Nanometer phase change film material and preparation method and application thereof
By depositing an Al composite Sb nanophase change film on the PEEK base material, the problems of slow phase change speed and poor thermal stability of traditional phase change materials are solved, achieving higher storage density and bending resistance, and is suitable for the field of flexible memory.
Patent Information
- Application Number
- CN202410767309.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-15
AI Technical Summary
The traditional phase change material Ge2Sb2Te5 has a slow phase change speed, low thermal stability, and poor stability of the Sb element, making it difficult to meet the needs of flexible memory for fast reading and writing, good thermal stability, and bending resistance.
Al composite Sb material is used, and a nano-phase change film is deposited on the PEEK base material through magnetron sputtering technology. The general chemical formula is [Al(10-X)/SbX]a, which improves the thermal stability and phase change speed of the material. And through multiple cycles of sputtering, films of different thicknesses are obtained.
It significantly improves storage density, thermal stability, anti-bending performance and low power consumption, reduces device power consumption, and provides higher phase transition temperature and lower resistance drift.
Smart Images

Figure CN118773559A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present application relate to the technical field of phase change materials for information storage, and in particular to a nano phase change thin film material and a preparation method and application thereof. Background Art
[0002] The rapid development of today's society is inseparable from the contribution of science and technology. However, it relies heavily on the progress of computer and data storage technology. Non-volatile storage technology plays a vital role in the storage energy efficiency of computer systems. Phase change memory (PCM) is a new type of non-volatile memory that uses the conductivity difference between sulfide compounds when they transform between crystalline and amorphous states to store data. In recent years, with the rapid development of wearable devices, medical implantable devices, electronic skin and smart electronic fabrics, new requirements have been put forward for the flexibility of integrated circuits and memories. Flexible memories are not only required to have fast read and write speeds, good thermal stability, low energy consumption, etc., but also have good anti-bending and anti-extrusion properties. Therefore, further improving the performance of flexible phase change memory has become a key issue.
[0003] Traditional phase change material Ge 2 Sb 2 Te 5 (GST) is relatively mature, but due to its slow phase change speed, its thermal stability is not very high; and the Te element contains certain toxins, which is not very friendly to the environment. The stability of the phase change material Sb is poor and the crystallization temperature is low. Sb is a layered metal (space group: R3m), each layer contains a connected wrinkled six-membered ring structure, and the nearest and second nearest antimony atoms form a deformed octahedron. The weak bonding between the layers also makes it very soft and brittle. Summary of the invention
[0004] In view of this, the embodiments of the present application provide a nano phase change thin film material and a preparation method and application thereof, which utilizes Al composite Sb to improve the thermal stability and phase change speed of the material. The nano phase change thin film material has good three-state storage performance, can effectively improve the storage density, and also has the advantages of good thermal stability, low resistance drift, and good bending resistance. It can be well applied to the field of phase change memory and can effectively overcome the defects of the above-mentioned prior art.
[0005] The first aspect of the embodiment of the present application provides a nano phase change thin film material, which is composed of Al composite Sb metal and then deposited on a base material. The chemical formula of the material is [Al (10-X) / Sb X ] a ;
[0006] Wherein, x is the proportion of Sb element, and 0 < x ≤ 10; a is the number of deposition cycles.
[0007] Polydimethylsiloxane (PDMS) is an organic material with a colorless and transparent appearance and hydrophobicity, but its thermal conductivity is not ideal. Polyethylene terephthalate (PET) is light in weight and high in toughness, but it is not heat-resistant. Polyimide (PI) has problems in the application of the microelectronics industry that it is difficult to balance the mechanical strength and thermal expansion coefficient, which may affect its use effect. Polyetheretherketone (PEEK) has various advantages, including good thermoplasticity, excellent stability, low production cost, and relatively simple production process, etc.; in addition, it also has certain corrosion resistance, insulation, and good deformation ability, which can meet various working environments and usage requirements. The excellent ductility of PEEK provides a good opportunity for us to study the effects of external factors such as bending, stretching, and compression on the film. The relatively high melting point of PEEK (334 °C) also makes it possible to provide a phase change film with high thermal stability. Therefore, PEEK is used as the flexible substrate in this paper.
[0008] Aluminum (Al) is a high-quality conductive material with a resistivity half that of copper, which can provide good current transmission and connection effects; when used as an inhibition layer in semiconductor materials, aluminum can ensure the smooth transmission of current, reduce resistance loss, and improve the efficiency of the device.
[0009] In some embodiments that may include the above embodiments, the base material is made of PEEK material.
