressure sputtering is achieved to prepare Mo films, which solves the problem of high process gas consumption in the high-pressure coating process, reduces costs, and improves the uniformity and electrical properties of the film. performance.
Patent Information
- Application Number
- CN202310356955.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-10-15
AI Technical Summary
In the large-area coating process, when Mo thin films are prepared by high-pressure sputtering deposition, the consumption of process gases increases significantly, resulting in high costs.
By using a butterfly valve in the deposition chamber to accurately control the sputtering deposition gas pressure, Mo thin films can be prepared by high-pressure sputtering with a lower flow rate of process gas, reducing process costs.
Significantly saving 0-80% of process gas consumption, the prepared Mo film has a uniform surface, excellent electrical properties, and the thickness, structure and performance are consistent with those under high-flow process conditions.
Smart Images

Figure CN118773541A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of thin-film solar cells, and in particular relates to a Mo thin film and a preparation method and application thereof. Background Art
[0002] Molybdenum (Mo) metal has a high melting point, high high temperature strength, hardness and rigidity, good thermal shock resistance, thermal conductivity and electrical conductivity. Mo thin film also has good electrical conductivity, thermal stability, chemical stability and high infrared reflectivity, and can be widely used in thin film solar cells, liquid crystal displays and microelectronics. The main technologies for preparing Mo thin films include precision turning, precision rolling, physical vapor deposition, electron beam evaporation, etc. Among them, the Mo thin film prepared by magnetron sputtering has high purity, low surface roughness, good thickness uniformity, high electrical conductivity, strong bonding with the substrate, and is widely used. At present, in order to realize high-pressure sputtering deposition to prepare high-pressure Mo thin film, the method of increasing the flow rate of the process gas to increase the deposition pressure is usually adopted. This method consumes a large amount of process gas, especially in large-area coating processes, and there is a problem of significantly increased sputtering process gas consumption. Summary of the invention
[0003] The purpose of the present disclosure is to provide a Mo film and a preparation method thereof. The Mo film prepared by the present invention has a uniform surface and excellent electrical properties. Compared with other Mo films prepared under conditions of higher flow rate process gas, the Mo film is consistent in thickness, structure and performance. The preparation method of the present invention uses a butterfly valve to accurately control the sputtering deposition gas pressure in the deposition chamber, so as to realize the preparation of the Mo film by high-pressure sputtering with a lower flow rate process gas, thereby significantly reducing the process cost.
[0004] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a Mo thin film, wherein the method comprises:
[0005] Introducing process gas into the deposition chamber to cause the substrate to be sputter-deposited in the deposition chamber to form a Mo film on the surface of the substrate;
[0006] The ratio of the flow rate of the process gas to the volume of the deposition chamber is 0.1-4 sccm / L, and the deposition pressure of the sputtering deposition is controlled by a butterfly valve arranged on the chamber wall of the deposition chamber, and the deposition pressure is 0.5-10 Pa.
[0007] Optionally, the sputtering deposition includes: fixing the target material and moving the substrate linearly and reciprocatingly continuously in the deposition chamber.
[0008] The speed of the linear reciprocating continuous movement is 0.5-6 m / min.
[0009] Optionally, the method comprises the following steps:
[0010] (1) ultrasonically cleaning the substrate in alkaline detergent aqueous solution, ethanol aqueous solution and ultrapure water in sequence and drying the substrate, then sending the cleaned substrate into a sample injection chamber for evacuation, and then transferring the substrate into the deposition chamber;
[0011] (2) When the vacuum degree of the deposition chamber reaches the critical vacuum degree, Ar gas is introduced, and the deposition gas pressure is adjusted to the first pressure by using a butterfly valve, and the target gun power is increased to 400W to 800W for ignition;
[0012] (3) adjusting the Ar gas flow rate and using a butterfly valve to adjust the deposition gas pressure to a second pressure so that the substrate is sputtered and deposited a desired number of times;
[0013] (4) reducing the target gun power, stopping the introduction of Ar gas, and taking out the substrate when the vacuum degree of the deposition chamber reaches the critical vacuum degree;
[0014] The critical vacuum degree is 2×10 -5 ~5×10 -3 Pa.
