Method for preparing intrinsic hydrogenated amorphous silicon film by hot filament CVD (chemical vapor deposition)
By depositing a multi-layer film structure of buffer layer and main layer in hot wire CVD equipment, combined with oxygen-carbon doping gas and hydrogen, the problem of insufficient passivation quality of intrinsically hydrogenated amorphous silicon film in hot wire CVD technology is solved and improved It improves the photoelectric conversion efficiency and minority carrier lifetime of SHJ solar cells, and reduces equipment costs and production material losses.
Patent Information
- Application Number
- CN202410791671.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-15
AI Technical Summary
Hot filament CVD technology is inferior to PECVD technology in preparing intrinsically hydrogenated amorphous silicon films with high passivation quality, resulting in insufficient minority carrier lifetime and affecting the photoelectric conversion efficiency of SHJ solar cells.
Using hot filament CVD equipment at a hot filament temperature of 1600-2200°C, the intrinsic hydrogenated non-ferrous metal with high passivation quality is prepared by depositing a multi-layer film structure of the buffer layer and the main layer, combined with oxygen-carbon doping gas and hydrogen. Crystalline silicon film improves minority carrier lifetime and photoelectric conversion efficiency.
It effectively reduces equipment costs, significantly improves passivation quality and photoelectric conversion efficiency, is suitable for traditional and back-contact SHJ solar cells, and reduces production material losses.
Smart Images

Figure CN118773571A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solar cells, and in particular to a method for preparing an intrinsic hydrogenated amorphous silicon film by hot-wire CVD. Background Art
[0002] Although PERC solar cells are still the mainstream in the global photovoltaic market, their photoelectric conversion efficiency is getting closer and closer to the theoretical limit, and it is becoming increasingly difficult for the industry to improve efficiency. It has become an industry consensus that they will be replaced by more efficient solar cells in the future. At present, tunnel oxide passivated contact (TOPcon) solar cells and silicon heterojunction (SHJ) solar cells have the highest efficiency and relatively mature technology. They are generally valued by the industry and are being put into mass production.
[0003] Compared with TOPcon solar cells, SHJ solar cells have many advantages such as higher photoelectric conversion efficiency, lower temperature coefficient, stronger weak light response and relatively simple industrial manufacturing process, but due to cost issues, SHJ solar cells are at a disadvantage in the industrial competition with TOPcon solar cells. Among them, the relatively high equipment cost investment is one of the shortcomings of SHJ solar cells that are criticized. Its production line equipment investment is about 60% higher than that of TOPcon cells, of which PECVD equipment for coating amorphous silicon thin films accounts for 50% of the total equipment investment. Therefore, reducing the equipment cost of this process can greatly reduce the total cost, thereby promoting the development of SHJ solar cells.
[0004] Since PECVD equipment is widely used in the photovoltaic industry and has undergone several years of development, its equipment cost has been difficult to continue to reduce. Therefore, using other cheap equipment and technologies as a substitute has become the most effective way to reduce costs. Since hot-filament CVD technology can also coat SHJ solar cells with amorphous silicon thin films, compared with PECVD equipment, hot-filament CVD has the advantages of fast coating rate, low gas loss, no plasma damage, easy large-area coating and low equipment cost. Therefore, the use of hot-filament CVD technology can effectively reduce equipment costs and reduce production material losses, and has good application prospects.
[0005] However, the hot-wire CVD technology is still inferior to the PECVD technology in the preparation of high-passivation quality intrinsic hydrogenated amorphous silicon films. Since the intrinsic hydrogenated amorphous silicon film is responsible for passivation in SHJ solar cells, it is the key to achieving high efficiency. For a long time, the intrinsic hydrogenated amorphous silicon films prepared by the hot-wire CVD technology have all been single-layer film structures without a buffer layer to inhibit epitaxy, which makes it difficult for the minority carrier lifetime to reach more than 3ms. Therefore, it is urgent to provide a solution to improve the above problems. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing an intrinsic hydrogenated amorphous silicon film by hot wire CVD. By adopting the hot wire CVD technology to prepare the intrinsic hydrogenated amorphous silicon film, the equipment cost can be effectively reduced, and the intrinsic hydrogenated amorphous silicon film deposited by multilayer film can effectively inhibit epitaxy, which can improve the passivation quality, improve the minority carrier lifetime and the photoelectric conversion efficiency.
