Iridium black nano-catalyst for PEM water electrolysis hydrogen production and preparation method of iridium black nano-catalyst
The preparation of iridium black nanocatalysts through hydrothermal reaction under alkaline conditions solves the problems of complex synthesis and high cost of existing iridium-based catalysts, and achieves high activity and stability of iridium black nanocatalysts for proton exchange membrane electrolysis of water production. Hydrogen significantly improves catalytic performance and stability.
Patent Information
- Application Number
- CN202410766934.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing iridium-based catalyst synthesis methods are complex, time-consuming, high-cost and have low catalytic activity, which limits its application in the process of electrolyzing water to produce hydrogen.
The hydrothermal reaction between iridium chloride and organic ligands is carried out under alkaline conditions, and the iridium black nanocatalyst is obtained through reduction with a reducing agent. An iridium black nanocatalyst with smaller size and uniform particle distribution is prepared for proton exchange membrane electrolysis of water. Hydrogen production.
It significantly reduces the anode oxygen evolution overpotential, increases the reaction current, has excellent catalytic performance, has good use stability, simplifies the synthesis process, reduces the cost, and is suitable for large-scale production.
Smart Images

Figure CN118773645A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nano material synthesis and electrocatalysis, and in particular to an iridium black nano catalyst for PEM water electrolysis to produce hydrogen and a preparation method thereof. Background Art
[0002] Hydrogen energy is becoming an important part of the global energy transformation due to its advantages such as cleanliness, environmental protection and renewable nature. In terms of green production of hydrogen energy, water electrolysis is undoubtedly the current mainstream technology. Hydrogen production by water electrolysis is a method of producing hydrogen by providing energy to water through electricity and destroying the hydrogen-oxygen bonds of water molecules. The process is simple and pollution-free, and is considered to be one of the most promising ways to efficiently and cleanly produce ultra-pure hydrogen. The water electrolysis process includes two half reactions: the hydrogen evolution reaction (HER) at the cathode and the oxygen evolution reaction (OER) at the anode. Among them, the cathode HER is a relatively simple two-electron transfer process that can occur at a lower potential; but the anode OER process requires a four-electron transfer process, and the kinetic reaction rate is low, which is the rate-controlling step that restricts the efficiency of hydrogen production by water electrolysis.
[0003] Proton exchange membrane water electrolysis has huge advantages over traditional alkaline water electrolysis. First of all, proton exchange membrane water electrolysis can directly use pure water as the electrolyte instead of highly corrosive acid and alkali solutions. Furthermore, thanks to the thinner proton exchange membrane and its excellent ion conductivity, proton exchange membrane water electrolysis can have a current density several times that of alkaline water electrolysis, and can also respond to the start and stop of current within seconds. At the same current density, proton exchange membrane water electrolysis technology has a higher thermal conversion efficiency and can better adapt to fluctuating electricity such as wind energy and solar energy.
[0004] Anode catalyst is one of the key materials for hydrogen production by proton exchange membrane water electrolysis. Under normal circumstances, the anode overpotential is much higher than that of the cathode. Therefore, an anode catalyst with excellent catalytic performance is one of the main factors determining the efficiency of hydrogen production by water electrolysis.
[0005] Iridium-based catalysts (iridium black and its oxides) have the characteristics of high stability, high catalytic activity, strong oxidation resistance and acid and alkali corrosion resistance, but their large-scale application is hindered by their high cost and low reserves. Patent CN113802130B discloses a water electrolysis catalyst and a preparation method thereof. The water electrolysis catalyst includes a substrate, the substrate is Nb-SnO2, and the substrate is loaded with Ir and Ru bimetallics, and the atomic ratio of Ir / Ru is 5 / 1 to 1 / 5. This patent uses Ir / Ru to form a bimetallic catalyst, which is costly and limits its large-scale application. Patent CN114481196B discloses a supported iridium-based catalyst thin layer and a preparation method thereof, which uses electrochemical deposition technology to achieve uniform loading of iridium oxide on the surface of a nanorod array carrier to form a nanorod array membrane electrode with a double-layer structure, which can achieve 10 to 200 μg cm -2The iridium loading range is much larger than that of the membrane electrode prepared by the traditional spraying method (1-2 mg cm -2 ), which has obvious advantages, but its preparation process has many steps and the operation is complicated.
