P-type monocrystalline silicon and growth method thereof
By using a composite doping source of phosphorus and gallium arsenide in the preparation of P-type single crystal silicon, the uniform distribution of resistivity and the improvement of crystal strength are achieved, which solves the problem of unstable resistivity changes in the traditional process and improves the silicon The photoelectric conversion efficiency and production efficiency of the chip reduce the cost of photovoltaic power generation.
Patent Information
- Application Number
- CN202411051188.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-10-15
AI Technical Summary
In the traditional P-type monocrystalline silicon preparation process, a single doping of gallium causes the resistivity change trend to be too large and the crystal resistivity range to be too wide, affecting the processing of silicon wafers and photoelectric conversion efficiency, and making it difficult to meet high-efficiency, high-quality production needs.
A composite doping source of polycrystalline silicon, phosphorus and gallium arsenide is used to grow single crystal silicon by melting it in an inert atmosphere and introducing seed crystals to control the crystal growth rate and resistivity to achieve uniform distribution and improvement of resistivity.
It improves the uniformity of the resistivity distribution of P-type monocrystalline silicon, slows down the rapid decline of resistivity, enhances the strength and stability of the crystal rod, improves the photoelectric conversion efficiency and production efficiency of the silicon wafer, and reduces the cost.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the field of semiconductor technology, and particularly relates to a P-type single crystal silicon and a growth method thereof. Background Art
[0002] In order to fully, accurately and comprehensively implement the new development concept, we must seize the major opportunities for the development of new energy and consolidate the remarkable achievements made in the development of the photovoltaic industry. In the photovoltaic industry and the semiconductor industry, the performance optimization of single crystal silicon as a basic electronic material is crucial to improving the efficiency of the entire electronic equipment. Especially in terms of reducing power consumption, low-resistivity P-type single crystal silicon materials have attracted widespread attention due to their excellent optoelectronic properties and low production costs. In order to reduce the cost of front-end single crystal pulling of P-type Passivated Emitter and Rear Cell (PERC), the production of uniform single crystal silicon resistivity and ultra-thin silicon wafers has become an important technical challenge. .
[0003] At present, the preparation process of P-type monocrystalline silicon mainly relies on a single doping element such as gallium. However, this single gallium doping method often leads to a large resistivity change trend and a wide crystal resistivity range due to the low segregation coefficient of gallium in silicon, which in turn affects the subsequent processing of silicon wafers and the photoelectric conversion efficiency of batteries. In addition, with the rapid development of the photovoltaic industry, the quality requirements for P-type monocrystalline silicon materials are increasing, and traditional preparation processes can no longer meet the production needs of high efficiency and high quality. Summary of the invention
[0004] The object of the present invention is to provide a P-type single crystal silicon and a growth method thereof. Through the P-type single crystal silicon and a growth method thereof provided by the present invention, the resistivity of the P-type single crystal silicon can be improved, the resistivity distribution of the single crystal silicon is more uniform, the brittleness of the crystal rod can be improved, the strength of the single crystal silicon is increased, and an ultra-thin silicon wafer is obtained.
[0005] In order to solve the above technical problems, the present invention provides a method for growing P-type single crystal silicon, comprising the following steps:
[0006] uniformly mixing polycrystalline silicon and a doping source according to a mass ratio to obtain a mixed powder, wherein the doping source comprises phosphorus and gallium arsenide, and the molar ratio of the phosphorus to the gallium arsenide is 5-10:90-95; and
[0007] The mixed powder is melted at a preset temperature under an inert atmosphere, and a seed crystal is introduced to grow single crystal silicon.
[0008] In one embodiment of the present invention, the mass ratio of the polysilicon to the doping source is 40190:1 to 40200:1.
[0009] In one embodiment of the present invention, the preset temperature is 1450°C to 1550°C.
[0010] In one embodiment of the present invention, the single crystal silicon is grown by using a Czochralski method or a floating zone melting method.