[0007] The present invention provides a method for preparing an intrinsic hydrogenated amorphous silicon film by hot-wire CVD, comprising the following steps: depositing a buffer layer on the surface of a silicon wafer to be coated at a hot-wire temperature of 1600-2200° C., a silane flow rate of 5-1000sccm, and a pressure of 0.3-5Pa in a hot-wire CVD device to obtain an intermediate silicon wafer; depositing a main layer on the surface of the buffer layer of the intermediate silicon wafer at a hot-wire temperature of 1600-2200° C., a silane flow rate of 5-1000sccm, a hydrogen flow rate of 2-3000sccm, and a pressure of 0.3-5Pa to obtain a silicon wafer deposited with an intrinsic hydrogenated amorphous silicon film; wherein the intrinsic hydrogenated amorphous silicon film comprises a buffer layer and a main layer which are deposited and formed in sequence.
[0008] The method provided by the present invention adopts hot wire CVD equipment to prepare intrinsic hydrogenated amorphous silicon film, which can effectively reduce equipment cost. At the same time, a buffer layer is deposited on the surface of the silicon wafer to be coated in advance, which can effectively inhibit epitaxy and significantly improve the passivation quality. The prepared intrinsic hydrogenated amorphous silicon film can be applied not only to traditional double-sided SHJ solar cells, but also to other high-efficiency solar cells such as back-contact SHJ solar cells.
[0009] Optionally, in the process of depositing a buffer layer on the surface of the silicon wafer to be coated to obtain an intermediate silicon wafer, oxygen-carbon doped gas is also introduced into the hot wire CVD equipment, and the flow rate of the oxygen-carbon doped gas is 0.1-500sccm; wherein the oxygen-carbon doped gas includes one of carbon dioxide, methane, nitrous oxide, acetylene, ethylene, and monomethylsilane.
[0010] Optionally, in the process of depositing a buffer layer on the surface of the silicon wafer to be coated to obtain an intermediate silicon wafer, 1-3000 sccm of hydrogen is also introduced into the hot wire CVD equipment.
[0011] Optionally, in the process of depositing a buffer layer on the surface of the silicon wafer to be coated to obtain an intermediate silicon wafer, the deposition time is 1-50s; and the formed thickness of the buffer layer in the intermediate silicon wafer is 0.5-2nm.
[0012] Optionally, in the process of depositing the main layer on the surface of the buffer layer of the intermediate silicon wafer, N monomer layers are sequentially deposited on the surface of the buffer layer of the intermediate silicon wafer, and the N stacked monomer layers constitute the main layer; wherein N is a positive integer greater than or equal to 2. By setting the main layer as N monomer layers, it is possible to obtain a lower contact resistivity, increase the minority carrier lifetime and reduce the microstructure factor, improve the passivation quality, and further improve the conversion efficiency of the SHJ solar cell.
[0013] Optionally, in the process of depositing N monomer layers in sequence on the buffer layer surface of the intermediate silicon wafer, the hot wire temperature during the deposition of each monomer layer is independently any temperature value within the range of 1600-2200°C, the silane flow rate during the deposition of each monomer layer is independently any flow rate value within the range of 5-1000sccm, and the hydrogen flow rate during the deposition of each monomer layer is independently any flow rate value within the range of 2-3000sccm.
[0014] Optionally, during the process of depositing the main layer on the surface of the buffer layer of the intermediate silicon wafer, a carbon-oxygen doped gas is also introduced into the hot wire CVD equipment, and the flow rate of the carbon-oxygen doped gas is 0.1-500sccm; wherein the carbon-oxygen doped gas includes one of carbon dioxide, methane, nitrous oxide, acetylene, ethylene, and monomethylsilane.
