Reflective mask blank and method for manufacturing reflective mask

By using an absorber film with a specific layer structure and a chromium (Cr) hard mask film in the reflective mask blank, the problem of damage to the protective film during dry etching and cleaning processes is solved, and the tolerance of the reflective mask is improved. and stability, extending its service life.

CN118778342APending Publication Date: 2024-10-15SHIN ETSU CHEMICAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410393516.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-04
Filing Date
2024-04-02
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The protective film of the existing reflective mask blank is easily damaged during dry etching and cleaning processes, resulting in functional degradation of the multi-layer reflective film. Especially when using gases containing chlorine and oxygen or sulfuric acid-hydrogen peroxide mixture, the protective film The thickness is reduced, affecting the performance of the reflective mask.

Method used

An absorber film with a specific layer structure is formed on a protective film containing ruthenium (Ru), including a first layer and a second layer containing tantalum (Ta). The first layer does not contain nitrogen, and the second layer contains tantalum and nitrogen. , reducing sensitivity to chlorine and oxygen-containing gases by optimizing the layer structure, and forming a chromium (Cr) hard mask film on the hard mask film to control damage during etching and cleaning processes.

Benefits of technology

It effectively reduces the damage and thickness reduction of the protective film caused by chlorine- and oxygen-containing gas etching and sulfuric acid-hydrogen peroxide cleaning, improves the tolerance and stability of the reflective mask blank, and extends its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118778342A_ABST
    Figure CN118778342A_ABST
Patent Text Reader

Abstract

In a reflective mask blank including a substrate, a multilayer reflective film, a protective film, an absorber film, and a hard mask film, the protective film is composed of a material containing ruthenium (Ru), the absorber film is composed of a first layer having a composition containing tantalum (Ta) and not containing nitrogen (N), or a first layer, a second layer, and a third layer, the first layer having a composition containing tantalum (Ta) and nitrogen (N), the second layer having a composition containing tantalum (Ta) and nitrogen (N), and the third layer having a composition containing tantalum (Ta) and nitrogen (N). The third layer has a composition containing tantalum (Ta), nitrogen (N), and oxygen (O), and the hard mask film is composed of a material containing chromium (Cr).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a reflective mask blank which is a material for manufacturing a reflective mask of a semiconductor device such as LSI, and a method for manufacturing a reflective mask from the reflective mask blank. Background Art

[0002] In the manufacturing process of semiconductor devices, photolithography is repeatedly used, in which the exposure light is irradiated onto the transfer mask through a reduction projection optical system, and the circuit pattern formed on the transfer mask is transferred to the semiconductor substrate (semiconductor wafer). Conventionally, the mainstream wavelength of the exposure light is 193nm through an argon fluoride (ArF) excimer laser. By adopting a process called multiple patterning, a pattern with a size smaller than the exposure wavelength is finally formed, in which the exposure process and the processing process are combined multiple times.

[0003] However, because it is necessary to form further fine patterns under the continuous miniaturization of device patterns, extreme ultraviolet lithography technology using extreme ultraviolet (hereinafter referred to as "EUV") light with a wavelength shorter than the wavelength of ArF excimer laser as exposure light has been used. EUV light is light with a wavelength of about 0.2 to 100 nm, in particular, light with a wavelength of about 13.5 nm. EUV light has very low transmittance to matter and cannot be used in conventional transmission projection optical systems or masks, so reflective optical element devices are applied. Therefore, reflective masks are also used as masks for pattern transfer.

[0004] In the reflective mask, a multilayer reflective film that reflects EUV light is formed on a substrate, and an absorber film formed in a pattern that absorbs EUV light is further formed on the multilayer reflective film. On the other hand, the material before the absorber film is patterned (including the state in which the resist layer is formed) is called a reflective mask blank, and is used as the material of the reflective mask. The reflective mask blank generally has a basic structure that includes a low thermal expansion substrate, a multilayer reflective film formed on one of the two main surfaces of the substrate and reflecting EUV light, and an absorber film formed thereon and absorbing EUV light.

