Preparation method of indium phosphide single crystal and stepped crucible for indium phosphide single crystal growth

By using a stepped crucible and a vertical gradient condensation method in the same reaction space to grow indium phosphide single crystals at a decreasing condensation growth rate, the problems of high production cost and uneven electrical properties of large-sized indium phosphide single crystals are solved, and high efficiency is achieved. , low-cost and high-quality indium phosphide single crystal production.

CN118773718APending Publication Date: 2024-10-15GUANGDONG XIANRUI TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411083679.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing technology is difficult to produce large-sized indium phosphide single crystals at high efficiency and low cost, leading to problems such as low yield, high dislocation density and uneven electrical properties.

Method used

Using the stepped crucible and vertical gradient condensation method, indium phosphide single crystals of different sizes are grown in the same reaction space through decreasing condensation growth rates. The mixed melt of indium phosphide polycrystal and S powder is used for condensation growth and control. temperature gradient and taper angle to improve yield and electrical performance uniformity.

Benefits of technology

It is possible to grow indium phosphide single crystals of different sizes in the same reaction space, with the maximum size up to 6 inches. The yield is high, the dislocation density is low, and the electrical properties are uniform, which significantly improves the production of indium phosphide single crystals. efficiency and quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention relates to the field of semiconductors, in particular to a preparation method of an indium phosphide single crystal and a stepped crucible for indium phosphide single crystal growth. According to the preparation method provided by the invention, indium phosphide single crystals with different sizes can be prepared in the same reaction space, the maximum size can reach 6 inches, the yield is high, the dislocation density (EPD) is low, and the electrical property uniformity is good. Experiments show that through the preparation method, the indium phosphide single crystals with three sizes are prepared at the same time, the yield of the grown 6-inch indium phosphide single crystals can reach 25% or above, the EPD can be lower than 1500 / cm < 2 >, and the electrical property uniformity reaches 90% or above; and the crystal forming rate, EPD and electrical property uniformity of the indium phosphide single crystal are obviously superior to those of the indium phosphide single crystal grown at different condensation rates in an equal-diameter growth container.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of semiconductors, in particular to a method for preparing an indium phosphide single crystal and a stepped crucible for growing the indium phosphide single crystal. Background Art

[0002] Indium phosphide (InP) is a III-V compound semiconductor composed of IIIA element indium (In) and VA element phosphorus (P). The crystal is dark gray, with a molecular weight of 145.8 and a density of 4.78 g / cm 3 , microhardness 435±20 / mm. It has zinc blende crystal structure, lattice constant 5.869A. Bandgap width 1.35 eV at room temperature, direct transition type energy band structure, emission wavelength 0.92 μm.

[0003] At present, the mainstream technology for growing single crystals of indium phosphide is the VGF method, which is to load the synthesized indium phosphide polycrystals, B2O3 and seed crystals into a PBN crucible and seal them in a vacuum quartz tube. The furnace body is placed vertically and heated by a resistance wire. The quartz tube is placed vertically in the middle of the furnace body. After the indium phosphide polycrystal is melted at high temperature, it is welded with the indium phosphide single crystal seed crystal. Under a certain temperature gradient, the indium phosphide single crystal slowly grows upward from the end of the indium phosphide single crystal seed crystal. The VGF method has the advantages of small thermal field temperature gradient and low dislocation density of the grown crystal. However, due to the small decomposable critical shear stress (CRSS) and stacking fault energy of indium phosphide, the preparation process of indium phosphide single crystal is more difficult than that of GaAs, and the crystallization rate is lower. Therefore, the production cost of indium phosphide single crystal is high, and its current output is still far lower than that of GaAs.

[0004] The current mainstream size of indium phosphide substrates is 3-inch products, and the entire market is relatively mature. With the development of technologies such as crystal growth and epitaxy, the market is gradually moving towards 4-6 inches. Compared with 3-inch indium phosphide products, large-size indium phosphide has a larger available area and lower costs in epitaxy and related processing. According to the development trend of the semiconductor industry, 4-6-inch indium phosphide products will be the mainstream of the industry in the future.