[0006] The current synthesis process of iridium-based catalysts is complex, time-consuming, and costly, and the synthesized catalysts have low catalytic activity. Therefore, it is crucial to explore anode catalysts with low noble metal usage, high catalytic activity, and stability. Summary of the invention
[0007] The purpose of the present invention is to provide an iridium black nanocatalyst for PEM water electrolysis to produce hydrogen and a preparation method thereof, aiming to solve the problems of the existing iridium-based catalyst synthesis method, such as complex operation, long time consumption, high cost and low catalyst activity.
[0008] The present invention is specifically implemented by the following technical scheme. According to the preparation method of an iridium black nanocatalyst proposed by the present invention, the method specifically comprises the following steps:
[0009] Dissolve chloroiridic acid and a certain amount of organic ligand in a certain volume of ultrapure water, stir at room temperature for 30 to 120 minutes, then adjust the pH of the reaction solution to 8 to 9, add a reducing agent to the reaction solution, transfer the obtained reaction mixture to a stainless steel high-pressure reactor lined with polytetrafluoroethylene for hydrothermal reaction at 100 to 140° C. for 8 to 12 hours, and after the reaction is completed, wash the reaction product several times with ultrapure water by centrifugation, and obtain the iridium black nanocatalyst after drying.
[0010] In the aforementioned method for preparing the iridium black nanocatalyst, the organic ligand is selected from one or more of C4-C8 organic polyacids and their soluble salts, preferably citric acid, sodium alginate or aspartic acid.
[0011] In the preparation method of the iridium black nanocatalyst, the mass percentage of iridium in the chloroiridic acid is 35%, the organic ligand is sodium alginate, and the ratio of the mass of sodium alginate to the volume of the chloroiridic acid is 110 mg:1 mL.
[0012] In the aforementioned method for preparing the iridium black nanocatalyst, the reducing agent is sodium borohydride.
[0013] Preferably, the reducing agent is a sodium borohydride solution with a concentration of 3.8 mg / mL, and the volume ratio of the sodium borohydride solution to chloroiridic acid is 2:1.
[0014] The aforementioned method for preparing the iridium black nanocatalyst can use one or more of sodium carbonate solution, sodium bicarbonate solution, and sodium hydroxide solution to adjust the pH value of the solution to 8-9.
[0015] In the above-mentioned preparation method of iridium black nanocatalyst, during centrifugal washing, when the conductivity value of the supernatant after centrifugal washing is detected to be close to pure water or its pH value is neutral, the washing operation can be ended. Preferably, the washing operation is ended when the conductivity value of the supernatant after washing is detected to be close to pure water.
[0016] The above-mentioned preparation method of iridium black nano-catalyst is finally dried in a blast drying oven. The drying temperature can be 60-70° C. and the drying time is 10-24 hours.
[0017] Furthermore, the present invention also provides an iridium black nanocatalyst obtained according to the above preparation method and its application as an anode catalyst in PEM water electrolysis hydrogen production. The iridium black nanocatalyst is in the form of nanoparticles with a particle size of about 2 to 3 nm and uniform size. Its XRD spectrum includes Ir's (111) crystal plane diffraction peak, (002) crystal plane diffraction peak, (022) crystal plane diffraction peak, (113) crystal plane diffraction peak and (222) crystal plane diffraction peak.
[0018] Compared with the prior art, the present invention has obvious advantages and beneficial effects. By means of the above technical solution, the present invention can achieve considerable technical progress and practicality, and has a wide range of utilization value, and has at least the following advantages:
[0019] The present invention uses chloroiridic acid as a raw material, combines it with an organic ligand, reduces it with a reducing agent under alkaline conditions, and performs a hydrothermal reaction. The "one-pot method" prepares a small-sized, uniformly distributed iridium black nanocatalyst. The iridium black nanocatalyst has an ultrafine size, is in the form of nanoparticles, has a particle size of about 2 to 3nm, has a uniform size, and has good conductivity and electrochemical stability. It is used as an anode catalyst for PEM water electrolysis to produce hydrogen, which can significantly reduce the anode oxygen evolution overpotential, increase the reaction current, have excellent catalytic performance, and have good use stability.
