Copper foil surface treatment process
Through two-step roughening and magnetron sputtering technology, combined with pickling, curing and passivation treatments, the problems of roughness and high peel strength of the existing copper foil surface treatment process are solved, and fine copper nodules on the surface of the copper foil are achieved. The balance of appearance and high peel strength meets the high-frequency signal transmission needs in the 5G field.
Patent Information
- Application Number
- CN202410809319.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-15
AI Technical Summary
The existing copper foil surface treatment process has problems such as long processing time, serious environmental pollution, and unstable effects. It is difficult to meet the needs of high-frequency signal transmission and high-performance printed circuit boards.
Using two-step roughening treatment and magnetron sputtering technology, through pickling, primary roughening, secondary roughening, curing, anti-diffusion barrier layer and passivation treatment, combined with silanization treatment, the fine copper tumor layer morphology and Uniform and dense plating, reducing the roughness of the copper foil surface and improving high peel strength.
It achieves a balance between reducing the surface roughness of the copper foil and high peel strength, meeting the needs of high-frequency signal transmission in the 5G field, and improving the corrosion resistance and performance of the copper foil.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal surface treatment, and in particular to a copper foil surface treatment process. Background Art
[0002] With the rapid development of the electronics industry today, the quality and technical level of multilayer printed circuit boards (PCBs) as the core components of electronic products directly affect the performance and service life of electronic products. In the manufacturing process of multilayer PCBs, copper foil, as an important conductive material, has a surface treatment process that is directly related to key indicators such as the interlayer bonding force and conductor surface roughness of the PCB, which in turn affects the overall performance of the PCB. The copper foil surface treatment process is one of the key links in the PCB manufacturing process. High-quality copper foil surface treatment technology can not only improve and enhance the interlayer bonding force and control the surface roughness of the conductor, thereby improving the quality of the PCB, but also meet the skin effect requirements of high-frequency signals and ensure stable signal transmission. In addition, with the rapid development of high-end industries such as 5G communications and new energy vehicles, higher requirements are placed on the performance of electrolytic copper foil products, further highlighting the importance of copper foil surface treatment technology.
[0003] The development of copper foil surface treatment technology can be traced back to the early 1960s. At that time, domestic and foreign copper foil manufacturers mainly used traditional processes such as anodizing and electroplating to treat the surface of copper foil. However, these traditional processes have problems such as long processing time, serious environmental pollution, and unstable processing effects, which are difficult to meet the growing market demand. Entering the 21st century, with the advancement of science and technology and the improvement of environmental protection requirements, the copper foil surface treatment process has developed rapidly. New surface treatment technologies continue to emerge, such as rolled copper foil degreasing pickling, roughening, curing, nickel-cobalt-zinc-chromium electroplating and silane coating, which not only improve the surface quality of copper foil, but also reduce environmental pollution and achieve green and environmentally friendly production. Although the copper foil surface treatment process has made significant progress, it still faces many challenges. As electronic products develop towards high integration, lightness, and high performance, more stringent requirements are placed on the fine circuit manufacturing technology of printed circuit boards. The performance of the inner copper foil used as a printed circuit board also needs to be further improved to ensure high-frequency and high-speed transmission of signals while maintaining the bonding force between the copper foil and the substrate, which places very high demands on the surface treatment process of copper foil. Summary of the invention
[0004] Based on the problems existing in the background technology, the present invention provides a surface treatment process for copper foil, which can balance the two-way requirements of reducing the roughness of the copper foil and achieving a relatively high peel strength.
[0005] The present invention is implemented by the following technical solutions:
[0006] The present invention discloses a copper foil surface treatment process, comprising the following steps:
[0007] (1) Pickling treatment: placing the raw copper foil in a pickling solution for pickling treatment;
[0008] (2) Primary roughening treatment: placing the pickled copper foil in a primary roughening solution for roughening treatment;
[0009] (3) Secondary roughening treatment: placing the copper foil after the primary roughening treatment in a secondary roughening solution for roughening treatment;
[0010] (4) Curing treatment: placing the copper foil after the secondary roughening treatment in a curing liquid for curing treatment;
[0011] (5) Anti-diffusion barrier layer treatment: using magnetron sputtering vacuum coating technology to sputter an anti-diffusion barrier layer on the surface of the copper foil after curing;
[0012] (6) Passivation treatment: placing the copper foil treated with the diffusion barrier layer in a passivation solution for passivation treatment;
[0013] (7) Silanization and drying treatment: The copper foil after passivation treatment is immersed in a silane coupling agent solution and then dried with hot air to complete the surface treatment of the copper foil.