[0015] Optionally, in the process of depositing the main layer on the surface of the buffer layer of the intermediate silicon wafer to obtain a silicon wafer deposited with an intrinsic hydrogenated amorphous silicon film, the deposition time is 1-200s; and the formed thickness of the intrinsic hydrogenated amorphous silicon film is 3-10nm. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 A flowchart of a method for preparing an intrinsic hydrogenated amorphous silicon film by hot-wire CVD provided in an embodiment of the present invention;
[0017] Figure 2 It is a schematic diagram of the structure after the intrinsic hydrogenated amorphous silicon film is deposited on the surface of the silicon wafer to be coated according to an embodiment of the present invention;
[0018] Figure 3 FTIR absorption spectra of the buffer layer in the intrinsic hydrogenated amorphous silicon film prepared in Examples 1 to 3 of the present invention;
[0019] Figure 4 The cell performance characterization diagram of the semi-finished silicon wafers prepared in Examples 1 to 3 of the present invention and Comparative Example 1 after being prepared into SHJ solar cells;
[0020] Figure 5 The contact resistivity and minority carrier lifetime variation diagrams on the n-side and p-side of the intrinsic hydrogenated amorphous silicon films prepared in Examples 1, 4 to 9 of the present invention;
[0021] Figure 6 This is a cell performance characterization diagram of SHJ solar cells made from the semi-finished silicon wafers prepared in Examples 1 and 4 to 13 of the present invention. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be understood by people with general skills in the field to which the present invention belongs. "Including" and similar words used in this article mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects.
[0023] Reference Figure 1 The embodiment of the present invention provides a method for preparing an intrinsic hydrogenated amorphous silicon film by hot wire CVD, comprising the following steps:
[0024] S1. Depositing a buffer layer: depositing a buffer layer on the surface of the silicon wafer to be coated at a hot wire temperature of 1600-2200° C., a silane flow rate of 5-1000 sccm, and a pressure of 0.3-5 Pa in a hot wire CVD device to obtain an intermediate silicon wafer;
[0025] S2. Depositing the main layer: depositing the main layer on the buffer layer surface of the intermediate silicon wafer at a hot wire temperature of 1600-2200°C, a silane flow rate of 5-1000sccm, a hydrogen flow rate of 2-3000sccm, and a pressure of 0.3-5Pa to obtain a silicon wafer deposited with an intrinsic hydrogenated amorphous silicon film.
[0026] In some embodiments, when executing step S1 to deposit the buffer layer, the silicon wafer to be coated is one of a polished silicon wafer and a textured silicon wafer. When the silicon wafer to be coated is used, the surface pretreatment of the silicon wafer to be coated can be performed, such as surface cleaning. In fact, conventional processing steps in the field can be used for surface pretreatment of the silicon wafer to be coated. In fact, the full name of the gas flow unit sccm used is Standard cubic centimeter per minute, which stands for standard cubic centimeters per minute. In fact, when depositing an intrinsic hydrogenated amorphous silicon film on the silicon wafer to be coated, deposition can be performed on one side or both sides of the silicon wafer.
[0027] In fact, when the silicon wafers to be coated are respectively the textured silicon wafer 11 and the polished silicon wafer 12, and after the intrinsic hydrogenated amorphous silicon film 2 is deposited on the surface of the silicon wafer to be coated, the structure is as follows Figure 2 (a) and Figure 2 (c). Figure 2 (a) and Figure 2 It can be seen in (c) that the surfaces of the textured silicon wafer 11 and the polished silicon wafer 12 are respectively formed with a buffer layer 21 and a main layer 22, and the buffer layer 21 and the main layer 22 together constitute an intrinsic hydrogenated amorphous silicon film 2. Through the hot wire CVD technology, the buffer layer 21 is uniformly deposited on the surface of the silicon wafer to be coated, and the buffer layer 21 separates the silicon wafer to be coated and the main layer 22, which can inhibit epitaxy.
[0028] In some embodiments, when executing step S1 to deposit the buffer layer, the hot wire CVD equipment used can be vertical or horizontal, the gases used include silane, hydrogen, argon, carbon dioxide, methane, nitrous oxide, ethylene, acetylene, monomethylsilane, and the hot wire material used is tantalum wire, tungsten wire, rhenium wire, molybdenum wire, iridium wire, and alloy wires of the above materials.
[0029] In some embodiments, when performing step S1 to deposit the buffer layer, the furnace of the hot wire CVD equipment is vacuumed in advance.