[0015] Optionally, in step (1), the alkaline detergent aqueous solution includes one or more of calcium bicarbonate, sodium carbonate, and sodium hydroxide; the cleaning time is 5 to 30 minutes;
[0016] The vacuum pumping is performed until the vacuum degree of the injection chamber reaches 2×10 -5 ~5×10 -3 Pa.
[0017] Optionally, in step (2), the ratio of the flow rate of the Ar gas to the volume of the deposition chamber is 0.1 to 4 sccm / L, and the first pressure is 1.0 to 6.0 Pa.
[0018] Optionally, in step (3), the ratio of the flow rate of the Ar gas to the volume of the deposition chamber is 0.1 to 4 sccm / L, the second pressure is 0.1 to 3.0 Pa, and the required number of times is 10 to 50 times.
[0019] Optionally, the butterfly valve is arranged on the top wall of the deposition chamber, and a vacuum pump is connected to the outer side of the butterfly valve.
[0020] The second aspect of the present invention provides a Mo film prepared by the method described in the first aspect of the present invention.
[0021] Optionally, the thickness of the Mo film is 50-1000 nm; the sheet resistance of the Mo film is 0.5-5Ω / □, the conductivity of the Mo film is 5000-50000 S / cm; the XRD spectrum of the Mo film has a characteristic peak at 40-41.5°.
[0022] The third aspect of the present invention provides use of the Mo thin film according to the second aspect of the present disclosure in thin-film solar cells, liquid crystal displays or microelectronics.
[0023] Through the above technical scheme, the present invention accurately controls the sputtering deposition gas pressure through a butterfly valve to achieve high-pressure sputtering preparation of Mo film with a relatively low flow rate of process gas, which can save 0 to 80% of process gas consumption and significantly reduce process costs. The prepared Mo film has a uniform surface, has preferential orientation growth on the (110) crystal plane, and has excellent electrical properties. Compared with other Mo films prepared under higher flow rate process gas conditions, the thickness, film uniformity, crystal quality and electrical properties are consistent.
[0024] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings:
[0026] Figure 1 It is a schematic diagram of the internal structure of a deposition chamber of a magnetron sputtering deposition device in one embodiment of the present invention.
[0027] Figure 2 This is the SEM image of the Mo film prepared in Example 1 of the present invention.
[0028] Figure 3 This is the XRD pattern of the Mo film prepared in Example 1 of the present invention.
[0029] Description of Reference Numerals
[0030] 1-vacuum pump, 2-butterfly valve, 3-deposition chamber, 4-substrate, 5-target, 6-air inlet DETAILED DESCRIPTION
[0031] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.
[0032] A first aspect of the present invention provides a method for preparing a Mo thin film, wherein the method comprises:
[0033] Introducing process gas into the deposition chamber to cause the substrate to be sputter-deposited in the deposition chamber to form a Mo film on the surface of the substrate;
[0034] Among them, the ratio of the flow rate of the process gas to the volume of the deposition chamber is 0.1~4sccm / L, preferably 0.1~1sccm / L, and the deposition gas pressure of the sputtering deposition is controlled by a butterfly valve arranged on the wall of the deposition chamber, and the deposition gas pressure is 0.5~10Pa, preferably 1~3Pa.
[0035] The preparation method of the present invention uses a butterfly valve to accurately control the sputtering deposition gas pressure, thereby realizing high-pressure sputtering preparation of Mo thin films with a relatively low flow rate of process gas, which can save 0-80% of process gas consumption and significantly reduce process costs.