[0014] Furthermore, the pickling solution in step (1) is a sulfuric acid solution with a concentration of 10-20wt%, and the pickling time is 3-5s.
[0015] Furthermore, in step (2), the concentration of sulfuric acid in the primary roughening solution is 80-120 g / L, the concentration of copper ions is 6-12 g / L, and the concentration of chloride ions is 30-35 mg / L;
[0016] The conditions for the primary roughening treatment are: current density 25-35A / dm 2 , temperature 25-35℃, electrodeposition time 2-3s.
[0017] Furthermore, in the secondary roughening solution of step (3), the concentration of sulfuric acid is 80-120 g / L, the concentration of copper ions is 6-12 g / L, the concentration of gelatin is 80-120 mg / L, the concentration of sodium thiopropane sulfonate is 8-12 mg / L, the concentration of PEG is 5-8 mg / L, and the concentration of hydroxyethyl cellulose is 5-8 mg / L;
[0018] The conditions for the secondary roughening treatment are: current density 25-35A / dm 2 , temperature 25-35℃, electrodeposition time 4-6s.
[0019] Furthermore, in step (4), the concentration of sulfuric acid in the solidifying liquid is 80-120 g / L, and the concentration of copper ions is 50-60 g / L;
[0020] The curing conditions are: current density 25-35A / dm 2 , temperature 45-55°C, electrodeposition time 5-10s;
[0021] Furthermore, in step (5), the magnetron sputtering vacuum coating technology uses CoNiMo alloy as a target material, the element atomic ratio of the CoNiMo alloy is 1:1:1, and the thickness of the anti-diffusion barrier layer is 5-20nm.
[0022] Furthermore, in step (6), the Cr0 2 4 - The concentration is 2.0-2.5g / L, the concentration of K4P2O7 is 70-100g / L, and the pH value of the passivation solution is 11-12;
[0023] The passivation treatment conditions are: current density 2.5-3.5A / dm 2 , temperature is 35-45℃, and passivation treatment time is 5-10s.
[0024] Furthermore, in step (7), the concentration of the silane coupling agent solution is 5-8 g / L, and the soaking time is 2-5 s;
[0025] The hot air drying temperature is 180-220℃.
[0026] Another aspect of the present invention discloses a copper foil prepared by the copper foil surface treatment process as described above, and application of the copper foil in a printed circuit board.
[0027] Beneficial effects of the present invention:
[0028] 1. The present invention adopts a two-step roughening treatment. Chloride ions are added to the first roughening solution to promote the deposition rate and quickly achieve the deposition of copper particles. The second roughening solution uses the combined action of several additives to enhance the preferential growth of copper on the copper crystal surface, which has a more obvious particle refinement effect, reduces the grain size, and can also prevent the formation of pinholes and promote the fine density of crystal grains. The present invention forms a fine copper nodule layer on the surface of the copper foil through the second roughening process, reduces the roughness of the copper foil surface and ensures a higher specific surface area.
[0029] 2. The present invention adopts magnetron sputtering technology to sputter an anti-diffusion barrier layer on the surface of the copper foil after curing. The magnetron sputtering process can form a uniform, dense, and high-performance anti-diffusion barrier layer, thereby improving the corrosion resistance of the copper foil. By adjusting the sputtering parameters and the type of target material, precise control of the structure and performance of the anti-diffusion barrier layer can be achieved.
[0030] 3. The copper foil processing process of the present invention can form a uniform and dense coating on the surface of the copper foil. It adopts two-step roughening treatment and magnetron sputtering treatment steps to improve the performance of the copper foil, and balances the two-way requirements of reducing the roughness of the copper foil while achieving a relatively high peel strength. It can be used to prepare printed circuit boards to better meet the characteristics of fast high-frequency signal transmission and low loss in the 5G field. DETAILED DESCRIPTION
[0031] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments, but the protection scope of the present invention is not limited to the following embodiments.