[0010] In some embodiments that may include the above embodiments, a takes the value of 10.
[0011] The second aspect of the embodiments of the present application also provides a preparation method of the above-mentioned nano-phase change thin film material, including the following steps:
[0012] (1) Install the Al metal target and the Sb metal target on two target positions respectively, place the base material on the base, and then evacuate the sputtering chamber.
[0013] (2) Rotate the base to the target positions corresponding to the Al metal target and the Sb metal target in sequence, and perform magnetron sputtering to obtain the nano-phase change thin film material.
[0014] In some embodiments that may include the above embodiments, it further includes step (3) repeating step (2)
[0015] multiple times to obtain nano-phase change thin film materials with different thicknesses.
[0016] In some embodiments that may include the above embodiments, in step (1), the base material is further pre-treated before being placed on the base, and the specific process is: cutting, cleaning and drying the base material for standby use.
[0017] In some embodiments that may include the above embodiments, in step (2), the sputtering gas is Ar gas, the volume percentage of Ar gas is ≥99.999%, the Ar gas flow rate is 30-40 sccm, and the sputtering gas pressure is 0.2-0.4 Pa.
[0018] In some embodiments that may include the above embodiments, in step (1), the purity of the Al metal target and the Sb metal target are both greater than 99.999%.
[0019] In some embodiments that may include the above embodiments, in step (2), the sputtering rate of the Al metal target is 4.5 s / nm, the sputtering power of the Al metal target is 100 W, and the sputtering time of the Al metal target is 18 s; or
[0020] The sputtering rate of the Sb metal target is 1.29-1.9 s / nm, the sputtering power of the Sb metal target is 30 W, and the sputtering time of the Sb metal target is 11 s.
[0021] A third aspect of the embodiments of the present application also provides an application of the above-mentioned nano phase change thin film material in a phase change memory.
[0022] Compared with the prior art, the embodiments of the present application have the following beneficial effects:
[0023] 1. The nano phase change film material with flexible performance in this application is deposited on the PEEK base material by magnetron sputtering. The PEEK is a stable polymer that not only has excellent thermal stability and chemical corrosion resistance, but also has a relatively high melting point and can withstand high temperatures up to 400°C.
[0024] 2. The nano phase change film material with flexible performance in this application is prepared by Al composite Sb on PEEK substrate. Compared with traditional GST and pure Sb materials, the thermal stability and phase change speed are significantly improved, and it also has good three-state storage performance, which can effectively improve the storage density;
[0025] 3. The nano phase change thin film material with flexible properties provided in the present application has a lower threshold voltage when changing from amorphous to crystalline state, thereby reducing device power consumption; in addition, the material also has good bending resistance and extremely low resistance drift. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0027] Figure 1 The graph is a relationship between the in-situ resistance and temperature of the thin film materials prepared in Examples 1 to 5 and Comparative Example 1, wherein the abscissa Temperature represents the temperature, and Resistance represents the resistance of the thin film;
[0028] Figure 2 The film material prepared in Example 4 is subjected to a stretching cycle test of 50 times, 100 times, 200 times and 400 times of stretching at a stretching degree of 10%;
[0029] Figure 3 (a) and (b) are phase transition temperature diagrams obtained by testing the thin film material prepared in Example 4 in the outer bending and inner bending zone states of Flat, 10,000 times of bending, 20,000 times of bending, 40,000 times of bending, and 80,000 times of bending, respectively; Figure 3 (c) and (d) are the graphs showing the changes in the amorphous and crystalline resistances of the thin film material prepared in Example 4 at 85°C after inner bending and outer bending, as well as the phase transition temperature after bending. The results show that with the increase in the number of bending times, the amorphous and crystalline resistances of the film both show a slight increase trend, while the phase transition temperature shows a downward trend;
[0030] Figure 4 (a) is a comparison diagram of the energy band gap of the thin film material prepared in Example 4 at different bending times after annealing; Figure 4 (b), (c) and (d) are resistance drift diagrams of the thin film material prepared in Example 4 after being flat, internally bent and externally bent, respectively;
[0031] Figure 5 (a)-(e) are AFM atomic force microscope scans of the thin film material prepared in Example 4 at different bending times after annealing; Figure 5 (f) is the electrostatic potential diagram of the thin film material prepared in Example 4 in a flat state after annealing; Figure 5 (g)-(j) are crack scanning images of the thin film material prepared in Example 4 at different bending states and different bending times after annealing. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0033] Unless otherwise specified, the experimental methods used in the examples of this application are all conventional methods.
[0034] In the following examples and comparative examples, unless otherwise specified, all raw materials can be obtained by commercial purchase or conventional methods.