[0005] As a multilayer reflective film, a multilayer reflective film that ensures the necessary reflectivity for EUV light by alternately stacking molybdenum (Mo) layers and silicon (Si) layers is generally used. On the other hand, tantalum (Ta) having a relatively large extinction coefficient for EUV light is used for the absorber film (Patent Document 1: JP-A 2002-246299).

[0006] In addition, as disclosed in JP-A 2002-122981 (Patent Document 2), as a protective film for protecting the multilayer reflective film, a ruthenium (Ru) film is formed on the multilayer reflective film. In addition, as an etching mask for patterning the absorber film, in some cases, a hard mask film containing chromium (Cr) is formed on the absorber film. On the other hand, a conductive film is formed on the other main surface of the substrate. As the conductive film, a metal nitride film for electrostatic adsorption is proposed, and a film containing chromium (Cr) or tantalum (Ta) is exemplified.

[0007] Reference List

[0008] Patent Document 1: JP-A 2002-246299

[0009] Patent Document 2: JP-A 2002-122981 Summary of the invention

[0010] The protective film is required to have a function of protecting the multilayer reflective film. In particular, a function for protecting the multilayer reflective film so as not to expose the multilayer reflective film to etching gas and cleaning liquid when processing the pattern of the absorber film, and a function for suppressing a decrease in reflectivity due to repeated exposure in exposure using a reflective mask are exemplified.

[0011] In the manufacturing process of a reflective mask using a reflective mask blank as a material, when dry etching an absorber film to form a pattern of the absorber film, a certain degree of over-etching is usually performed to control the pattern shape. Due to over-etching, the protective film is exposed to etching and damaged. When the absorber film is composed of a material containing tantalum (Ta), it is preferred to use a gas containing chlorine and not containing oxygen as an etching gas. Therefore, the protective film is required to be resistant to dry etching using a gas containing chlorine and not containing oxygen.

[0012] In addition, when a hard mask pattern obtained by forming a pattern of a hard mask film composed of a material containing chromium (Cr) is used as an etching mask when forming a pattern of an absorber film, after forming the pattern of the absorber film, the pattern of the hard mask film is generally removed by dry etching using a gas containing chlorine and oxygen. The protective film is also exposed to the dry etching using a gas containing chlorine and oxygen at that time. Therefore, the protective film is also required to have resistance to dry etching using a gas containing chlorine and oxygen.

[0013] In addition, in order to remove the residue of the resist used to manufacture the reflective mask and remove the contaminants generated in the repeated use of the reflective mask, a sulfuric acid-hydrogen peroxide mixture (SPM) is used for cleaning. Therefore, the protective film is also required to have resistance to the sulfuric acid-hydrogen peroxide mixture (SPM).

[0014] If the protective film is damaged during etching in the manufacture of the reflective mask, and changes in film quality and thickness are caused, problems occur in the protective film, such as loss of the function of protecting the multilayer reflective film. Therefore, for the protective film containing ruthenium (Ru), a protective film to which an additive element such as niobium (Nb) is added has been proposed to enhance the function of protecting the multilayer reflective film by improving resistance to dry etching.

[0015] However, even when the resistance to dry etching is enhanced by adding an additive element such as niobium (Nb) to the protective film containing ruthenium (Ru), the protective film will become thinner when it is exposed to a gas containing chlorine and no oxygen during dry etching to an absorber film composed of a material containing tantalum (Ta). In addition, when the protective film is exposed to a gas containing chlorine and oxygen to remove the pattern of the hard mask film, the protective film will also become thinner. In addition, the protective film will also become thinner in cleaning using a sulfuric acid-hydrogen peroxide mixture (SPM).

[0016] As described above, it is difficult to avoid chemical damage to the protective film, and the protective film will become thinner due to physical damage. Therefore, it is necessary to control the function of the protective film to prevent the multilayer reflective film from deteriorating due to thickness reduction.