[0032] The thickness of the raw copper foil selected in the embodiments and comparative examples of the present invention is 12 μm.
[0033] Example 1
[0034] A copper foil surface treatment process comprises the following steps:
[0035] (1) Pickling treatment: placing the raw copper foil in a pickling solution for pickling treatment;
[0036] The pickling solution is a sulfuric acid solution with a concentration of 15wt%, and the pickling time is 5s.
[0037] (2) Primary roughening treatment: placing the pickled copper foil in a primary roughening solution for roughening treatment;
[0038] The concentration of sulfuric acid in the primary roughening solution is 100 g / L, the concentration of copper ions is 10 g / L, and the concentration of chloride ions is 35 mg / L;
[0039] The conditions for the primary roughening treatment are: current density 30A / dm 2 , temperature 30℃, electrodeposition time 3s.
[0040] (3) Secondary roughening treatment: placing the copper foil after the primary roughening treatment in a secondary roughening solution for roughening treatment;
[0041] The concentration of sulfuric acid in the secondary roughening solution is 100 g / L, the concentration of copper ions is 10 g / L, the concentration of gelatin is 100 mg / L, the concentration of sodium thiopropane sulfonate is 10 mg / L, the concentration of PEG is 6 mg / L, and the concentration of hydroxyethyl cellulose is 6 mg / L;
[0042] The conditions for the secondary roughening treatment are: current density 30A / dm 2 , temperature 30℃, electrodeposition time 5s.
[0043] (4) Curing treatment: placing the copper foil after the secondary roughening treatment in a curing liquid for curing treatment;
[0044] The sulfuric acid concentration in the curing liquid is 100g / L, and the copper ion concentration is 55g / L;
[0045] The curing conditions are: current density 30A / dm 2 , temperature 50 °C, electrodeposition time 6 s;
[0046] (5) Anti-diffusion barrier layer treatment: using magnetron sputtering vacuum coating technology to sputter an anti-diffusion barrier layer on the surface of the copper foil after curing;
[0047] The magnetron sputtering vacuum coating technology uses CoNiMo alloy as the target material. The element atomic ratio of CoNiMo alloy is 1:1:1, and the thickness of the anti-diffusion barrier layer is 10nm.
[0048] (6) Passivation treatment: placing the copper foil treated with the diffusion barrier layer in a passivation solution for passivation treatment;
[0049] Cr0 in passivation solution 2 4 - The concentration is 2.2 g / L, the concentration of K4P2O7 is 80 g / L, and the pH value of the passivation solution is 11;
[0050] The passivation treatment conditions are: current density 3A / dm 2 , temperature is 38℃, and passivation treatment time is 8s.
[0051] (7) Silanization and drying treatment: The copper foil after passivation treatment is immersed in a silane coupling agent solution and then dried with hot air to complete the surface treatment of the copper foil.
[0052] The concentration of silane coupling agent KH-550 solution is 6 g / L, and the immersion time is 3 s;
[0053] The hot air drying temperature is 200℃.
[0054] Example 2
[0055] The difference between this embodiment and embodiment 1 is that in the secondary roughening solution of step (3), the concentration of sulfuric acid is 100 g / L, the concentration of copper ions is 10 g / L, the concentration of gelatin is 80 mg / L, the concentration of sodium thiopropane sulfonate is 10 mg / L, the concentration of PEG is 6 mg / L, and the concentration of hydroxyethyl cellulose is 6 mg / L;
[0056] The rest is the same as in Example 1.
[0057] Example 3
[0058] The difference between this embodiment and embodiment 1 is that in the step (3) the concentration of sulfuric acid in the secondary roughening solution is 100 g / L, the concentration of copper ions is 10 g / L, the concentration of gelatin is 100 mg / L, the concentration of sodium thiopropane sulfonate is 12 mg / L, the concentration of PEG is 6 mg / L, and the concentration of hydroxyethyl cellulose is 6 mg / L;
[0059] The rest is the same as in Example 1.