[0011] In one embodiment of the present invention, the crystal growth rate of the single crystal silicon is controlled at 1.0 mm / min to 1.1 mm / min.
[0012] In one embodiment of the present invention, the crystal growth direction of the single crystal silicon is <100> The length of the obtained single crystal silicon rod is 3.5m to 4.2m.
[0013] In one embodiment of the present invention, the resistivity of the head of the crystal rod is 0.85Ω·cm to 1.1Ω·cm, and the resistivity of the tail of the crystal rod is 0.6Ω·cm to 1.0Ω·cm.
[0014] In one embodiment of the present invention, the crystal rod is sliced to obtain silicon wafers, and the thickness of the silicon wafers is 80 μm to 130 μm.
[0015] The present invention also provides a P-type single crystal silicon obtained by adopting the above-mentioned growth method.
[0016] In summary, the present invention provides a P-type single crystal silicon and a growth method thereof, which can improve the resistivity of P-type single crystal silicon, improve the resistivity of the tail of P-type single crystal silicon, make the resistivity distribution more uniform, slow down the rapid decline of resistivity, achieve effective control of the resistivity of single crystal silicon, and improve the utilization range of the crystal rod. It can improve the brittleness of the crystal rod, improve the strength of single crystal silicon, thereby improving the crystal quality and stability, reducing material consumption and improving the performance and production efficiency of the equipment. It can improve the crystal quality of silicon wafers, so that the photoelectric conversion efficiency of silicon wafer batteries can be improved, which helps to reduce the cost of photovoltaic power generation and improve its competitiveness in the energy field. It can improve the strength of silicon wafers, so that silicon wafers can be further thinned without affecting subsequent processing, and ultra-thin silicon wafers can be obtained, making P-type single crystal silicon materials more economical and efficient, and promoting further reduction in the cost of photovoltaic power generation.
[0017] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. DETAILED DESCRIPTION
[0018] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0019] It should be understood that the present invention can be implemented in different forms and should not be interpreted as limited to the embodiments set forth herein. On the contrary, these embodiments are provided to make the disclosure thorough and complete and to fully convey the scope of the present invention to those skilled in the art.
[0020] The technical solution of the present invention is further described in detail below in conjunction with several embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0022] The present invention provides a method for growing P-type single crystal silicon, which at least includes the following steps: uniformly mixing polycrystalline silicon and a doping source according to a mass ratio to obtain a mixed powder, melting the mixed powder under an inert atmosphere at a preset temperature, and introducing a seed crystal to grow single crystal silicon. The doping source includes, for example, phosphorus and gallium arsenide, and the phosphorus is, for example, phosphorus powder or silicon-phosphorus master alloy, and the gallium arsenide is, for example, derived from a single gallium arsenide substance. By using phosphorus and gallium arsenide at the same time, it is possible to effectively control the resistivity of P-type single crystal silicon, slow down the decrease in the resistivity of the single crystal silicon rod, make the resistivity more concentrated in a range, improve the strength of the single crystal silicon, and thus improve the crystal quality and stability.
[0023] In one embodiment of the present invention, the mass ratio of polysilicon to doping source is, for example, 40190:1 to 40200:1. After the polysilicon and the doping source are evenly mixed, a mixed powder is obtained, wherein the molar ratio of phosphorus to gallium arsenide is, for example, 5 to 10:90 to 95, to avoid inversion caused by excessive phosphorus content. The mixed powder is placed in a quartz crucible, for example, and the quartz crucible is placed in a single crystal furnace. After the furnace is loaded, the furnace is evacuated to check for leaks, and then, for example, under the protection of an inert gas such as argon, the temperature of the single crystal furnace is heated to a preset temperature to melt the polysilicon. In one embodiment of the present application, the preset temperature is, for example, 1450°C to 1550°C.