[0020] The synthesis method of the iridium black nanocatalyst provided by the invention is simple, has few operation steps, is short in time consumption, has low cost, does not require expensive instruments and equipment, has readily available raw materials, is economical and environmentally friendly, and is easy to mass produce. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is the XRD pattern of the ultrafine-sized iridium black nanocatalyst prepared in Example 1;
[0022] Figure 2 TEM images of the ultrafine-sized iridium black nanocatalyst prepared in Example 1 at different magnifications;
[0023] Figure 3 is a comparison diagram of LSV curves of the ultrafine-sized iridium black nanocatalyst prepared in Example 1 and the commercial iridium black catalyst in Comparative Example 1 under acidic conditions for oxygen evolution reaction;
[0024] Figure 4 This is a stability test effect diagram of the ultrafine-sized iridium black nanocatalyst prepared in Example 1. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] The chloroiridic acid described in the following examples is commercially available chloroiridic acid, and the mass percentage of iridium is 35%.
[0027] Example 1
[0028] A method for synthesizing an ultrafine-sized iridium black nanocatalyst comprises the following steps:
[0029] First, 1 mL of chloroiridic acid and 110 mg of sodium alginate were dissolved in 30 mL of ultrapure water and magnetically stirred at room temperature for 30 min. Then, 2 mol / L of sodium carbonate solution was added to adjust the pH of the reaction solution to 9.0, and 2 mL of 3.8 mg / mL NaBH4 solution was added to the reaction solution. The mixture was then transferred to a 50 mL polytetrafluoroethylene-lined stainless steel autoclave and heated at 120 ° C for 10 h. After the hydrothermal reaction was completed, the reaction product was centrifuged and washed several times with ultrapure water, and then dried in a 70 ° C vacuum oven for 10 h to obtain an ultrafine size iridium black nanocatalyst.
[0030] Example 2
[0031] A preparation method of iridium black nanocatalyst comprises the following steps:
[0032] First, 1 mL of chloroiridic acid and 110 mg of sodium alginate were dissolved in 30 mL of ultrapure water and magnetically stirred at room temperature for 30 min. Then, 2 mol / L of sodium carbonate solution was added to adjust the pH of the reaction solution to 9.0, and 2 mL of 3.8 mg / mL NaBH4 solution was added to the reaction solution. The mixture was then transferred to a 50 mL polytetrafluoroethylene-lined stainless steel autoclave and heated at 100 ° C for 10 h. After the hydrothermal reaction was completed, the reaction product was centrifuged and washed several times with ultrapure water, and then dried in a 70 ° C vacuum oven for 10 h to obtain an ultrafine size iridium black nanocatalyst.
[0033] Example 3
[0034] A preparation method of iridium black nanocatalyst comprises the following steps:
[0035] First, 1 mL of chloroiridic acid and 110 mg of sodium alginate were dissolved in 30 mL of ultrapure water and magnetically stirred at room temperature for 30 min. Then, 2 mol / L of sodium carbonate solution was added to adjust the pH of the reaction solution to 9.0, and 2 mL of 3.8 mg / mL NaBH4 solution was added to the reaction solution. The mixture was then transferred to a 50 mL polytetrafluoroethylene-lined stainless steel autoclave and heated at 140 ° C for 10 h. After the hydrothermal reaction was completed, the reaction product was centrifuged and washed several times with ultrapure water, and then dried in a 70 ° C vacuum oven for 10 h to obtain an ultrafine size iridium black nanocatalyst.
[0036] Example 4
[0037] A preparation method of iridium black nanocatalyst comprises the following steps:
[0038] First, 1 mL of chloroiridic acid and 110 mg of sodium alginate were dissolved in 30 mL of ultrapure water and magnetically stirred at room temperature for 30 min. Then, 2 mol / L of sodium carbonate solution was added to adjust the pH of the reaction solution to 9.0, and 2 mL of 3.8 mg / mL NaBH4 solution was added to the reaction solution. The mixture was then transferred to a 50 mL polytetrafluoroethylene-lined stainless steel autoclave and heated at 120 ° C for 8 h. After the hydrothermal reaction was completed, the reaction product was centrifuged and washed several times with ultrapure water, and then dried in a 70 ° C vacuum oven for 10 h to obtain an ultrafine size iridium black nanocatalyst.