[0005] Some companies in the industry have developed 6-inch indium phosphide products, but the entire industry is still immature and has not yet formed a stable supply chain. In addition, the yield of 6-inch indium phosphide products is low, with an EPD as high as 5000 / cm 2 The above problems include uneven electrical properties. Summary of the invention

[0006] In view of this, the technical problem to be solved by the present invention is to provide a method for preparing an indium phosphide single crystal and a stepped crucible for growing an indium phosphide single crystal. The preparation method provided by the present invention can prepare indium phosphide single crystals of different sizes in the same reaction space, with a maximum size of up to 6 inches, a high yield, a low dislocation density (EPD), and good uniformity of electrical properties.

[0007] The present invention provides a method for preparing an indium phosphide single crystal, comprising the following steps:

[0008] The indium phosphide single crystal seed crystal is condensed and grown in a mixed molten liquid of indium phosphide polycrystal and S powder in the stepped space to obtain an indium phosphide single crystal;

[0009] The stepped space includes a first area, a second area and a third area from bottom to top;

[0010] The diameters of the first area, the second area and the third area increase successively, and the diameter difference between adjacent areas is 25 mm to 50 mm;

[0011] The condensation growth rates of the indium phosphide single crystal seed crystal in the first region, the second region and the third region are independently 0.07 mm / h~0.12 mm / h, and the condensation growth rates of the indium phosphide single crystal seed crystal in the first region, the second region and the third region decrease successively.

[0012] The inventors of the present application creatively discovered that by growing indium phosphide single crystal seed crystals at a decreasing condensation growth rate in a stepped space with increasing diameters from bottom to top, not only can three indium phosphide single crystals with different diameters be grown in the same growth space, but also the yield is high, the dislocation density is low, and the electrical property uniformity is good.

[0013] The present invention condenses and grows an indium phosphide single crystal seed crystal in a mixed melt of indium phosphide polycrystal and S powder in a stepped space, wherein the stepped space includes a first region, a second region, and a third region from bottom to top; the first region is the lowest region, in which a small-diameter indium phosphide single crystal grows; the second region is the middle region, in which a medium-diameter single crystal grows; the third region is a large-diameter region, in which a large-diameter single crystal grows. In some embodiments of the present invention, the diameter of the first region is 50 mm to 100 mm; the diameter of the second region is 75 mm to 125 mm; and the diameter of the third region is 100 mm to 150 mm.

[0014] The cone angles between different step levels of the stepped space of the present invention are designed to be 60° to 135°; specifically, in the first region, the second region and the third region of the stepped space, adjacent regions are connected by cones of 60° to 135°. The gentle angle can keep the solid-liquid interface in the indium phosphide growth process in a convex state, thereby improving the yield rate.

[0015] The indium phosphide polycrystal and S powder mixed melt of the present invention is obtained by mixing and melting indium phosphide polycrystal and S powder; the weight of the S powder is 0.005% to 0.04% of the indium phosphide polycrystal. The indium phosphide polycrystal and S powder mixed melt of the present invention is prepared by the following method: melting indium phosphide polycrystal and S powder at 1070°C to 1200°C for 15 h to 30 h to obtain the indium phosphide polycrystal and S powder mixed melt. In certain embodiments of the present invention, the indium phosphide polycrystal and S powder are melted at 1070°C to 1100°C for 16 h to 24 h in an atmosphere with a vacuum degree of 1 MPa to 4 MPa to obtain the indium phosphide polycrystal and S powder mixed melt. The present invention allows the polycrystalline material to be in a molten liquid state, so that the impurity metal ions of indium phosphide are transferred to the tail of the crystal part under the action of segregation, so that the purity of the indium phosphide inside is higher.