[0030] In some embodiments, when performing step S1 to deposit the buffer layer, an oxygen-carbon doping gas is also introduced into the hot filament CVD device, and the flow rate of the oxygen-carbon doping gas is 0.1-500 sccm. In fact, the element doping ratio and element doping type in the buffer layer can be adjusted by adjusting the flow rate ratio of the oxygen-carbon doping gas and the silane gas.
[0031] In fact, when the buffer layer is deposited in step S1 and the oxygen-carbon doping gas is introduced into the hot wire CVD device, the oxygen-carbon doping gas used includes one of carbon dioxide, methane, laughing gas, acetylene, ethylene, and monomethylsilane. Specifically, the oxygen-carbon doping gas may include any carbon-containing or oxygen-containing single gas or mixed gas commonly used in the art.
[0032] In some embodiments, when performing step S1 to deposit the buffer layer, 1-3000 sccm of hydrogen is also introduced into the hot wire CVD device. In fact, by adjusting the flow ratio of hydrogen and silane gas, the ratio of hydrogen and silicon in the hot wire CVD device is adjusted, thereby adjusting the element doping ratio and element doping type of the buffer layer.
[0033] In some embodiments, when performing step S1 to deposit the buffer layer, an inert gas is also introduced into the hot wire CVD device. By adjusting the flow rate of the inert gas, the proportion of the deposition gas in the furnace of the hot wire CVD device can be adjusted as a whole, thereby regulating the rate of buffer layer deposition on the surface of the silicon wafer to be coated. Specifically, the introduced inert gas can be a mixed gas of one or more of argon, helium, and neon.
[0034] In some embodiments, when executing step S1 to deposit the buffer layer, the deposition time on the surface of the silicon wafer to be coated is controlled to be 1-50s. At this time, after the intermediate silicon wafer is obtained, the thickness of the buffer layer on the surface of the intermediate silicon wafer is 0.5-2nm.
[0035] In some embodiments, during the process of performing step S2 to deposit the main layer, N monomer layers are sequentially deposited on the surface of the buffer layer of the intermediate silicon wafer, and the N stacked monomer layers constitute the main layer, where N is a positive integer greater than or equal to 2. By setting the main layer as a multi-layer structure, the photoelectric conversion efficiency of the SHJ solar cell can be further improved, a higher passivation quality can be obtained, and the minority carrier lifetime can be increased.
[0036] In fact, when the silicon wafers to be coated are respectively the textured silicon wafer 11 and the polished silicon wafer 12, and two monomer layers are deposited on the surface of the silicon wafer to be coated, the structure is as follows: Figure 2 (b) and Figure 2 (d). Figure 2 (b) and Figure 2 As can be seen in (d), the first monomer layer 221 and the second monomer layer 222 are sequentially formed on the surface of the buffer layer 21, thereby forming a main body layer 22 of a double-layer membrane structure.
[0037] In some embodiments, when performing step S2 to deposit the main layer and sequentially depositing N monomer layers on the surface of the buffer layer of the intermediate silicon wafer, when each monomer layer is deposited, the corresponding hot wire temperature is independent of each other, the corresponding silane flow rate is also independent of each other, and the corresponding hydrogen flow rate is also independent of each other. Specifically, when each monomer layer is deposited, the corresponding hot wire temperature can be any temperature value within the range of 1600-2200°C, the corresponding silane flow rate can be any flow rate value within the range of 5-1000sccm, and the corresponding hydrogen flow rate can be any flow rate value within the range of 2-3000sccm.
[0038] In some embodiments, when the main layer is deposited in step S2 and N monomer layers are sequentially deposited on the surface of the buffer layer of the intermediate silicon wafer, the temperature of the hot wires corresponding to the N monomer layers deposited outward from the buffer layer increases or decreases sequentially. Specifically, when the temperature of the hot wires increases or decreases sequentially, the temperature difference of the hot wires corresponding to two adjacent monomer layers is 0-600°C.
[0039] In some embodiments, when performing step S2 to deposit the main layer, a carbon-oxygen doping gas is also introduced into the hot wire CVD device, and the flow rate of the carbon-oxygen doping gas is 0.1-500 sccm. In fact, the element doping ratio and element doping type in the main layer can be adjusted by adjusting the flow rate ratio of the carbon-oxygen doping gas, the silane gas, and the hydrogen gas.