[0060] Comparative Example 1
[0061] The difference between this comparative example and Example 1 is that it does not include a secondary roughening treatment step;
[0062] The rest is the same as in Example 1.
[0063] Comparative Example 2
[0064] The difference between this comparative example and Example 1 is that it does not include a roughening treatment step;
[0065] The rest is the same as in Example 1.
[0066] Comparative Example 3
[0067] The difference between this comparative example and Example 1 is that in the step (3) the concentration of sulfuric acid in the secondary roughening solution is 100 g / L, the concentration of copper ions is 10 g / L, the concentration of sodium thiopropane sulfonate is 10 mg / L, the concentration of PEG is 6 mg / L, and the concentration of hydroxyethyl cellulose is 6 mg / L;
[0068] The rest is the same as in Example 1.
[0069] Comparative Example 4
[0070] The difference between this comparative example and Example 1 is that in the step (3) the concentration of sulfuric acid in the secondary roughening solution is 100 g / L, the concentration of copper ions is 10 g / L, the concentration of gelatin is 100 mg / L, the concentration of PEG is 6 mg / L, and the concentration of hydroxyethyl cellulose is 6 mg / L;
[0071] The rest is the same as in Example 1.
[0072] Comparative Example 5
[0073] The difference between this comparative example and Example 1 is that in the step (3) the concentration of sulfuric acid in the secondary roughening solution is 100 g / L, the concentration of copper ions is 10 g / L, the concentration of gelatin is 100 mg / L, the concentration of sodium thiopropane sulfonate is 10 mg / L, and the concentration of hydroxyethyl cellulose is 6 mg / L;
[0074] The rest is the same as in Example 1.
[0075] Comparative Example 6
[0076] The difference between this comparative example and Example 1 is that the specific operation of step (5) of anti-diffusion barrier layer treatment is: placing the copper foil after the curing treatment in the anti-diffusion barrier layer liquid for passivation treatment;
[0077] In the diffusion barrier layer liquid, the concentration of cobalt ions is 1.5 g / L, the concentration of nickel ions is 1.5 g / L, and the concentration of molybdenum ions is 1.5 g / L;
[0078] The conditions for the diffusion barrier treatment are: current density 15A / dm 2 , temperature is 38℃, and passivation treatment time is 5s.
[0079] The rest is the same as in Example 1.
[0080] Test example
[0081] The surface treated copper foils of Examples 1-3 and Comparative Examples 1-6 were subjected to roughness R Z Test and peel strength test. Among them, the roughness R Z Tested with a roughness meter; Peel strength: refer to "7.4 Separation strength of thin copper foil and carrier" in GB / T29847-2013; specific test results are shown in Table 1.
[0082] Table 1
[0083] Group <![CDATA[Roughness R Z (μm)]]> Peel strength(N / mm) Example 1 1.21 2.06 Example 2 1.30 2.14 Example 3 1.18 2.01 Comparative Example 1 2.15 2.34 Comparative Example 2 1.28 1.75 Comparative Example 3 1.67 1.96 Comparative Example 4 1.74 2.12 Comparative Example 5 1.88 2.28 Comparative Example 6 1.64 2.20
[0084] From the results in Table 1, it can be seen that the copper foil treated by the surface treatment process of the present invention has a lower surface roughness R Z , and the anti-peeling is still superior to that in the comparative example. It can be seen that the surface treatment process of the present invention realizes the control of the copper nodule morphology on the copper foil surface, and balances the reduction of the copper foil roughness while achieving the two-way requirements of high peel strength; it can be used to prepare printed circuit boards to better meet the characteristics of fast high-frequency signal transmission and low loss in the 5G field. In comparative example 1, only a conventional roughening treatment step was used, and the copper foil surface formed uneven dendritic copper nodules, and the copper foil obtained by the final treatment had a high roughness R Z In Comparative Example 2, the secondary roughening treatment step was directly adopted without the primary roughening treatment. It was found that the final copper foil roughness R Z The peel strength is significantly lower than that in the example, indicating that omitting the first roughening step will affect the structure of the coating, thereby affecting the peel strength of the copper foil. In Comparative Examples 3-5, the components of the roughening solution in the second roughening step were adjusted, and it was found that the adjustment of the components of the roughening solution would affect the morphology of the copper nodules on the surface of the copper foil, making the surface roughness R Z Increase, resulting in roughness R ZIn Comparative Example 6, the anti-diffusion barrier layer was not deposited using magnetron sputtering technology, but using conventional electrodeposition method. The surface roughness R Z Significant improvement.