[0016] The diameter of the S powder of the present invention is less than 1 mm; the indium phosphide polycrystal is an indium phosphide polycrystal with a particle size of less than 5 mm, preferably an indium phosphide polycrystal with a particle size of less than 3 mm. The present invention crushes the indium phosphide polycrystal into particles less than 5 mm, the diameter of the polycrystalline material becomes smaller, does not occupy more reaction space, and can be loaded into a crucible to grow longer and larger indium phosphide single crystals. At the same time, the polycrystalline material becomes small particles, which are easier to melt evenly when the material is heated at high temperature, so that the impurities of the indium phosphide melt are discharged to the tail of the crystal under the effect of segregation, which can improve the purity of the single crystal material and reduce the EPD of the crystal.

[0017] The present invention condenses and grows the indium phosphide single crystal seed crystal in a mixed melt of indium phosphide polycrystal and S powder in a stepped space by controlling the vertical gradient condensation method to obtain an indium phosphide single crystal. Specifically, the present invention condenses and grows the indium phosphide single crystal seed crystal in a mixed melt of indium phosphide polycrystal and S powder in a stepped space at a temperature of 1000°C to 1200°C, preferably at a temperature of 1070°C to 1100°C, at a temperature gradient condensation growth rate of 0.07 mm / h to 0.12 mm / h, so that the indium phosphide solid-liquid interface moves vertically upward from the bottom of the polycrystal, that is, the indium phosphide single crystal seed crystal condenses and grows from the first region of the stepped space to the third region of the stepped space, thereby obtaining an indium phosphide single crystal. In certain embodiments of the present invention, the condensation rate of the indium phosphide single crystal seed crystal in the first region is 0.1 mm / h~0.12 mm / h; the condensation rate of the indium phosphide single crystal seed crystal in the second region is 0.08 mm / h~0.11 mm / h; the condensation rate of the indium phosphide single crystal seed crystal in the third region is 0.07 mm / h~0.1 mm / h.

[0018] In certain embodiments of the present invention, when the indium phosphide single crystal seed crystal is condensed and grown in a mixed molten liquid of indium phosphide polycrystal and S powder in a stepped space, boron oxide is also required to be added. The boron oxide serves as a liquid sealant. After the high-temperature boron oxide melts, it will float on the top of the indium phosphide single crystal to prevent the top of the indium phosphide from decomposing and enriching indium under high-temperature conditions. The mass ratio of the boron oxide to the indium phosphide polycrystal is (50 g~100 g): (10 kg~15 kg).

[0019] The present invention also provides an indium phosphide single crystal obtained by any of the above technical solutions. In certain embodiments of the present invention, the obtained indium phosphide single crystal includes an indium phosphide single crystal with a crystal diameter of 50 mm to 75 mm, an indium phosphide single crystal with a crystal diameter of 75 mm to 100 mm, and an indium phosphide single crystal with a crystal diameter of 100 mm to 150 mm. The dislocation density of the indium phosphide single crystal obtained by the present invention is less than 1500 / cm 2 , the uniformity of electrical properties is over 90%.

[0020] The present invention also provides a stepped crucible for growing indium phosphide single crystals, which comprises a first region, a second region and a third region from bottom to top; the diameters of the first region, the second region and the third region increase successively, and the diameter difference between adjacent regions is 25 mm to 50 mm.

[0021] In the step-type crucible for growing indium phosphide single crystals of the present invention, the diameter of the first region is 50 mm to 100 mm; the diameter of the second region is 75 mm to 125 mm; the diameter of the third region is 100 mm to 150 mm; the first region is the lowest region, which can be used for the growth of small-diameter indium phosphide single crystals; the second region is the middle region, which can be used for the growth of medium-diameter single crystals; the third region is the large-diameter region, which can be used for the growth of large-diameter single crystals. The step-type crucible provided by the present invention can grow single crystals of three different diameters in the same crucible, with the smallest single crystal diameter being 2 inches (i.e., 50 mm) and the largest single crystal diameter being up to 6 inches (i.e., 150 mm).

[0022] In the step-type crucible for growing an indium phosphide single crystal of the present invention, adjacent regions in the first region, the second region and the third region of the step-shaped space are connected by a cone portion with an angle of 60° to 135°. The gentle angle can keep the solid-liquid interface in the indium phosphide growth process in a convex state, thereby improving the yield rate.