[0040] In fact, when the main layer is deposited in step S2 and the carbon-oxygen doped gas is introduced into the hot wire CVD device, the carbon-oxygen doped gas used includes one of carbon dioxide, methane, laughing gas, acetylene, ethylene, and monomethylsilane. Specifically, the carbon-oxygen doped gas may include any carbon-containing or oxygen-containing single gas or mixed gas commonly used in the art.
[0041] In some embodiments, when performing step S2 to deposit the main layer, an inert gas is also introduced into the hot wire CVD device. By adjusting the flow rate of the inert gas, the proportion of the deposition gas in the furnace of the hot wire CVD device can be adjusted as a whole, thereby regulating the rate of the main layer deposition on the surface of the silicon wafer to be coated. Specifically, the inert gas introduced can be a mixed gas of one or more of argon, helium, and neon.
[0042] In some embodiments, when performing step S2 to deposit the main layer, the deposition time on the surface of the intermediate silicon wafer is controlled to be 1-200s, and the thickness of the obtained intrinsic hydrogenated amorphous silicon film is 3-10nm.
[0043] Example 1
[0044] This embodiment 1 provides a method for preparing an intrinsic hydrogenated amorphous silicon film by hot-filament CVD, comprising the following steps:
[0045] S1. Deposition of buffer layer: Place the textured silicon wafer after surface cleaning and drying in the furnace of the hot wire CVD equipment, and evacuate the hot wire CVD equipment until the pressure in the furnace is 0.3-5Pa, then heat the hot wire to 1650°C, and deposit a buffer layer on the surface of the textured silicon wafer at a silane flow rate of 30sccm and a pressure of 1Pa, and control the deposition time of the buffer layer to be 5s. After the deposition is completed, an intermediate silicon wafer is obtained; wherein, the thickness of the buffer layer on the surface of the intermediate silicon wafer is 1nm;
[0046] S2. Deposition of the main layer: at a hot wire temperature of 1800°C, a silane flow rate of 30 sccm, a hydrogen flow rate of 15 sccm, and a pressure of 1 Pa, a single main layer is deposited on the surface of the buffer layer of the intermediate silicon wafer to obtain a silicon wafer with an 8 nm thick intrinsic hydrogenated amorphous silicon film deposited thereon.
[0047] Example 2
[0048] This embodiment 2 provides a method for preparing an intrinsic hydrogenated amorphous silicon film by hot-filament CVD, which is different from the embodiment 1 in that, when depositing the buffer layer in step S1, the temperature of the hot-filament is controlled to be 1800°C.
[0049] Example 3
[0050] This embodiment 3 provides a method for preparing an intrinsic hydrogenated amorphous silicon film by hot-filament CVD, which is different from the embodiment 1 in that, when depositing the buffer layer in step S1, the temperature of the hot-filament is controlled to be 2000°C.
[0051] Example 4
[0052] This embodiment 4 provides a method for preparing an intrinsic hydrogenated amorphous silicon film by hot-filament CVD, which is different from the embodiment 1 in that the temperature of the hot-filament is controlled to be 1700° C. when S2 deposits the main layer.
[0053] Example 5
[0054] This embodiment 5 provides a method for preparing an intrinsic hydrogenated amorphous silicon film by hot-filament CVD, which is different from the embodiment 1 in that the temperature of the hot-filament is controlled to be 1750° C. when S2 deposits the main layer.
[0055] Example 6
[0056] This embodiment 6 provides a method for preparing an intrinsic hydrogenated amorphous silicon film by hot-filament CVD, which is different from the embodiment 1 in that the temperature of the hot-filament is controlled to be 1850° C. when S2 deposits the main layer.
[0057] Example 7
[0058] This embodiment 7 provides a method for preparing an intrinsic hydrogenated amorphous silicon film by hot-filament CVD, which is different from the embodiment 1 in that the temperature of the hot-filament is controlled to be 1900° C. when S2 deposits the main layer.
[0059] Example 8
[0060] This embodiment 8 provides a method for preparing an intrinsic hydrogenated amorphous silicon film by hot-filament CVD, which is different from the embodiment 1 in that the temperature of the hot-filament is controlled to be 1950° C. when S2 is depositing the main layer.