[0036] In a specific embodiment of the present invention, the sputtering deposition includes: fixing the target material and moving the substrate linearly and reciprocatingly continuously within the deposition chamber;
[0037] The speed of the linear reciprocating continuous movement is 0.5-6 m / min, preferably 1-3 m / min. In the present invention, by accurately adjusting the speed of the substrate reciprocating movement, the Mo particles reach the (110) crystal plane nucleation energy threshold when they reach the substrate, and the film grains achieve (110) crystal plane preferred orientation growth.
[0038] In a specific embodiment of the present invention, the preparation method comprises the following steps:
[0039] (1) ultrasonically cleaning the substrate in alkaline detergent aqueous solution, ethanol aqueous solution and ultrapure water in sequence and drying the substrate, then sending the cleaned substrate into a sample injection chamber for evacuation, and then transferring the substrate into the deposition chamber;
[0040] (2) When the vacuum degree of the deposition chamber reaches the critical vacuum degree, Ar gas is introduced, and the deposition gas pressure is adjusted to the first pressure by using a butterfly valve, and the target gun power is increased to 400W to 800W for ignition;
[0041] (3) adjusting the Ar gas flow rate and using a butterfly valve to adjust the deposition gas pressure to a second pressure so that the substrate is sputtered and deposited a desired number of times;
[0042] (4) reducing the target gun power, stopping the introduction of Ar gas, and taking out the substrate when the vacuum degree of the deposition chamber reaches the critical vacuum degree;
[0043] The critical vacuum degree is 2×10 -5 ~5×10 -3 Pa, preferably 2×10 -5 ~5×10 -4 Pa.
[0044] In a specific embodiment of the present invention, in step (1), the alkaline detergent aqueous solution includes one or more of calcium bicarbonate, sodium carbonate, and sodium hydroxide, preferably sodium carbonate; the cleaning time is 5 to 30 minutes, preferably 20 to 30 minutes;
[0045] The vacuum pumping is performed until the vacuum degree of the injection chamber reaches 2×10 -5 ~5×10 -3 Pa, preferably 2×10 -5 ~5×10 -4 Pa.
[0046] In a specific embodiment of the present invention, in step (2), the ratio of the flow rate of the Ar gas to the volume of the deposition chamber is 0.1 to 4 sccm / L, preferably 0.5 to 1 sccm / L, and the first pressure is 1.0 to 6.0 Pa, preferably 5 to 6 Pa.
[0047] In a specific embodiment of the present invention, in step (3), the ratio of the flow rate of the Ar gas to the volume of the deposition chamber is 0.1 to 4 sccm / L, preferably 0.1 to 1 sccm / L, the second pressure is 0.1 to 3.0 Pa, preferably 1 to 2 Pa, and the required number of times is 10 to 50 times, preferably 20 to 30 times.
[0048] In a specific embodiment of the present invention, the butterfly valve is arranged on the top wall of the deposition chamber, and a vacuum pump is connected to the outside of the butterfly valve. By adjusting the opening of the butterfly valve, the pumping speed of the vacuum pump can be controlled, thereby controlling the air pressure in the deposition chamber.
[0049] In a specific embodiment of the present invention, the deposition chamber 3 is provided with a vacuum pump 1, a butterfly valve 2, a substrate 4, a target material 5 and an Ar gas inlet 6, wherein the substrate 3 is arranged in the middle of the deposition chamber, the target material 4 and the gas inlet are arranged on the bottom wall of the deposition chamber, and the gas inlet is located on both sides of the target material. The specific structural diagram of the deposition chamber is as shown in FIG. Figure 1 shown.
[0050] The second aspect of the present invention provides a Mo film prepared by the method described in the first aspect of the present invention.
[0051] The Mo film prepared by the present invention has a uniform surface and excellent electrical properties. Compared with Mo films prepared under other conditions of higher flow process gas, the Mo film has the same thickness, film uniformity, crystal quality and electrical properties.
[0052] In a specific embodiment of the present invention, the thickness of the Mo film is 50 to 1000 nm, preferably 200 to 400 nm; the sheet resistance of the Mo film is 0.5 to 5 Ω / □, preferably 1 to 3 Ω / □, the conductivity of the Mo film is 5000 to 50000 S / cm, preferably 10000 to 20000 S / cm; the XRD spectrum of the Mo film has a characteristic peak at 40 to 41.5°.