[0023] The present invention provides a method for preparing an indium phosphide single crystal and a stepped crucible for growing an indium phosphide single crystal. The preparation method provided by the present invention can prepare indium phosphide single crystals of different sizes in the same reaction space, with a maximum size of up to 6 inches, a high yield, a low dislocation density (EPD), and good uniformity of electrical properties. Experiments show that the present invention simultaneously prepares three sizes of indium phosphide single crystals through the preparation method, and the yield of the grown 6-inch indium phosphide single crystal can reach more than 25%, and the EPD can be lower than 1500 / cm 2 The uniformity of electrical properties reaches more than 90%. Whether it is the crystallization rate, EPD or electrical property uniformity, it is significantly better than the indium phosphide single crystal grown in an equal-diameter growth container at different condensation rates. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The external schematic diagram of the equipment for applying the method for preparing the indium phosphide single crystal of the present invention;

[0025] Figure 2 A schematic diagram of the internal materials of the equipment for applying the method for preparing the indium phosphide single crystal of the present invention;

[0026] Figure 3 The internal schematic diagram of the equipment for applying the method for preparing the indium phosphide single crystal of the present invention;

[0027] Figure 4 This is a schematic diagram of the 6-inch indium phosphide single crystal growth equipment used in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0028] The present invention discloses a method for preparing an indium phosphide single crystal and a stepped crucible for growing an indium phosphide single crystal. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve the same. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the method and application of this article without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.

[0029] The present invention will be further described below in conjunction with embodiments:

[0030] Example 1

[0031] Step 1: Place the cleaned and dried stepped boron nitride crucible, with the bottom layer diameter of 2 inches, the middle layer diameter of 3 inches, and the top layer diameter of 4 inches, into a matching stepped quartz tube; place a seed crystal in the seed crystal cavity of the boron nitride crucible, and then place 60 g of boron oxide;

[0032] The second step: vertically weld the quartz cap and the quartz tube with hydroxide, so that the quartz tube and the quartz cap are sealed, and the feed pipe on the top of the quartz cap is not sealed, and the indium phosphide polycrystalline particles are transported and the air in the tube is removed; Figure 1 As shown, Figure 1 The figure is a schematic diagram of the external structure of the equipment for applying the method for preparing the indium phosphide single crystal of the present invention, wherein 1-1 is a stepped boron nitride crucible, 1-2 is a stepped quartz tube, and 1-3 is a quartz cap feed tube;

[0033] Step 3: Pour 12 kg of indium phosphide polycrystalline particles with a diameter less than 5 mm and add 0.8 g of dopant S powder with a diameter less than 1 mm from the feed pipe of the quartz cap;

[0034] Step 4: After the quartz tube is loaded with polycrystalline material and S powder, the quartz cap feed tube is connected to the vacuum tube for vacuuming, and the air in the quartz tube is exhausted. When the vacuum degree reaches below -3 MPa, the quartz cap feed tube is welded and sealed with a hydrogen-oxygen flame; Figure 2 As shown, Figure 2 Schematic diagram of the internal materials of the equipment for applying the method for preparing indium phosphide single crystal of the present invention, in which 2-1 is a seed crystal, 2-2 is boron oxide, 2-3 is an indium phosphide polycrystalline particle, 2-4 is the welding place of the quartz cap feed pipe, and 2-5 is a vacuum pipe;

[0035] Step 5: Put the welded quartz tube into the single crystal growth furnace, use a quartz support tube to vertically support the quartz tube at the bottom of the furnace, and buckle the single crystal furnace cover to make the quartz tube completely covered in the single crystal growth furnace; Figure 3 As shown, Figure 3This is a schematic diagram of the internal structure of the equipment for applying the method for preparing indium phosphide single crystals of the present invention. In the figure, 3-1 is a loading quartz tube, 3-2 is a single crystal growth furnace, 3-3 is a 6-temperature zone heater, 3-4 is a supporting quartz tube, and 3-5 is a supporting platform.