[0017] The present invention is made to solve the above problems, and an object of the present invention is to provide a reflective mask blank including an absorber film composed of a material containing tantalum (Ta) as a reflective mask blank in which an absorber film composed of a material containing ruthenium (Ru) is formed on a protective film composed of a material containing ruthenium (Ru), which can reduce damage to the protective film caused by over-etching the absorber film composed of a material containing tantalum (Ta) using a gas containing chlorine and not containing oxygen, and can control the reduction in the thickness of the protective film caused by dry etching using a gas containing chlorine and oxygen or cleaning using a sulfuric acid-hydrogen peroxide mixture (SPM). Another object of the present invention is to provide a method for manufacturing a reflective mask using the reflective mask blank.

[0018] In order to solve the above-mentioned problems, the inventors have conducted earnest research. As a result, the inventors have found that, for a reflective mask blank in which an absorber film composed of a material containing tantalum (Ta) is formed on a protective film composed of a material containing ruthenium (Ru), the absorber film has a structure including, from the substrate side, a first layer having a composition containing tantalum (Ta) and not containing nitrogen (N) and a second layer having a composition containing tantalum (Ta) and nitrogen (N). In addition, the inventors have found that the reflective mask blank having this structure can reduce damage to the protective film caused by over-etching the absorber film composed of a material containing tantalum (Ta) using a gas containing chlorine and not containing oxygen, and can control the reduction in the thickness of the protective film caused by dry etching using a gas containing chlorine and oxygen or cleaning using a sulfuric acid-hydrogen peroxide mixture (SPM).

[0019] In one aspect, the present invention provides a reflective mask blank comprising a substrate, a multilayer reflective film formed on one main surface of the substrate and reflecting exposure light, a protective film formed on and in contact with the multilayer reflective film, an absorber film formed on and in contact with the protective film and absorbing the exposure light, and a hard mask film formed on and in contact with the absorber film and serving as an etching mask in dry etching of the absorber film, the reflective mask blank being a material for a reflective mask in EUV lithography using EUV light as exposure light, wherein:

[0020] The protective film is composed of a material containing ruthenium (Ru) and has a thickness of not less than 2 nm and not more than 5 nm,

[0021] The absorber film is composed of a material containing tantalum (Ta), and is composed of a first layer and a second layer, or a first layer, a second layer, and a third layer from the substrate side,

[0022] The first layer has a composition containing tantalum (Ta) and no nitrogen (N), and has a thickness of not less than 0.5 nm and not more than 2 nm,

[0023] the second layer has a composition containing tantalum (Ta) and nitrogen (N), and the composition has a nitrogen (N) content of not less than 10 atomic % and an oxygen (O) content of not more than 5 atomic %,

[0024] The first layer and the second layer have a total thickness of not less than 50 nm and not more than 80 nm,

[0025] The third layer has a composition containing tantalum (Ta), nitrogen (N), and oxygen (O) and has a thickness of not more than 20 nm, and the composition has an oxygen (O) content of not less than 30 atomic % and not more than 70 atomic %, and

[0026] The hard mask film is composed of a material containing chromium (Cr) and has a thickness of not less than 5 nm and not more than 20 nm.

[0027] Preferably, the composition of the first layer further includes oxygen (O).

[0028] Preferably, the composition of the first layer has an oxygen (O) content of not less than 5 atomic %.

[0029] Preferably, the composition of the second layer has a tantalum (Ta) content of not less than 55 atomic % and not more than 70 atomic %, and a nitrogen (N) content of not less than 30 atomic % and not more than 45 atomic %.

[0030] Preferably, the material containing ruthenium (Ru) is a single substance of ruthenium (Ru) or an alloy consisting of ruthenium (Ru) and niobium (Nb).

[0031] Preferably, the alloy composed of ruthenium (Ru) and niobium (Nb) has a niobium (Nb) content of not more than 30 atomic % on average with respect to the entire protective film.

[0032] In another aspect, the present invention provides a method for manufacturing a reflective mask, comprising the steps of:

[0033] (A) preparing the reflective mask blank of claim 1,

[0034] (B) forming a resist pattern on the hard mask film,

[0035] (C) dry etching the hard mask film by using a gas containing chlorine and oxygen and utilizing the resist pattern as an etching mask to form a pattern of the hard mask film,

[0036] (D) forming patterns of the first and second layers in the absorber film by dry etching the first and second layers in the absorber film using a gas containing chlorine and not containing oxygen and utilizing the pattern of the hard mask film as an etching mask,

[0037] (E) after step (C) or (D), removing the resist pattern, and

[0038] (F) The pattern of the hard mask film is removed by dry etching using a gas containing chlorine and oxygen.