[0024] In one embodiment of the present invention, single crystal silicon is grown by a method such as a Czochralski method or a floating zone melting method. In this embodiment, the growth process of the crystal is described by a Czochralski method. Specifically, a seed crystal is introduced into the molten silicon liquid, and operations such as necking, necking and shouldering are performed, and the crystal enters the isodiametric growth stage. The isodiametric growth temperature is, for example, 1450°C to 1550°C, the crystal growth rate is, for example, controlled at 1.0mm / min to 1.1mm / min, and the crystal growth direction is, for example, <100> , the length of the obtained single crystal silicon ingot is, for example, 3.5m to 4.2m. In one embodiment of the present invention, during the single crystal growth process, the lifting speed of the lifting motor on the upper part of the single crystal furnace body is controlled to drive the seed crystal to lift the solidified single crystal solid upward, thereby ensuring that the crystal growth rate is 1.0mm / min to 1.1mm / min. During the growth process, the resistivity of the extracted single crystal silicon is controlled in real time, the resistivity of the single crystal silicon under the current raw material and growth conditions is recorded, and the influence of the growth conditions on the growth of the single crystal silicon is fed back. In the next single crystal silicon growth process, the growth of the single crystal silicon is regulated to improve the quality of the single crystal silicon. By controlling the equal-diameter growth temperature, the quality and performance of the grown single crystal silicon crystal are affected. Within the preset equal-diameter growth temperature range, the silicon crystal is slowly lifted from the high-temperature molten liquid to form a single crystal silicon fiber. Since the longer the crystal ingot grows, the higher the doping element, and the resistivity at the bottom of the crystal ingot decreases accordingly, therefore, controlling the crystal growth rate directly affects the purity and lattice structure of the crystal, and high-quality single crystal silicon is obtained. By optimizing the doping process and crystal growth conditions, efficient and low-cost P-type single crystal silicon preparation is achieved, which reduces energy consumption and material consumption in the production process, thereby reducing production costs, making P-type single crystal silicon materials more economical and efficient, and promoting their widespread application in mobile devices, photovoltaics and other fields.
[0025] In one embodiment of the present invention, when phosphorus and gallium arsenide are selected as doping sources, the atomic radius and segregation coefficient of each element in the raw material to silicon are shown in Table 1, the segregation coefficient of phosphorus to silicon is 0.35, the segregation coefficient of arsenic to silicon is 0.3, and the segregation coefficient of gallium to silicon is 0.008. When the P-type single crystal silicon is produced by the Czochralski method, the segregation coefficient of gallium to silicon is 0.008, and the uniformity of resistivity is poor. The segregation coefficient of phosphorus and arsenic is greater than the segregation coefficient of gallium to silicon, and the molar ratio of phosphorus to gallium arsenide is, for example, 5-10:90-95, wherein gallium (Ga) is a doping element for adjusting crystalline silicon to P-type, and phosphorus (P) and arsenic (As) are doping elements for adjusting crystalline silicon to N-type, so during the growth process, phosphorus (P) and arsenic (As) can effectively alleviate the downward trend of the resistivity of P-type single crystal silicon. This can improve the resistivity of the P-type single crystal silicon rod, improve the resistivity of the tail of the P-type single crystal silicon, slow down the rapid drop in resistivity, make the resistance distribution of the rod uniform, and increase the utilization range of the rod.
[0026] Table 1. Comparison table of atomic radius and silicon segregation coefficient
[0027]
[0028] In one embodiment of the present invention, in the obtained single crystal silicon ingot, the resistivity of the head of the ingot is, for example, 0.85Ω·cm to 1.1Ω·cm, and the resistivity of the tail of the ingot is, for example, 0.6Ω·cm to 1.0Ω·cm. By compound-doping phosphorus and gallium arsenide, the resistivity of the ingot can be more effectively concentrated in a certain range, the resistivity of the head and tail of the ingot can be reduced, and the resistivity distribution of the ingot can be uniform. By adopting the compound doping technology of phosphorus and gallium arsenide, more precise control of the resistivity of P-type single crystal silicon is achieved, the resistivity of the single crystal silicon ingot decreases slowly, and the resistivity distribution of the obtained crystal is more uniform, which not only improves the quality and stability of the single crystal silicon crystal, but also helps to improve the stability of subsequent silicon wafer processing and the photoelectric conversion efficiency.