[0053] In the present invention, the characteristic peak at 40-41.5° is the peak position of the (110) crystal plane.
[0054] In the present invention, the Mo film preferentially grown on the (110) crystal plane can be used as an excellent substrate for multilayer Mo films or other thin films such as CIGS, Al, and Ti. When used as a CIGS battery electrode, CIGS is grown on the (110) Mo surface, which is more likely to react to form a MoSe2 intermediate layer, which is beneficial to improving battery performance.
[0055] The third aspect of the present invention provides use of the Mo thin film described in the second aspect of the present disclosure in thin-film solar cells, liquid crystal displays or microelectronics.
[0056] The present invention is further illustrated by the following examples, but the present invention is not limited thereto.
[0057] The sputtering coating equipment used is a customized SYSKEY INLINE model. The purity of the Mo metal target is 99.95%, and the purity of the argon gas is above 99.95%.
[0058] Example 1
[0059] a. Cut the glass substrate into substrates of 30 cm × 30 cm in size using a glass cutter, and ultrasonically clean them in sodium carbonate solution, ethanol aqueous solution, and ultrapure water for 30 minutes respectively, and then blow dry or bake them;
[0060] b. Load the substrate into the sample chamber and evacuate it. When the vacuum degree of the sample chamber reaches 6.0 Pa, transfer it into the deposition chamber and evacuate it.
[0061] The vacuum degree of the deposition chamber reaches 2.0×10 -4 At 1.5 Pa, 0.5 sccm / L Ar gas was introduced, and the deposition gas pressure was adjusted to 6.0 Pa by a butterfly valve. The target gun power was gradually increased to 800 W at a rate of 50 W / s.
[0062] d. Adjust the flow rate of Ar gas to 0.27 sccm / L, use the butterfly valve to adjust the deposition gas pressure to 1.3 Pa, start coating, and make the substrate move linearly back and forth in the deposition chamber for 25 times at a continuous moving speed of 2.5 m / min.
[0063] After the coating is completed, the target gun power is reduced to 0W at 50W / s, and the Ar gas is stopped. The vacuum degree of the deposition chamber is pumped to 2.0×10 -4 When φ Pa, the substrate is transferred to the sample injection chamber, and the substrate and film are taken out.
[0064] Example 2
[0065] The method of Example 1 is adopted, except that the continuous moving speed in step d is 8.0 m / min.
[0066] Comparative Example 1
[0067] The method of Example 1 is adopted, except that the flow rate of Ar gas in step d is 1.5 sccm / L, the butterfly valve is fully opened, a normal pumping speed is adopted, and the pressure of the deposition chamber floats between 1.2-1.3 Pa.
[0068] Test Case
[0069] The Mo films of Examples 1-2 and Comparative Example 1 were tested as follows:
[0070] The thickness of the Mo film was tested using a German Bruker Dektak-XT step profiler, and the sheet resistance of the Mo film was measured using an American JANDEL RM3000 four-probe tester. The conductivity was calculated using the following formula: resistivity = sheet resistance × film thickness, conductivity = 1 / resistivity.
[0071] The results are shown in Table 1. The surface SEM image of the Mo film of Example 1 is as follows: Figure 2 (a) and Figure 2 (b) shows the cross-sectional SEM image. Figure 2 (c) shows the XRD pattern of the film. Figure 3 shown.
[0072] Table 1
[0073]
[0074] According to the test results in Table 1, it can be seen that the preparation method provided by the present invention, compared with the comparative example, adopts a butterfly valve to dynamically adjust the gas pressure in the deposition chamber, can accurately control the gas pressure, make it fluctuate within a very small range, and realize the preparation of Mo thin film by high-pressure sputtering with a relatively low flow rate of process gas, which significantly reduces the process cost, and the prepared Mo thin film is consistent in thickness, film uniformity, crystal quality and electrical properties.