[0039] Preferably, dry etching is performed in step (D) to expose the protective film.

[0040] Preferably, dry etching is performed in step (D) so that part of the absorber film remains without exposing the protective film, and

[0041] In step (F), dry etching is performed to expose the protective film.

[0042] Preferably, the method further comprises

[0043] (G) A treatment step subsequent to step (F) comprising contacting the exposed absorber film with a sulfuric acid-hydrogen peroxide mixture (SPM).

[0044] Preferably, the method further comprises

[0045] (G) a treatment step after step (F) comprising contacting the exposed absorber film with a sulfuric acid-hydrogen peroxide mixture (SPM), wherein

[0046] In steps (D) and (F), dry etching is performed so that a portion of the absorber film remains without exposing the protective film, and

[0047] In step (G), dry etching is performed to expose the protective film.

[0048] Preferably, the absorber film consists of a first layer, a second layer and a third layer starting from the substrate side, and

[0049] The method further comprises the following steps:

[0050] (C-1) After step (C) and before step (D), the pattern of the third layer in the absorber film is formed by dry etching the third layer in the absorber film using a fluorine-based gas and utilizing the pattern of the hard mask film.

[0051] Beneficial effects of the present invention

[0052] According to the present invention, the reflective mask blank of the present invention can reduce the damage of the protective film caused by over-etching the absorber film composed of a material containing tantalum (Ta) using a gas containing chlorine and not containing oxygen. In addition, the reflective mask blank of the present invention controls the reduction of the thickness of the protective film caused by dry etching using a gas containing chlorine and oxygen or cleaning using a sulfuric acid-hydrogen peroxide mixture (SPM). BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Figure 1 is a cross-sectional view showing an example of a reflective mask blank of the present invention.

[0054] Figure 2 is a cross-sectional view showing another example of the reflective mask blank of the present invention.

[0055] Figure 3 is a schematic diagram of an etching apparatus used in the experimental example and the comparative experimental example. DETAILED DESCRIPTION

[0056] The reflective mask blank of the present invention includes a substrate, a multilayer reflective film formed on one main surface (front side surface) of the substrate and reflecting exposure light, a protective film formed on the multilayer reflective film, an absorber film formed on the protective film and absorbing the exposure light, and a hard mask film formed on the absorber film. The reflective mask blank of the present invention is suitable for the material of a reflective mask used in EUV lithography using EUV light as exposure light. The wavelength of EUV light used in EUV lithography using EUV light as exposure light is 13 to 14 nm, typically about 13.5 nm. A reflective mask blank and a reflective mask using EUV light as exposure light are also referred to as an EUV mask blank and an EUV mask, respectively.

[0057] Figure 11 is a cross-sectional view showing an example of a reflective mask blank of the present invention. The reflective mask blank 11 includes a substrate 1, and on the substrate 1, a multilayer reflective film 2 formed in contact with the substrate 1, a protective film 3 formed in contact with the multilayer reflective film 2, an absorber film 4 formed in contact with the protective film 3, and a hard mask film 5 formed in contact with the absorber film 4. In this case, the absorber film 4 has a structure consisting of two layers of a first layer 41 and a second layer 42 from the substrate 1 side.

[0058] Figure 2 1 is a cross-sectional view showing another example of the reflective mask blank of the present invention. The reflective mask blank 12 includes a substrate 1, and on the substrate 1, a multilayer reflective film 2 formed in contact with the substrate 1, a protective film 3 formed in contact with the multilayer reflective film 2, an absorber film 4 formed in contact with the protective film 3, and a hard mask film 5 formed in contact with the absorber film 4. In this case, the absorber film 4 has a structure consisting of three layers of a first layer 41, a second layer 42, and a third layer 43 from the substrate 1 side.