[0036] Step 6: Heat to 1080°C to melt the polycrystalline material in the quartz tube and drip into the small diameter crucible at the bottom. After the indium phosphide polycrystalline material is melted, continue heating for 20 hours to make the polycrystalline material in a molten state;

[0037] Step 7: By controlling the vertical gradient condensation method, the temperature is controlled at 1070°C, so that the indium phosphide solid-liquid interface moves vertically upward from the bottom of the polycrystal. When growing a single crystal with a lower diameter of 2 inches, the temperature gradient condensation rate is controlled at 0.12 mm / h. When the middle layer diameter is 3 inches, the temperature gradient condensation rate is controlled at 0.1 mm / h. When the upper layer diameter is 4 inches, the temperature gradient condensation rate is controlled at 0.08 mm / h. The larger the diameter of the single crystal, the slower the condensation rate. Finally, the entire crystal rod is solidified into a crystal, cooled and taken out of the furnace to produce three sizes of S-doped semiconductor indium phosphide crystals with equal diameters of 2 inches, 3 inches and 4 inches.

[0038] Example 2

[0039] The difference from Example 1 is that when growing a single crystal with a lower layer diameter of 2 inches, the temperature gradient condensation rate is controlled at 0.12 mm / h, when growing to a middle layer diameter of 3 inches, the temperature gradient condensation rate is controlled at 0.11 mm / h, and when growing to an upper layer diameter of 4 inches, the temperature gradient condensation rate is controlled at 0.1 mm / h.

[0040] Example 3

[0041] The difference from Example 1 is that 12 kg of indium phosphide polycrystalline particles with a diameter less than 3 mm and 0.8 g of dopant S powder with a diameter less than 0.5 mm are added.

[0042] Example 4

[0043] Step 1: Place the cleaned and dried stepped boron nitride crucible, with the bottom layer diameter of 3 inches, the middle layer diameter of 4 inches, and the top layer diameter of 6 inches, into a matching stepped quartz tube; place a seed crystal in the seed crystal cavity of the boron nitride crucible, and then place 100 g of boron oxide;

[0044] Step 2: Use hydroxide to vertically weld the quartz cap and the quartz tube together, so that the quartz tube and the quartz cap are sealed, while the feed pipe on the top of the quartz cap is not sealed, and the indium phosphide polycrystalline particles are transported and the air in the tube is removed;

[0045] Step 3: Pour 15 kg of indium phosphide polycrystalline particles with a diameter less than 5 mm and add 1.2 g of dopant S powder with a diameter less than 1 mm from the feed pipe of the quartz cap;

[0046] Step 4: After the quartz tube is loaded with polycrystalline material and S powder, the quartz cap feed tube is connected to the vacuum tube for vacuuming to exhaust the air in the quartz tube. The vacuum degree reaches 4 MPa, and the quartz cap feed tube is welded and sealed with a hydrogen-oxygen flame;

[0047] Step 5: Put the welded quartz tube into the single crystal growth furnace, use a quartz support tube to vertically support the quartz tube at the bottom of the furnace, and buckle the single crystal furnace cover to make the quartz tube completely covered in the single crystal growth furnace;

[0048] Step 6: Heat to 1080°C to melt the polycrystalline material in the quartz tube and drip into the small diameter crucible at the bottom. After the indium phosphide polycrystalline material is melted, continue to heat for 24 hours to keep the polycrystalline material in a molten state.

[0049] Step 7: By controlling the vertical gradient condensation method, the temperature is controlled at 1070°C, so that the indium phosphide solid-liquid interface moves vertically upward from the bottom of the polycrystal. When growing a single crystal with a lower diameter of 3 inches, the temperature gradient condensation rate is controlled at 0.1 mm / h. When the middle layer diameter is 4 inches, the temperature gradient condensation rate is controlled at 0.08 mm / h. When the upper layer diameter is 6 inches, the temperature gradient condensation rate is controlled at 0.07 mm / h. The larger the diameter of the single crystal, the slower the condensation rate. Finally, the entire crystal rod is solidified into a crystal, cooled and taken out of the furnace, and three sizes of S-doped semiconductor indium phosphide crystals with equal diameters of 3 inches, 4 inches and 6 inches are produced for comparison.