[0035] Example 1
[0036] Al 1 / Sb 9 The preparation method of the nano phase change thin film material specifically comprises the following steps:
[0037] (1) Pretreatment of the flexible PEEK substrate: Cut the PEEK material and put it into a beaker filled with anhydrous ethanol. Then put the beaker into an ultrasonic cleaner for cleaning for 10-20 minutes. After cleaning, take out the PEEK, blow dry it with high-purity nitrogen, and finally leave it to dry completely for use.
[0038] (2) Preparation before magnetron sputtering: Al metal target and Sb metal target (with atomic percentage purity greater than 99.999%) were installed on two target positions respectively, the PEEK substrate material to be used in step (1) was placed on the base, and the sputtering chamber was evacuated to 3.5×10 -4 Pa or less, introduce high-purity Ar gas as sputtering gas, and the volume percentage of Ar gas is ≥99.999%, set the Ar gas flow rate to 30sccm, set the Al target sputtering power to 100W, set the Sb target sputtering power to 30W, and set the sputtering gas pressure to 0.4Pa;
[0039] (3) Preparation of nano phase change films by magnetron sputtering:
[0040] a) rotating the empty base to the corresponding target positions of the Al metal target and the Sb metal target respectively for pre-sputtering, cleaning the target and removing the oxidized part on the target surface;
[0041] b) After the target material is cleaned, the base with the PEEK material is transferred to the target positions corresponding to the Al metal target material and the Sb metal target material respectively and cycled for 10 cycles. The sputtering power of the Sb target position is set to 30 W, the sputtering time is 11 s, and the sputtering rate is 1.9 s / nm. The sputtering power of the Al target position is set to 100 W, the sputtering time is 18 s, and the sputtering rate is 4.5 s / nm. Then magnetron sputtering is started to obtain an Al-mixed Sb nano-phase change thin film material based on a PEEK substrate with a sputtering thickness of 100 nm, recorded as Al 1 / Sb 9 .
[0042] Example 2
[0043] The preparation method of the nano phase change film material provided in this embodiment can refer to Example 1, except that the contents of Al and Sb are changed, that is, x is 8, which is recorded as Al 2 / Sb 8 .
[0044] Example 3
[0045] The preparation method of the nano phase change film material provided in this embodiment can refer to Example 1, except that the contents of Al and Sb are changed, that is, x is set to 7, which is denoted as Al 3 / Sb 7 .
[0046] Example 4
[0047] The preparation method of the nano phase change film material provided in this embodiment can refer to Example 1, except that the contents of Al and Sb are changed, that is, x is 6, which is recorded as Al 4 / Sb 6 .
[0048] Example 5
[0049] The preparation method of the nano phase change film material provided in this embodiment can refer to Example 1, except that the contents of Al and Sb are changed, that is, x is 5, which is recorded as Al 5 / Sb 5 .
[0050] Comparative Example 1
[0051] The preparation method of the nano phase change thin film material provided in this comparative example can refer to Example 1, except that the target material is only a Sb metal target material, and no Al target material is added.
[0052] Performance Testing
[0053] 1. The performance of the flexible nano phase change film materials prepared in the above Examples 1 to 5 and Comparative Example 1 was tested. Figure 1As shown in the figure, initially all deposited thin film materials maintain a relatively high resistance, and as the temperature rises, the resistance slowly decreases. When the phase transition temperature is reached, the resistance drops sharply and remains unchanged after dropping to a certain value. At this time, the nano phase change thin film material undergoes a transition from amorphous to crystalline. The phase transition temperature of the Sb phase change thin film material based on the PEEK substrate is 146°C. The phase change thin film material after Al and Sb composite undergoes a secondary phase transition, presenting three stable resistance states, with the potential for multi-level storage. The phase transition temperature increases, with the highest values of 175°C and 270°C ( Figure 1 ), which greatly improves the thermal stability of the phase change thin film material; and both the amorphous resistance and the crystalline resistance of the phase change thin film material are increased, which is beneficial to reducing the power consumption of the phase change thin film material during the reversible transformation operation.
[0054] 2. The phase change film material prepared in the above-mentioned embodiment 4 is subjected to a tensile test. Figure 2 The phase change film material was stretched 50, 100, 200, and 400 times. The resistance and phase change temperature of the phase change film material changed slightly, but the complete phase change process could still be achieved.