[0059] For EUV exposure, the substrate preferably has low thermal expansion properties. For example, the substrate is made of a material having a thermal expansion of preferably ±2×10 -8 / ℃, more preferably within ±5×10 -9 As such a material, for example, titanium dioxide-doped quartz glass (SiO 2 -TiO 2 Base glass). In addition, it is preferred to use a substrate with a sufficiently flat surface. The main surface of the substrate has a surface roughness expressed in an RMS value of preferably not more than 0.5nm, more preferably not more than 0.2nm. Such surface roughness can be obtained by polishing the substrate or other methods. As the size of the substrate, the main surface of the substrate preferably has a 152mm square, and the substrate preferably has a thickness of 6.35 millimeters. The substrate with these dimensions is referred to as a 6025 substrate (a substrate with a main surface size of 6 inches square and 0.25 inches thick).

[0060] The multilayer reflective film is a film that reflects the exposure light in the reflective mask. The multilayer reflective film is preferably formed in a manner of contacting one main surface of the substrate, however, it can also be formed via another film, such as an underlayer film on one main surface of the substrate. The multilayer reflective film has a periodic stacked structure in which a high refractive index layer having a relatively high refractive index relative to the exposure light and a low refractive index layer having a relatively low refractive index relative to the exposure light are alternately stacked.

[0061] The high refractive index layer is preferably composed of a material containing silicon (Si). The high refractive index layer may contain at least one additive element selected from the group consisting of oxygen (O), nitrogen (N), carbon (C), boron (B) and hydrogen (H). In addition, the high refractive index layer may be composed of multiple layers, which include layers containing additive elements and layers that do not contain additive elements. The high refractive index layer has a thickness of preferably not less than 3.5 nm, more preferably not less than 4 nm, and preferably not more than 4.9 nm, more preferably not more than 4.4 nm.

[0062] The low refractive index layer is preferably composed of a material containing molybdenum (Mo). The low refractive index layer may contain at least one additive element selected from the group consisting of oxygen (O), nitrogen (N), carbon (C), boron (B) and hydrogen (H). In addition, the low refractive index layer may be composed of multiple layers, which include layers containing additive elements and layers that do not contain additive elements. The low refractive index layer has a thickness of preferably not less than 2.1 nm, more preferably not less than 2.6 nm, and preferably not more than 3.5 nm, more preferably not more than 3 nm.

[0063] The stacked structure constituting the periodic stacked structure may include high refractive index layer and low refractive index layer, and may include at least one high refractive index layer and at least one low refractive index layer.Stacked structure comprises at least two layers, and may be composed of, for example, a high refractive index layer and a low refractive index layer. In addition, stacked structure may include at least two high refractive index layers having different compositions (for example, different composition ratios, or having or not having the different compositions of added elements) from each other, and may include at least two low refractive index layers having different compositions (for example, different composition ratios, or having or not having the different compositions of added elements) from each other. In this case, stacked structure comprises at least three layers, and may include four or five or more layers, yet, preferably not more than eight layers.The periodic stacked structure has the circulation of the stacked structure preferably being no less than 30 cycles, preferably being no more than 50 cycles, more preferably being no more than 40 cycles.

[0064] The multilayer reflective film having a periodic stacking structure has a thickness of preferably not less than 200 nm, more preferably not less than 270 nm, and preferably not more than 400 nm, more preferably not more than 290 nm.

[0065] Examples of methods for forming a multilayer reflective film include a sputtering method, in which power is provided to a target for sputtering, and a plasma of an atmospheric gas is formed (the atmospheric gas is ionized) by the power provided, and an ion beam sputtering method, in which the target is irradiated with an ion beam. The sputtering method includes a DC sputtering method in which a DC voltage is applied to the target and an RF sputtering method in which a high-frequency voltage is applied to the target. The sputtering method is a film forming method utilizing the sputtering phenomenon of gas ions, which are generated by applying a voltage to the target and sending a sputtering gas into a chamber to ionize the gas. In particular, the magnetron sputtering method has advantages in terms of productivity. Power can be applied to the target by a DC system or an RF system. The DC system also includes pulsed sputtering, in which the negative bias applied to the target is reversed in a short time to prevent the target from charging.