[0029] In one embodiment of the present invention, the atomic radius of each element in the raw material is as shown in Table 1. The atomic radius of phosphorus is smaller than that of silicon, and the atomic radius of arsenic and gallium is larger than that of silicon. During the doping process, the doping element will replace the silicon atoms in the crystal lattice. The size of the atomic radius of the doping element affects the size of the atomic gap of crystalline silicon. When the doping atomic radius is too small, the gap between crystalline silicon atoms increases, and the processing performance of the crystal rod is poor, which is not conducive to the subsequent production of battery cells. When the doping atomic radius is larger, the gap between crystalline silicon atoms can be reduced, which has a positive effect on the processing of wafers. By doping silicon with phosphorus, arsenic and gallium, the atomic radii are matched with each other, the atomic distribution performance is improved, the brittleness of the crystal rod is improved, the processing strength of the crystal rod can be improved, and a thinner silicon wafer can be obtained. The strength of the silicon wafer can be improved, so that the silicon wafer can be further thinned without affecting subsequent processing, which helps to reduce material consumption and improve the performance of the equipment.
[0030] In one embodiment of the present invention, in the obtained single crystal silicon ingot, due to the growth conditions or impurity distribution during the growth of single crystal silicon, the head and tail of the crystal ingot often have different qualities from the middle part, especially at the tail, due to the accumulation of impurities and dislocations, the crystal quality may be significantly reduced. In this embodiment, after the crystal growth is completed, the length of the head of the extracted crystal ingot is cut off, for example, 15mm to 20mm, and the length of the tail is cut off is 20mm to 30mm, and the remaining crystal ingot is sliced using a diamond wire saw, for example. Since the resistance distribution of the crystal ingot is uniform, the remaining crystal ingot can be used to prepare high-efficiency solar cells after slicing, which can improve the utilization rate of the crystal ingot. The present invention achieves efficient and low-cost preparation of P-type single crystal silicon by optimizing the doping process and crystal growth conditions, reduces production costs, makes P-type single crystal silicon materials more economical and efficient, and promotes further reduction in the cost of photovoltaic power generation.
[0031] In one embodiment of the present invention, a single crystal silicon ingot is sliced, and the thickness of the obtained silicon wafer is, for example, 80 μm to 130 μm, and for example, 80 μm to 100 μm, and the photoelectric conversion efficiency of the silicon wafer is, for example, 24% to 24.8%. By optimizing the crystal growth conditions, the overall performance of the silicon wafer is improved. The strength of the silicon wafer is enhanced, and it can withstand thinner preparation process requirements, which helps to reduce material consumption and improve equipment performance. In the same length of the crystal ingot, more silicon wafers can be cut out, which increases the production capacity of the company's silicon wafer production and reduces costs. At the same time, the crystal quality is improved through the composite doping process, so that the photoelectric conversion efficiency of the subsequent preparation of silicon wafer batteries can be significantly improved, which helps to reduce the cost of photovoltaic power generation, promote further reduction of photovoltaic power generation costs, and improve its competitiveness in the energy field.
[0032] Hereinafter, the present invention will be explained in more detail by citing examples, which should not be construed as limiting. Appropriate modifications may be made within the scope consistent with the gist of the present invention, all of which fall within the technical scope of the present invention.
[0033] Example 1
[0034] After the polysilicon and the doping source are mixed evenly at a mass ratio of 40190:1, a mixed powder is obtained, and the molar ratio of phosphorus and gallium arsenide in the doping source is, for example, 10:90. The mixed powder is placed in a quartz crucible, and the quartz crucible is placed in a single crystal furnace. After the furnace is loaded, it is evacuated to check for leaks, and under the protection of an inert gas such as argon, the temperature of the single crystal furnace is heated to 1460°C to melt the polysilicon.