[0061] Example 9
[0062] This embodiment 9 provides a method for preparing an intrinsic hydrogenated amorphous silicon film by hot-filament CVD, which is different from the embodiment 1 in that the temperature of the hot-filament is controlled to be 2000° C. when S2 deposits the main layer.
[0063] Example 10
[0064] This embodiment 10 provides a method for preparing an intrinsic hydrogenated amorphous silicon film by hot filament CVD, which is different from embodiment 1 in that S2 deposits the main layer: at a hot filament temperature of 1800°C, a silane flow rate of 30sccm, a hydrogen flow rate of 15sccm, and a pressure of 1Pa, a first monomer layer is deposited on the surface of the buffer layer of the intermediate silicon wafer; on the intermediate silicon wafer deposited with the first monomer layer, a second monomer layer is deposited on the surface of the first monomer layer at a hot filament temperature of 1850°C, a silane flow rate of 30sccm, a hydrogen flow rate of 15sccm, and a pressure of 1Pa, to obtain a silicon wafer deposited with an 8nm thick intrinsic hydrogenated amorphous silicon film.
[0065] Embodiment 11
[0066] This embodiment 11 provides a method for preparing an intrinsic hydrogenated amorphous silicon film by hot-filament CVD, which is different from embodiment 10 in that the hot-filament temperature during the deposition of the second monomer layer in step S2 is 1900°C.
[0067] Example 12
[0068] This embodiment 12 provides a method for preparing an intrinsic hydrogenated amorphous silicon film by hot-filament CVD, which is different from the embodiment 10 in that the hot-filament temperature during the deposition of the second monomer layer in step S2 is 1950°C.
[0069] Embodiment 13
[0070] This embodiment 13 provides a method for preparing an intrinsic hydrogenated amorphous silicon film by hot-filament CVD, which is different from embodiment 10 in that the hot-filament temperature during the deposition of the second monomer layer in step S2 is 2000°C.
[0071] Comparative Example 1
[0072] This comparative example 1 provides a method for preparing an intrinsic hydrogenated amorphous silicon film by hot wire CVD, comprising the following steps: placing a textured silicon wafer after surface cleaning and drying treatment in the furnace of a hot wire CVD device, and evacuating the hot wire CVD device until the pressure in the furnace is 0.3-5Pa, and then depositing an intrinsic hydrogenated amorphous silicon film on the surface of the textured silicon wafer at a hot wire temperature of 1800°C, a silane flow rate of 30sccm, a hydrogen flow rate of 15sccm, and a pressure of 1Pa to obtain a silicon wafer with an 8nm thick intrinsic hydrogenated amorphous silicon film deposited thereon.
[0073] Detection and analysis1
[0074] The buffer layer of the intrinsic hydrogenated amorphous silicon film prepared in Examples 1 to 3 was subjected to microstructure testing and analysis, and the FTIR absorption spectrum data thereof are as follows: Figure 3 (a) to Figure 3 (c) shows the 2000cm obtained by Gaussian distribution fitting. -1and 2100cm -1 The absorption peaks at represent Si-H bonds and Si-H2 bonds, respectively, and the microstructure factor R (R = I Si-H2 / (I Si-H2 +I Si-H ))Evaluate the microstructure of the buffer layer.
[0075] from Figure 3 It can be seen that after using 1650℃ and 1800℃ hot wire temperatures for buffer layer deposition, a buffer layer film with a higher Si-H2 bond ratio than Si-H bonds can be prepared, and the film prepared at a hot wire temperature of 1650℃ has a higher Si-H2 bond ratio, which means that when the buffer layer is prepared at a lower temperature, it is more conducive to increasing the Si-H2 bond ratio in the buffer layer film. When the hot wire temperature of 2000℃ is used for deposition, the Si-H bond ratio in the prepared film is higher. This is because the hot wire temperature has a very strong silane decomposition ability at 2000℃.
[0076] Detection and analysis 2
[0077] After the intrinsic hydrogenated amorphous silicon film was deposited on both sides of the silicon wafer by the method described in Examples 1 to 3 and Comparative Example 1, the corresponding minority carrier lifetimes of the semi-finished silicon wafers were measured respectively. The results of the measurement under transient conditions using a Sinton WCT-120 device are shown in Table 1.