[0055] 3. The phase change film material prepared in Example 4 is subjected to a bending test. Figure 3 As shown in (a) and (b), the phase change film material was bent 10,000, 20,000, 40,000 and 80,000 times in the outward bending and inward bending states respectively. The phase change temperature of the phase change film material was slightly affected, but the complete phase change process could still be carried out. Figure 3 (c) and (d) are line graphs of the crystalline and amorphous resistances and phase change temperature of the flexible phase change film material prepared in Example 4, respectively. It can be seen that when the phase change film material is bent inward and outward, as the number of bending times increases, the crystalline and amorphous resistances of the film remain basically unchanged, and the phase change temperature has a slight downward trend.
[0056] 4. The phase change film material prepared in Example 4 was subjected to near infrared testing. Figure 4 As shown in (a), the diffuse reflectance spectra of the annealed phase change film material at different bending times were measured by a near-infrared spectrophotometer, and Eg was obtained by the Tauc equation. After annealing, the energy band gap of the phase change film material decreases slightly after the outer bending, and the energy band gap remains almost unchanged after the inner bending. The above results show that Al 4 / Sb 6 The electronic structure of flexible phase change film materials maintains good performance during bending. Figure 4 (b)-(d) are the resistance drift coefficients of the film after different bending times. It can be seen that after bending under different bending conditions, the resistance drift coefficient of the film fluctuates slightly, but the overall change is not large. The results show that Al 4 / Sb 6Flexible phase change films have excellent bending resistance.
[0057] 5. Bend the annealed thin film material for different times and observe the AFM images after bending, such as Figure 5 As shown in (a)-(e), the surface morphology of the film material after annealing at different bending times was observed using an atomic force microscope. It can be seen that microcracks appeared on the film surface after different bending times, regardless of whether it was in an inward or outward bending state. Figure 5 (f) is the electrostatic potential diagram under flat state, Figure 5 (g) and (h) are the crack scanning images after bending 40,000 times and 80,000 times in the inner bending state, respectively. Figure 5 (i) and (j) are the crack scanning images of bending 40,000 times and 80,000 times in the external bending state, respectively. From the above figures, it can be concluded that bending has limited effect on the film structure, which further illustrates that Al 4 / Sb 6 Flexible phase change film has good bending resistance.
[0058] Through a series of test data, it can be seen that the Al-composite Sb flexible multi-level phase change thin film material based on flexible PEEK substrate has higher thermal stability, excellent bending resistance, extremely low resistance drift, higher storage density and lower power consumption, and has great potential in phase change storage fields such as electronic skin and smart wearable electronic devices.
[0059] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A nano phase change thin film material, characterized in that: The material is composed of Al composite Sb metal and then deposited on the base material. The chemical formula of the material is [Al (10-X) / Sb X ] a ; Among them, x is the proportion of the Sb element, and 0 < x ≤ 10; a is the number of deposition cycles.
2. The nano phase change thin film material according to claim 1, characterized in that: The base material is made of PEEK material.
3. The nano phase change thin film material according to claim 1, characterized in that: a takes the value of 10.
4. A method for preparing the nano phase change thin film material according to any one of claims 1 to 3, characterized in that: It includes the following steps: (1) Install the Al metal target and the Sb metal target on two target positions respectively, place the base material on the substrate holder, and then evacuate the sputtering chamber. (2) Rotate the substrate holder to the target positions corresponding to the Al metal target and the Sb metal target successively, and perform magnetron sputtering to obtain the nano-phase change thin film material.
5. The preparation method according to claim 4, characterized in that: It further includes step (3). After repeating step (2) multiple times, nano-phase change thin film materials with different thicknesses are obtained.
6. The preparation method according to claim 4, characterized in that: In step (1), before placing the base material on the substrate holder, pre-treatment of the base material is also included. The specific process is: cut, clean and dry the base material for later use.
7. The preparation method according to claim 4, characterized in that: In step (2), the sputtering gas is Ar gas, the volume percentage of Ar gas ≥ 99.999%, the Ar gas flow rate is 30 - 40 sccm, and the sputtering pressure is 0.2 - 0.4 Pa.
8. The preparation method according to claim 4, characterized in that: In step (1), the purities of the Al metal target and the Sb metal target are both greater than 99.999%.
9. The preparation method according to claim 4, characterized in that: In step (2), the sputtering rate of the Al metal target is 4.5 s / nm, the sputtering power of the Al metal target is 100 W, and the sputtering time of the Al metal target is 18 s; or the sputtering rate of the Sb metal target is 1.29 - 1.9 s / nm, the sputtering power of the Sb metal target is 30 W, and the sputtering time of the Sb metal target is 11 s.
10. Application of the nano-phase change thin film material according to any one of claims 1 - 3 in a phase change memory.