[0035] The seed crystal is introduced into the molten silicon liquid, and the operations of necking, necking and shouldering are performed, and the crystal enters the isodiameter growth stage. The isodiameter growth temperature is, for example, 1460°C, the crystal growth rate is controlled at 1.1 mm / min, and the crystal growth direction is <100> The length of the obtained single crystal silicon rod is 3.5m.
[0036] Example 2
[0037] After the polysilicon and the doping source are mixed evenly at a mass ratio of 40190:1, a mixed powder is obtained, and the molar ratio of phosphorus and gallium arsenide in the doping source is, for example, 8:92. The mixed powder is placed in a quartz crucible, and the quartz crucible is placed in a single crystal furnace. After the furnace is loaded, it is evacuated to check for leaks, and under the protection of an inert gas such as argon, the temperature of the single crystal furnace is heated to 1460°C to melt the polysilicon.
[0038] The seed crystal is introduced into the molten silicon liquid, and the operations of necking, necking and shouldering are performed, and the crystal enters the isodiameter growth stage. The isodiameter growth temperature is, for example, 1460°C, the crystal growth rate is controlled at 1.1 mm / min, and the crystal growth direction is <100> The length of the obtained single crystal silicon rod is 3.5m.
[0039] Example 3
[0040] After the polysilicon and the doping source are mixed evenly at a mass ratio of 40190:1, a mixed powder is obtained, and the molar ratio of phosphorus and gallium arsenide in the doping source is, for example, 10:90. The mixed powder is placed in a quartz crucible, and the quartz crucible is placed in a single crystal furnace. After the furnace is loaded, it is evacuated to check for leaks, and under the protection of an inert gas such as argon, the temperature of the single crystal furnace is heated to 1460°C to melt the polysilicon.
[0041] The seed crystal is introduced into the molten silicon liquid, and the operations of necking, necking and shouldering are performed, and the crystal enters the isodiameter growth stage. The isodiameter growth temperature is, for example, 1460°C, the crystal growth rate is controlled at 1.1 mm / min, and the crystal growth direction is <100> The length of the obtained single crystal silicon rod is 4.2m.
[0042] Example 4
[0043] After the polysilicon and the doping source are mixed evenly at a mass ratio of 40190:1, a mixed powder is obtained, and the molar ratio of phosphorus and gallium arsenide in the doping source is, for example, 5:95. The mixed powder is placed in a quartz crucible, and the quartz crucible is placed in a single crystal furnace. After the furnace is loaded, it is evacuated to check for leaks, and under the protection of an inert gas such as argon, the temperature of the single crystal furnace is heated to 1460°C to melt the polysilicon.
[0044] The seed crystal is introduced into the molten silicon liquid, and the operations of necking, necking and shouldering are performed, and the crystal enters the isodiameter growth stage. The isodiameter growth temperature is, for example, 1460°C, the crystal growth rate is controlled at 1.1 mm / min, and the crystal growth direction is <100> The length of the obtained single crystal silicon rod is 4.2m.
[0045] Example 5
[0046] After the polysilicon and the doping source are mixed evenly at a mass ratio of 40190:1, a mixed powder is obtained, and the molar ratio of phosphorus and gallium arsenide in the doping source is, for example, 7:93. The mixed powder is placed in a quartz crucible, and the quartz crucible is placed in a single crystal furnace. After the furnace is loaded, it is evacuated to check for leaks, and under the protection of an inert gas such as argon, the temperature of the single crystal furnace is heated to 1460°C to melt the polysilicon.
[0047] The seed crystal is introduced into the molten silicon liquid, and the operations of necking, necking and shouldering are performed, and the crystal enters the isodiameter growth stage. The isodiameter growth temperature is, for example, 1460°C, the crystal growth rate is controlled at 1.1 mm / min, and the crystal growth direction is <100> The length of the obtained single crystal silicon rod is 4.2m.