[0075] From the comparison of the test results of Examples 1 and 2, it can be seen that when the movement speed of the sputtering deposition substrate is within the preferred range defined by the present invention, the effect and performance of the product prepared by the present invention can be further improved. The prepared Mo film preferentially grows on the (110) crystal plane and can be used as an excellent substrate for other thin films such as multilayer Mo films and CIGS.
[0076] From the test results of Comparative Example 1, it can be seen that Comparative Example 1 does not use a butterfly valve for adjustment, and a higher process gas flow rate is required to achieve high-pressure sputtering deposition of Mo film. A large amount of process gas is consumed in the large-area coating process, and the process cost is significantly increased.
[0077] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0078] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0079] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for preparing a Mo thin film, wherein: The method includes: Introducing process gas into the deposition chamber to cause the substrate to be sputter-deposited in the deposition chamber to form a Mo film on the surface of the substrate; The ratio of the flow rate of the process gas to the volume of the deposition chamber is 0.1-4 sccm / L, and the deposition pressure of the sputtering deposition is controlled by a butterfly valve arranged on the wall of the deposition chamber, and the deposition pressure is 0.5-10 Pa.
2. The method according to claim 1, wherein: The sputtering deposition comprises: fixing the target material and moving the substrate linearly and reciprocatingly and continuously in the deposition chamber; The speed of the linear reciprocating continuous movement is 0.5-6 m / min.
3. The method according to claim 1 or 2, wherein: The method comprises the following steps: (1) ultrasonically cleaning the substrate in alkaline detergent aqueous solution, ethanol aqueous solution and ultrapure water in sequence and drying the substrate, then sending the cleaned substrate into a sample injection chamber for evacuation, and then transferring the substrate into the deposition chamber; (2) When the vacuum degree of the deposition chamber reaches the critical vacuum degree, Ar gas is introduced, and the deposition gas pressure is adjusted to the first pressure by using a butterfly valve, and the target gun power is increased to 400W to 800W for ignition; (3) adjusting the Ar gas flow rate and using a butterfly valve to adjust the deposition gas pressure to a second pressure so that the substrate is sputtered and deposited a desired number of times; (4) reducing the target gun power, stopping the introduction of Ar gas, and taking out the substrate when the vacuum degree of the deposition chamber reaches the critical vacuum degree; The critical vacuum degree is 2×10 -5 ~5×10 -3 Pa.
4. The method according to claim 3, wherein: In step (1), the alkaline detergent aqueous solution includes one or more of calcium bicarbonate, sodium carbonate, and sodium hydroxide; the cleaning time is 5 to 30 minutes; The vacuum pumping is performed until the vacuum degree of the injection chamber reaches 2×10 -5 ~5×10 -3 Pa.
5. The method according to claim 3, wherein: In step (2), the ratio of the flow rate of the Ar gas to the volume of the deposition chamber is 0.1 to 4 sccm / L, and the first pressure is 1.0 to 6.0 Pa.
6. The method according to claim 3, wherein: In step (3), the ratio of the flow rate of the Ar gas to the volume of the deposition chamber is 0.1 to 4 sccm / L, the second pressure is 0.1 to 3.0 Pa, and the required number of times is 10 to 50 times.
7. The method according to claim 1, wherein: The butterfly valve is arranged on the top wall of the deposition chamber, and a vacuum pump is connected to the outer side of the butterfly valve.
8. A Mo thin film prepared by the method according to any one of claims 1 to 7.
9. The Mo thin film according to claim 8, wherein The thickness of the Mo film is 50-1000 nm; the square resistance of the Mo film is 0.5-5Ω / □; the conductivity of the Mo film is 5000-50000 S / cm; the XRD spectrum of the Mo film has a characteristic peak at 40-41.5°.
10. Use of the Mo thin film according to claim 8 or 9 in thin-film solar cells, liquid crystal displays or microelectronics.