[0085] Finally, it should be noted that the above-mentioned embodiments only express several implementation methods of the present invention and are not intended to limit the invention. For those skilled in the art, any modification, equivalent replacement, improvement, etc. made without departing from the concept of the present invention should be included in the protection scope of the invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A copper foil surface treatment process, characterized in that: The following steps are involved: (1) Pickling treatment: placing the raw copper foil in a pickling solution for pickling treatment; (2) Primary roughening treatment: placing the pickled copper foil in a primary roughening solution for roughening treatment; (3) Secondary roughening treatment: placing the copper foil after the primary roughening treatment in a secondary roughening solution for roughening treatment; (4) Curing treatment: placing the copper foil after the secondary roughening treatment in a curing liquid for curing treatment; (5) Anti-diffusion barrier layer treatment: using magnetron sputtering vacuum coating technology to sputter an anti-diffusion barrier layer on the surface of the copper foil after curing; (6) Passivation treatment: placing the copper foil treated with the diffusion barrier layer in a passivation solution for passivation treatment; (7) Silanization and drying treatment: The copper foil after passivation treatment is immersed in a silane coupling agent solution, and then dried with hot air to complete the surface treatment of the copper foil.
2. The process according to claim 1, characterized in that: The pickling solution in step (1) is a sulfuric acid solution with a concentration of 10-20wt%, and the pickling time is 3-5s.
3. The process according to claim 1, characterized in that: In step (2), the concentration of sulfuric acid in the primary roughening solution is 80-120 g / L, the concentration of copper ions is 6-12 g / L, and the concentration of chloride ions is 30-35 mg / L; The conditions for the primary roughening treatment are: current density 25-35A / dm 2 , temperature 25-35℃, electrodeposition time 2-3s.
4. The process according to claim 1, characterized in that: In step (3), the concentration of sulfuric acid in the secondary roughening solution is 80-120 g / L, the concentration of copper ions is 6-12 g / L, the concentration of gelatin is 80-120 mg / L, the concentration of sodium thiopropane sulfonate is 8-12 mg / L, the concentration of PEG is 5-8 mg / L, and the concentration of hydroxyethyl cellulose is 5-8 mg / L; The conditions for the secondary roughening treatment are: current density 25-35A / dm 2 , temperature 25-35℃, electrodeposition time 4-6s.
5. The process according to claim 1, characterized in that: Step (4) The concentration of sulfuric acid in the solidifying liquid is 80-120 g / L, and the concentration of copper ions is 50-60 g / L; The curing conditions are: current density 25-35A / dm 2 , temperature 45-55℃, electrodeposition time 5-10s.
6. The process according to claim 1, characterized in that: Step (5) The magnetron sputtering vacuum coating technology uses CoNiMo alloy as the target material.
7. The process according to claim 6, characterized in that: The element atomic ratio of the CoNiMo alloy is 1:1:1, and the thickness of the anti-diffusion barrier layer is 5-20nm.
8. The process according to claim 1, characterized in that: Step (6) Cr0 in the passivation solution 2 4 - The concentration is 2.0-2.5g / L, the concentration of K4P2O7 is 70-100g / L, and the pH value of the passivation solution is 11-12; The passivation treatment conditions are: current density 2.5-3.5A / dm 2 , temperature is 35-45℃, and passivation treatment time is 5-10s.
9. The process according to claim 1, characterized in that: The concentration of the silane coupling agent solution in step (7) is 5-8 g / L, and the soaking time is 2-5 s.
10. The process according to claim 1, characterized in that: The hot air drying temperature in step (7) is 180-220°C.