[0048] Comparative Example 1
[0049] After the polysilicon and the doping source are mixed evenly at a mass ratio of 40190:1, a mixed powder is obtained, and gallium is selected as the doping source. The mixed powder is placed in a quartz crucible, and the quartz crucible is placed in a single crystal furnace. After the furnace is loaded, it is evacuated to check for leaks. Under the protection of inert gases such as argon, the temperature of the single crystal furnace is heated to 1460°C to melt the polysilicon.
[0050] Introduce seed crystal into molten silicon liquid, and carry out operations such as necking, necking and shouldering, and the crystal enters the isodiameter growth stage. The isodiameter growth temperature is, for example, 40190, the crystal growth rate is controlled at 1.1mm / min, and the crystal growth direction is <100> The length of the obtained single crystal silicon rod is 3.5m.
[0051] Comparative Example 2
[0052] After the polysilicon and the doping source are mixed evenly at a mass ratio of 40190:1, a mixed powder is obtained, and gallium is selected as the doping source. The mixed powder is placed in a quartz crucible, and the quartz crucible is placed in a single crystal furnace. After the furnace is loaded, it is evacuated to check for leaks. Under the protection of inert gases such as argon, the temperature of the single crystal furnace is heated to 1460°C to melt the polysilicon.
[0053] The seed crystal is introduced into the molten silicon liquid, and the operations of necking, necking and shouldering are performed, and the crystal enters the isodiameter growth stage. The isodiameter growth temperature is, for example, 1460°C, the crystal growth rate is controlled at 1.1 mm / min, and the crystal growth direction is <100> The length of the obtained single crystal silicon rod is 4.2m.
[0054] After obtaining the single crystal silicon, the single crystal silicon ingots obtained in Examples 1-5 and Comparative Examples 1-2 were tested, and the test results are shown in Tables 2 and 3. First, based on the real-time monitoring of the resistivity during the growth process, the resistivity of the head and tail of the ingot is obtained. In one embodiment of the present invention, when the fragmentation rate of the finished silicon wafer is ≤0.03%, the limit thickness of the single crystal silicon wafer is obtained by wire cutting, the single crystal silicon wafer is assembled into a solar cell, and the photoelectric conversion efficiency of the single crystal silicon is calculated.
[0055] Table 2 Experimental conditions and resistivity of Examples 1-5 and Comparative Examples 1-2
[0056]
[0057] Table 3. Limit thickness and photoelectric conversion rate of single crystal silicon slices of Examples 3-5 and Comparative Example 2
[0058]
[0059] Please refer to Table 2. Under the same doping conditions, as the growth length increases, the resistivity of the tail of the crystal rod decreases. Through Examples 1-2 and Comparative Example 1, the composite doping of phosphorus and gallium arsenide can more effectively concentrate the resistivity of the crystal rod in a certain range than gallium doping alone. Under the same growth length, the resistivity difference between the head and tail of the composite doped crystal rod is smaller. The reason is. Based on the silicon segregation coefficient of 1, the silicon segregation coefficient of the doping element is less than 1. The longer the crystal rod grows, the higher the doping element, and the resistivity at the bottom of the crystal rod decreases accordingly. Phosphorus and arsenic are doping elements that adjust the single crystal silicon to N-type, and gallium is a doping element that adjusts the single crystal silicon to P-type. Doping with phosphorus and arsenic can effectively alleviate the downward trend of the resistivity of P-type single crystal silicon. Therefore, compared with Examples 1 and 3, as the crystal rod grows longer, the doping element is higher, and the resistivity at the bottom of the crystal rod decreases accordingly.
[0060] Please refer to Table 2 and Table 3. As the proportion of GaAs increases during the mixed doping process, the resistivity at the end of the crystal rod decreases. At the same time, the composite doping of phosphorus and GaAs can effectively improve the brittleness of silicon wafers, and the greater the proportion of GaAs, the more obvious the improvement effect. The principle is as follows: In the atomic structure of single-crystalline silicon, the doping element will replace the silicon atoms in the lattice, the acceptor element (IIIA group elements) will form holes, and the donor element (VA group elements) will form electrons. The size of the atomic radius of the doping element affects the size of the atomic gap of the crystalline silicon. If the atomic radius is too small, it is not conducive to the later production of solar cells. The atomic radius of Ga is larger than that of silicon, which has a positive effect on the thinning of silicon wafers. Therefore, under the same fragmentation rate, the limit thickness of the silicon wafer decreases, and the photoelectric conversion efficiency is improved.