[0050] Comparative Example 1

[0051] This comparative example provides a 6-inch indium phosphide single crystal growth device, such as Figure 4 As shown, Figure 4 This is a schematic diagram of a 6-inch indium phosphide single crystal growth device used in Comparative Example 1 of the present invention. This comparative example prepares an indium phosphide single crystal according to the following steps:

[0052] Step 1: The crucible for growing indium phosphide single crystal is a 6-inch cylindrical crucible with a funnel-shaped bottom and only one equal-diameter part; put the seed crystal into the seed crystal cavity of the boron nitride crucible, and then put in 100 g of boron oxide;

[0053] Step 2: Use hydroxide to vertically weld the quartz cap and the quartz tube together, so that the quartz tube and the quartz cap are sealed, while the feed pipe on the top of the quartz cap is not sealed, and the indium phosphide polycrystalline particles are transported and the air in the tube is removed;

[0054] Step 3: Pour 15 kg of indium phosphide polycrystalline particles with a diameter less than 5 mm and add 0.8 g of dopant S powder with a diameter less than 1 mm from the feed pipe of the quartz cap;

[0055] Step 4: After the quartz tube is loaded with polycrystalline material and S powder, the quartz cap feed tube is connected to the vacuum tube for vacuuming to exhaust the air in the quartz tube. When the vacuum degree reaches below -3 MPa, the quartz cap feed tube is welded and sealed with a hydrogen-oxygen flame.

[0056] Step 5: Put the welded quartz tube into the single crystal growth furnace, use a quartz support tube to vertically support the quartz tube at the bottom of the furnace, and buckle the single crystal furnace cover to make the quartz tube completely covered in the single crystal growth furnace;

[0057] Step 6: Heat to 1080°C to melt the polycrystalline material in the quartz tube and drip into the small diameter crucible at the bottom. After the indium phosphide polycrystalline material is melted, continue heating for 20 hours to make the polycrystalline material in a molten state;

[0058] Step 7: By controlling the vertical gradient condensation method, the temperature is controlled at 1070°C, so that the indium phosphide solid-liquid interface moves vertically upward from the bottom of the polycrystal. When growing the cone (i.e. the funnel-shaped part of the crucible), the temperature gradient condensation rate is controlled at 0.12 mm / h; when growing to the middle position from the funnel to the equal-diameter part, the temperature gradient condensation rate is controlled at 0.1 mm / h; when growing from the middle position to the tail of the crystal, the temperature gradient condensation rate is controlled at 0.08 mm / h. The closer the growth position is to the tail of the crystal, the slower the condensation rate. Finally, the entire crystal rod is solidified into a crystal, cooled and taken out of the furnace to produce a 6-inch equal-diameter S-doped semiconductor indium phosphide crystal.

[0059] The indium phosphide single crystals of Examples 1 to 4 and Comparative Example 1 were tested, and the results are shown in Table 1:

[0060] Table 1

[0061]

[0062] Note: The crystallization rate is the overall crystallization rate of three sizes of indium phosphide single crystals grown from a single crucible, that is, the crystallization rates of the three sizes are counted separately, and then the average value is calculated. From the test data of the single crystal material obtained in Example 1, it can be seen that for crystals of different diameters obtained from the same crystal rod, the smaller the diameter, the smaller the EPD, and the higher the uniformity of electrical properties. Compared with the test data of the single crystal materials obtained in Example 1 and Example 4, it can be seen that for crystal rods of different sizes made using crucibles of different sizes, the smaller the diameter of the same-level growth zone, the smaller the diameter of the obtained crystal, the smaller the EPD, and the higher the uniformity of electrical properties. The inventor explored the principle that: crystal rods with small diameters are more stably heated during the melting and crystal growth stages, and their performance is better.

[0063] Compared with the test data of the single crystal materials obtained in Example 1 and Example 3, it can be seen that when polycrystalline particles of different diameters are added, the smaller the diameter of the polycrystalline particles, the smaller the EPD and the more uniform the electrical properties. The inventors explored the principle that: the polycrystalline particles are small, the heat is more uniform, and it is easier to melt, and the impurities in the polycrystalline are easy to move to the tail of the crystal, making the interior of the crystal purer, with fewer heat dislocations, and better EPD.