[0039] Example 5
[0040] A preparation method of iridium black nanocatalyst comprises the following steps:
[0041] First, 1 mL of chloroiridic acid and 110 mg of sodium alginate were dissolved in 30 mL of ultrapure water and magnetically stirred at room temperature for 30 min. Then, 2 mol / L of sodium carbonate solution was added to adjust the pH of the reaction solution to 9.0, and 2 mL of 3.8 mg / mL NaBH4 solution was added to the reaction solution. The mixture was then transferred to a 50 mL polytetrafluoroethylene-lined stainless steel autoclave and heated at 120 ° C for 12 h. After the hydrothermal reaction was completed, the reaction product was centrifuged and washed several times with ultrapure water, and then dried in a 70 ° C vacuum oven for 10 h to obtain an ultrafine size iridium black nanocatalyst.
[0042] Comparative Example 1
[0043] A commercial iridium black catalyst was used, purchased from Alfa, product number: 010746.
[0044] Comparative Example 2
[0045] A commercial iridium oxide catalyst was used, purchased from Sigma Aldrich, product number 206237.
[0046] XRD test instrument adopts Japan-Rigaku-SmartLab 9kW, Cu-Kα diffraction The TEM+Mapping test instrument uses JEOL JEM-ARM200F Cs-corrected S / TEM for HAADF-STEM tomography.
[0047] The ultrafine size iridium black nanocatalyst prepared in Example 1 was characterized, and its XRD spectrum was as follows: Figure 1 As shown, in order to confirm the formation of the iridium black structure, a typical X-ray diffraction (XRD) test of Ir was carried out. There were five obvious peaks at 40.7°, 47.3°, 69.2°, 83.5° and 88.1°, corresponding to the (111) crystal plane diffraction peak, (002) plane diffraction peak, (022) plane diffraction peak, (113) plane diffraction peak and (222) plane diffraction peak, respectively. The results calculated according to the half-peak width showed that the average particle size of the ultrafine-sized iridium black nanocatalyst was 2.05 nm, indicating that extremely small-sized nanoparticles were synthesized.
[0048] Figure 2 TEM images of the ultrafine iridium black nanocatalyst prepared in Example 1 at different magnifications are shown in FIG. Figure 2 It can be seen that the ultrafine-sized iridium black nanocatalyst is in the form of nanoparticles, the particle size is about 2 to 3 nm, and the particles are evenly distributed.
[0049] Weigh 10 mg of the ultrafine iridium black nanocatalyst prepared in Examples 1 to 5 and the catalysts of Comparative Examples 1 and 2, respectively, add 109 μL of 5% Nafion solution, 542 μL of ultrapure water and 1349 μL of isopropanol to each catalyst to prepare a catalyst mixture, and ultrasonicate the catalyst mixture for at least 2 hours to mix it evenly. Use a pipette to take 15 μL of the catalyst mixture and evenly drop it on the surface of the glassy carbon electrode three times and dry it with an infrared lamp as the working electrode of the three-battery system, the saturated calomel electrode as the reference electrode, the platinum sheet as the counter electrode, and the electrolyte is a 0.5M H2SO4 solution. The OER performance of the catalyst is tested at room temperature.
[0050] Figure 3 The LSV curves of the ultrafine iridium black nanocatalyst prepared in Example 1 and the commercial iridium black catalyst in Comparative Example 1 under acidic conditions are compared. It can be seen that at 10 mA cm -2 At a current density of , the iridium black nanocatalyst prepared in Example 1 has a smaller overpotential than the commercial iridium black catalyst in Comparative Example 1, indicating that the ultrafine-sized iridium black nanocatalyst prepared in the present invention has better acidic oxygen evolution reaction activity than the commercial iridium black catalyst.
[0051] Figure 4 The stability test effect diagram of the ultrafine size iridium black nanocatalyst prepared in Example 1, wherein the dotted line is the initial LSV curve of the ultrafine size iridium black nanocatalyst prepared in Example 1 as a working electrode, and the solid line is the LSV curve after 30000 cycles. Figure 4 It can be seen that after 30,000 cycles, the overpotential of the ultrafine-sized iridium black nanocatalyst prepared in Example 1 as a working electrode only increased by 21 mV.