[0061] In summary, the present invention provides a P-type single crystal silicon and a growth method thereof, which can improve the resistivity of P-type single crystal silicon, improve the resistivity of the tail of P-type single crystal silicon, make the resistivity distribution more uniform, slow down the rapid decline of resistivity, achieve effective control of the resistivity of single crystal silicon, and improve the utilization range of the crystal rod. It can improve the brittleness of the crystal rod and improve the strength of single crystal silicon, thereby improving the crystal quality and stability, reducing material consumption and improving the performance and production efficiency of the equipment. It can improve the crystal quality of silicon wafers, so that the photoelectric conversion efficiency of silicon wafer batteries can be improved, which helps to reduce the cost of photovoltaic power generation and improve its competitiveness in the energy field. It can improve the strength of silicon wafers, so that silicon wafers can be further thinned without affecting subsequent processing, making P-type single crystal silicon materials more economical and efficient, and promoting further reduction in the cost of photovoltaic power generation.
[0062] The above description of the illustrated embodiments of the present invention (including the contents described in the Abstract) is not intended to be an exhaustive list or to limit the present invention to the precise form disclosed herein. Although specific embodiments of the present invention and examples of the present invention are described herein for illustrative purposes only, various equivalent modifications are possible within the spirit and scope of the present invention as will be recognized and appreciated by those skilled in the art. As noted, these modifications may be made to the present invention in accordance with the above description of the embodiments described in the present invention, and these modifications will be within the spirit and scope of the present invention.
[0063] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features without departing from the inventive concept, such as the technical solution formed by replacing the above features with the technical features with similar functions disclosed in this application (but not limited to). In addition to the technical features described in the specification, the remaining technical features are known technologies to those skilled in the art. In order to highlight the innovative features of the present invention, the remaining technical features will not be described in detail here.
Claims
1. A method for growing P-type single crystal silicon, characterized in that: The following steps are involved: uniformly mixing polycrystalline silicon and a doping source according to a mass ratio to obtain a mixed powder, wherein the doping source comprises phosphorus and gallium arsenide, and the molar ratio of the phosphorus to the gallium arsenide is 5-10:90-95; and The mixed powder is melted at a preset temperature under an inert atmosphere, and a seed crystal is introduced to grow single crystal silicon.
2. The method for growing P-type single crystal silicon according to claim 1, characterized in that: The mass ratio of the polysilicon to the doping source is 40190:1 to 40200:
1.
3. The method for growing P-type single crystal silicon according to claim 1, characterized in that: The preset temperature is 1450°C to 1550°C.
4. The method for growing P-type single crystal silicon according to claim 1, characterized in that: The single crystal silicon is grown by using a Czochralski method or a floating zone melting method.
5. The method for growing P-type single crystal silicon according to claim 1, characterized in that: The crystal growth rate of the single crystal silicon is controlled at 1.0 mm / min to 1.1 mm / min.
6. The method for growing P-type single crystal silicon according to claim 1, characterized in that: The crystal growth direction of the single crystal silicon is <100> The length of the obtained single crystal silicon rod is 3.5m to 4.2m.
7. The method for growing P-type single crystal silicon according to claim 6, characterized in that: The resistivity of the crystal rod head is 0.85Ω·cm to 1.1Ω·cm, and the resistivity of the crystal rod tail is 0.6Ω·cm to 1.0Ω·cm.
8. The method for growing P-type single crystal silicon according to claim 6, characterized in that: The crystal rod is sliced to obtain a silicon wafer, and the thickness of the silicon wafer is 80 μm to 130 μm.
9. A P-type single crystal silicon, characterized in that: Obtained by the growth method according to any one of claims 1 to 8.