[0064] Compared with the test data of the single crystal materials obtained in Example 1 and Example 2, it can be seen that the slower the temperature gradient condensation rate, the smaller the temperature difference in the crystal growth process, and the better the EPD and electrical properties. However, if the temperature gradient condensation rate is too slow, more energy will be consumed. Therefore, the temperature gradient condensation rate needs to be controlled within a reasonable range, so that it can reduce EPD and improve the uniformity of electrical properties, while reducing energy loss.

[0065] In comparative example 1, there is only one 6-inch indium phosphide single crystal with equal diameter, and the head, middle and tail have different temperature gradient condensation rates. The EPD of the grown indium phosphide crystal is relatively high, and the EPD of the head with a fast condensation rate is higher than that of the middle with a slow condensation rate. At the same time, there is only one 6-inch indium phosphide with equal diameter, and its yield is low.

[0066] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing an indium phosphide single crystal, It is characterized in that The following steps are involved: The indium phosphide single crystal seed crystal is condensed and grown in a mixed molten liquid of indium phosphide polycrystal and S powder in the stepped space to obtain an indium phosphide single crystal; The stepped space includes a first area, a second area and a third area from bottom to top; The diameters of the first area, the second area and the third area increase successively, and the diameter difference between adjacent areas is 25 mm to 50 mm; The condensation growth rates of the indium phosphide single crystal seed crystal in the first region, the second region and the third region are independently 0.07 mm / h~0.12 mm / h, and the condensation rates of the indium phosphide single crystal seed crystal in the first region, the second region and the third region decrease successively.

2. The preparation method according to claim 1, It is characterized in that The diameter of the first area is 50 mm to 100 mm; The diameter of the second area is 75 mm to 125 mm; The diameter of the third area is 100 mm to 150 mm.

3. The preparation method according to claim 1, It is characterized in that In the first area, the second area and the third area of ​​the stepped space, adjacent areas are connected by a taper portion with an angle of 60° to 135°.

4. The preparation method according to claim 1, It is characterized in that The condensation growth rate of the indium phosphide single crystal seed in the first region is 0.1 mm / h to 0.12 mm / h; The condensation growth rate of the indium phosphide single crystal seed in the second region is 0.08 mm / h to 0.11 mm / h; The condensation growth rate of the indium phosphide single crystal seed in the third region is 0.07 mm / h~0.1 mm / h.

5. The preparation method according to claim 1, It is characterized in that The weight of the S powder is 0.005% to 0.04% of the indium phosphide polycrystal.

6. The preparation method according to claim 1, It is characterized in that The indium phosphide polycrystal is an indium phosphide polycrystal particle with a diameter less than 5 mm; The diameter of the S powder is less than 1 mm.

7. The preparation method according to claim 1, It is characterized in that The mixed melt of indium phosphide polycrystal and S powder is prepared by the following method: The indium phosphide polycrystal and the S powder are melted at 1070° C. to 1200° C. for 15 h to 30 h to obtain a mixed melt of the indium phosphide polycrystal and the S powder.

8. A stepped crucible for growing indium phosphide single crystals, It is characterized in that From bottom to top, it includes a first area, a second area and a third area; The diameters of the first region, the second region and the third region increase successively, and the diameter difference between adjacent regions is 25 mm to 50 mm.

9. The step crucible for growing an indium phosphide single crystal according to claim 8, It is characterized in that The diameter of the first area is 50 mm to 100 mm; The diameter of the second area is 75 mm to 125 mm; The diameter of the third area is 100 mm to 150 mm.

10. The step crucible for growing an indium phosphide single crystal according to claim 8, It is characterized in that In the first area, the second area and the third area of ​​the stepped space, adjacent areas are connected by a taper portion with an angle of 60° to 135°.

Citation Information

Cited By

  • Preparation method of large-size P-type indium phosphide single crystal

    CN121183400A