[0078] Table 1 Minority carrier lifetime
[0079] Minority carrier lifetime (ms) Comparative Example 1 2.3 Example 1 7.5 Example 2 6.7 Example 3 5.3
[0080] Since the minority carrier lifetime is generally used to evaluate the passivation quality, the higher the minority carrier lifetime, the better the passivation quality. It can be seen from Table 1 that the introduction of the buffer layer in Examples 1 to 3 can greatly improve the passivation quality of the intrinsic hydrogenated amorphous silicon film, and the buffer layer deposited at the hot wire temperature of 1650°C has the highest minority carrier lifetime among the samples. As the hot wire temperature gradually increases, the minority carrier lifetime also gradually decreases, but it is still significantly better than the semi-finished silicon wafer of Comparative Example 1 without a buffer layer.
[0081] Detection and analysis 3
[0082] After the intrinsic hydrogenated amorphous silicon film was deposited on both sides of the silicon wafer using the method described in Examples 1 to 3 and Comparative Example 1, the semi-finished silicon wafer was prepared into SHJ solar cells. The cell performance of the solar cells corresponding to Examples 1 to 3 and Comparative Example 1 was measured using a VISION VS-6825A tester at AM 1.5G, 1000W / m 2, short circuit current density (Jsc), open circuit voltage (Voc), fill factor (FF), conversion efficiency (Efficiency) were measured at 25°C. The results are as follows: Figure 4 (a)- Figure 4 (d) as shown.
[0083] from Figure 4 It can be seen that the performance of the solar cell is significantly improved after the intrinsic hydrogenated amorphous silicon film prepared in Examples 1 to 3 is inserted into the buffer layer, which is consistent with the minority carrier lifetime of each cell in Table 1. Figure 4 It can also be seen that when the buffer layer prepared at a hot wire temperature of 1650°C is applied to the SHJ solar cell, the performance of the cell is more significantly improved. Compared with Comparative Example 1, the open circuit voltage of the solar cell in Example 1 is increased by 2mV, the fill factor is increased by 0.9%, and the short circuit current density is increased by 0.1mA / cm 2 , resulting in a battery efficiency improvement of approximately 0.4%.
[0084] Detection and analysis4
[0085] After the intrinsic hydrogenated amorphous silicon film was deposited on both sides of the silicon wafer using the methods described in Examples 1, 4 to 9, the contact resistivity and minority carrier lifetime on the n-side and p-side were measured. The results are as follows: Figure 5 shown.
[0086] from Figure 5 It can be seen that when the hot wire temperature is 1800℃ during the deposition of the main layer, the minority carrier lifetime of the intrinsic hydrogenated amorphous silicon film is the highest. However, for both the n-side and the p-side, the higher the hot wire temperature, the lower the contact resistivity. This shows that the higher the hot wire temperature, the more conducive the intrinsic hydrogenated amorphous silicon film formed by the main layer prepared is to the transport of carriers. However, this will lead to a significant decrease in the minority carrier lifetime, which shows that it is difficult for a single-layer main layer structure to take into account both the passivation quality and the carrier transport.
[0087] Detection and analysis5
[0088] After the intrinsic hydrogenated amorphous silicon film was deposited on both sides of the silicon wafer by the method described in Example 1, Example 4 to Example 13, the semi-finished silicon wafers were assembled into SHJ solar cells, and the cell performance (short circuit current density (Jsc), open circuit voltage (Voc), fill factor (FF), conversion efficiency (Efficiency)) of the corresponding solar cells of Example 1, Example 4 to Example 13 were measured respectively, and the measurement results are as follows: Figure 6 (a)- Figure 6 (d) as shown.
[0089] from Figure 6It can be seen that by depositing the main layer as a double-layer structure and at a hot wire temperature of 1800°C and 1900°C when depositing the second monomer layer, the efficiency of the solar cell is improved, and at 1900°C the efficiency of the solar cell is as high as 24.35%, which is about 0.15% higher than the best efficiency of the solar cell with only a single main layer.
[0090] Detection and analysis6
[0091] After the intrinsic hydrogenated amorphous silicon film is deposited on both sides of the silicon wafer by the method described in Example 1 and Example 11, the microstructure factor R (R = I Si-H2 / (I Si-H2 +I Si-H ))The microstructure of the buffer layer was evaluated, and the contact resistivity and minority carrier lifetime on the n-side and p-side were measured. The results are shown in Table 2.