[0052] The initial overpotential and the final overpotential after 30,000 cycles of the catalysts of Examples 1 to 5 and Comparative Examples 1 to 2 were tested in the same manner. The results are shown in Table 1 below:
[0053] Table 1. Electrochemical performance test results of catalysts of Examples 1 to 5 and Comparative Examples 1 to 2
[0054]
[0055] As shown in Table 1, the initial overpotentials of the ultrafine-sized iridium black nanocatalysts prepared in Examples 1 to 5 are lower than those of the commercial iridium black catalyst (Comparative Example 1) and the commercial iridium oxide catalyst (Comparative Example 2). After 30,000 cycles, the final overpotentials of the ultrafine-sized iridium black nanocatalysts prepared in Examples 1 to 5 are significantly lower than the overpotential increases of the catalysts in Comparative Examples 1 and 2 compared to the initial overpotential, indicating that the ultrafine-sized iridium black nanocatalysts prepared by the method of the present invention have both high activity and high stability.
[0056] The synthesis method of the iridium black nanocatalyst provided by the present invention is simple, has few operation steps, short time consumption, low cost, no need for expensive instruments and equipment, easy to obtain raw materials, economical and environmentally friendly, easy to scale production, and the prepared iridium black nanoparticle catalyst has a small particle size and a uniform structure. The iridium black nanocatalysts prepared in all embodiments have achieved significant effects in OER reactions, and the current density reaches 10 mA cm -2 The overpotential is less than 300mV; in particular, the overpotential of the catalyst prepared in Example 1 is only 258mV, which is much better than the commercial iridium-based catalyst. The iridium black nanocatalyst prepared by the present invention has excellent stability. After 30,000 cycles, the overpotential increase is less than the overpotential increase of the commercial iridium-based catalyst, indicating that it has excellent stability.
[0057] The above is only an embodiment of the present invention, and does not limit the present invention in any form. The present invention can also have other forms of embodiments according to the above structures and functions, which are not listed one by one. Therefore, any simple modification, equivalent change and modification made by any technician familiar with the profession to the above embodiment according to the technical essence of the present invention without departing from the scope of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A method for preparing an iridium black nanocatalyst, characterized in that The following steps are involved: Dissolve chloroiridic acid and a certain amount of organic ligand in a certain volume of ultrapure water, stir at room temperature for 30 to 120 minutes, then adjust the pH of the reaction solution to 8 to 9, add a reducing agent to the reaction solution, transfer the obtained reaction mixture to a stainless steel high-pressure reactor lined with polytetrafluoroethylene for hydrothermal reaction at 100 to 140° C. for 8 to 12 hours, and after the reaction is completed, wash the reaction product several times with ultrapure water by centrifugation, and obtain the iridium black nanocatalyst after drying.
2. The method for preparing the iridium black nanocatalyst as claimed in claim 1, characterized in that The organic ligand is selected from one or more of C4-C8 organic polyacids and soluble salts thereof.
3. The preparation method of iridium black nano catalyst as claimed in claim 1, characterized in that The organic ligand is citric acid, sodium alginate or aspartic acid.
4. The method for preparing the iridium black nanocatalyst as claimed in claim 1, characterized in that The mass percentage of iridium in the chloroiridic acid is 35%, the organic ligand is sodium alginate, and the ratio of the mass of sodium alginate to the volume of chloroiridic acid is 110 mg:1 mL.
5. The method for preparing the iridium black nanocatalyst as claimed in claim 1, characterized in that The reducing agent is sodium borohydride, and one or more of sodium carbonate solution, sodium bicarbonate solution and sodium hydroxide solution are used to adjust the pH value of the solution to 8-9.
6. The method for preparing the iridium black nanocatalyst as claimed in claim 1, characterized in that The reducing agent is a sodium borohydride solution with a concentration of 3.8 mg / mL, and the volume ratio of the sodium borohydride solution to chloroiridic acid is 2:
1.
7. The method for preparing the iridium black nanocatalyst as claimed in claim 1, characterized in that The drying temperature is 60-70°C and the drying time is 10-24h.
8. The iridium black nanocatalyst obtained by the preparation method according to any one of claims 1 to 7, which is in the form of nanoparticles with a particle size of 2 to 3 nm.
9. Use of the iridium black nanocatalyst as claimed in claim 8 as an anode catalyst in PEM water electrolysis to produce hydrogen.
Citation Information
Cited By
High-conductivity Ir-coated TiO2 anode catalyst, preparation method and application of high-conductivity Ir-coated TiO2 anode catalyst in proton exchange membrane electrolytic cell
CN116121807A
Highly conductive ir@tio2 anode catalyst, preparation method and application thereof in proton exchange membrane electrolyzer