[0092] Table 2 Performance characteristics of single-layer main layer and double-layer main layer
[0093]
[0094] As can be seen from Table 2, making the main layer into a double-layer structure can not only obtain lower contact resistivity and microstructure factor, but also improve the minority carrier lifetime, indicating that the passivation quality is also improved. It is the dual improvement of contact resistivity and passivation quality that achieves the improvement in battery efficiency.
[0095] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.
Claims
1. A method for preparing an intrinsic hydrogenated amorphous silicon film by hot wire CVD, characterized in that: The following steps are involved: In a hot wire CVD device, at a hot wire temperature of 1600-2200°C, a silane flow rate of 5-1000sccm, and a pressure of 0.3-5Pa, a buffer layer is deposited on the surface of a silicon wafer to be coated to obtain an intermediate silicon wafer; at a hot wire temperature of 1600-2200°C, a silane flow rate of 5-1000sccm, a hydrogen flow rate of 2-3000sccm, and a pressure of 0.3-5Pa, a main layer is deposited on the surface of the buffer layer of the intermediate silicon wafer to obtain a silicon wafer deposited with an intrinsic hydrogenated amorphous silicon film; wherein the intrinsic hydrogenated amorphous silicon film includes a buffer layer and a main layer deposited and formed in sequence.
2. The method according to claim 1, characterized in that In the process of depositing a buffer layer on the surface of the silicon wafer to be coated to obtain an intermediate silicon wafer, oxygen-carbon doped gas is also introduced into the hot wire CVD equipment, and the flow rate of the oxygen-carbon doped gas is 0.1-500sccm; wherein the oxygen-carbon doped gas includes one of carbon dioxide, methane, nitrous oxide, acetylene, ethylene, and monomethylsilane.
3. The method according to claim 1, characterized in that: In the process of depositing a buffer layer on the surface of the silicon wafer to be coated to obtain an intermediate silicon wafer, 1-3000 sccm of hydrogen is also introduced into the hot wire CVD equipment.
4. The method according to any one of claims 1 to 3, characterized in that: In the process of depositing a buffer layer on the surface of a silicon wafer to be coated to obtain an intermediate silicon wafer, the deposition time is 1-50s; and the formed thickness of the buffer layer in the intermediate silicon wafer is 0.5-2nm.
5. The method according to claim 1, characterized in that In the process of depositing the main layer on the buffer layer surface of the intermediate silicon wafer, N monomer layers are sequentially deposited on the buffer layer surface of the intermediate silicon wafer, and the N stacked monomer layers constitute the main layer; wherein N is a positive integer greater than or equal to 2.
6. The method according to claim 5, characterized in that In the process of depositing N monomer layers in sequence on the buffer layer surface of the intermediate silicon wafer, the hot wire temperature during the deposition of each monomer layer is independently any temperature value within the range of 1600-2200°C, the silane flow rate during the deposition of each monomer layer is independently any flow rate value within the range of 5-1000sccm, and the hydrogen flow rate during the deposition of each monomer layer is independently any flow rate value within the range of 2-3000sccm.
7. The method according to claim 1 or 5, characterized in that: During the process of depositing the main layer on the surface of the buffer layer of the intermediate silicon wafer, a carbon-oxygen doped gas is also introduced into the hot wire CVD equipment, and the flow rate of the carbon-oxygen doped gas is 0.1-500sccm; wherein the carbon-oxygen doped gas includes one of carbon dioxide, methane, nitrous oxide, acetylene, ethylene, and monomethylsilane.
8. The method according to claim 1 or 5, characterized in that: In the process of depositing a main layer on the surface of a buffer layer of an intermediate silicon wafer to obtain a silicon wafer deposited with an intrinsic hydrogenated amorphous silicon film, the deposition time is 1-200s; and the molding thickness of the intrinsic hydrogenated amorphous silicon film is 3-10nm.
Citation Information
Patent Citations
Heterojunction solar cell taking amorphous silicon oxide film as intrinsic passivation layer
CN111509058A
Cited By
Carrier plate heating method for vacuum coating equipment and carrier plate
CN120366719A