[0066] The multilayer reflective film can be formed by, for example, a sputtering method using a sputtering device that can be connected to a plurality of targets. In particular, a target appropriately selected from the group consisting of a molybdenum (Mo) target for forming a layer containing molybdenum (Mo), a silicon (Si) target for forming a layer containing silicon (Si), and other targets can be used as a target, and a rare gas such as helium (He) gas, argon (Ar) gas, krypton (Kr) gas, and xenon (Xe) gas can be used as a sputtering gas to form the multilayer reflective film.

[0067] In addition, in the case where the sputtering is reactive sputtering using a reactive gas, for example, a nitrogen-containing gas such as nitrogen (N 2 ) gas to form a nitrogen (N)-containing film, oxygen-containing gas such as oxygen (O 2 ) gas to form a film containing oxygen (O), nitrogen oxide gases such as nitrous oxide (N 2 O) gas, nitric oxide (NO) gas and nitrogen dioxide (NO 2 ) gas to form a film containing nitrogen (N) and oxygen (O), carbon oxide gases such as carbon monoxide (CO) gas and carbon dioxide (CO 2 ) gas to form a film containing carbon (C) and oxygen (O), hydrogen-containing gas such as hydrogen (H 2 ) gas to form a membrane containing hydrogen (H), or hydrocarbon gases such as methane (CH 4 )A gas for forming a film containing carbon (C) and hydrogen (H) can be used together with a rare gas.

[0068] Furthermore, a molybdenum (Mo) target to which boron (B) is added (molybdenum boride (MoB) target) or a silicon (Si) target to which boron (B) is added (silicon boride (SiB) target) may be used to form a layer containing boron (B).

[0069] The protective film is a film for protecting the multilayer reflective film. The protective film is formed in a manner in contact with the multilayer reflective film. The protective film is composed of a material containing ruthenium (Ru). Examples of materials containing ruthenium (Ru) include a simple substance of ruthenium (Ru), and an alloy composed of ruthenium (Ru) and other metals or metalloids different from ruthenium (Ru). Examples of other metals or metalloids different from ruthenium (Ru) include niobium (Nb), zirconium (Zr), titanium (Ti), chromium (Cr), silicon (Si), etc. Among the materials containing ruthenium (Ru), a simple substance of ruthenium (Ru) or an alloy composed of ruthenium (Ru) and niobium (Nb) is particularly preferred. For the protective film as a whole, the content of other metals or metalloids different from ruthenium (Ru) in the protective film is preferably not more than 30 atomic % on average, and more preferably not more than 20 atomic %. For the protective film as a whole, the lower limit of the content of other metals or metalloids other than ruthenium (Ru) in the protective film is preferably not less than 5 atomic % on average, more preferably not less than 10 atomic %, but is not limited thereto.

[0070] The protective film may have a single-layer structure or a multilayer structure in which a plurality of layers having different compositions are combined. In addition, each layer constituting the single layer or the plurality of layers may have a graded structure in which the composition changes continuously along the thickness direction. In particular, in the protective film, one or both of the side close to the multilayer reflective film (the layer close to the multilayer reflective film in the case of the multilayer structure) and the side farthest from the multilayer reflective film (the layer farthest from the multilayer reflective film in the case of the multilayer structure) may be composed of ruthenium (Ru).

[0071] In the case where the protective film has a multilayer structure or a composition-graded structure, another metal or metalloid other than ruthenium (Ru) preferably has a content that increases from the multilayer reflective film side to the side away from the multilayer reflective film in a portion or the entirety of the protective film in the thickness direction. In particular, in the case where niobium (Nb) is contained as another metal or metalloid other than ruthenium (Ru), niobium (Nb) effectively improves resistance to dry etching using a gas containing chlorine and oxygen. Therefore, niobium (Nb) preferably has a content that increases from the multilayer reflective film side to the side away from the multilayer reflective film in the thickness direction in a portion or the entirety of the protective film.

[0072] The protective film has a thickness of preferably not less than 2 nm, more preferably not less than 3 nm, and preferably not more than 5 nm, more preferably not more than 4 nm.

[0073] The protective film can be formed by sputtering using a ruthenium (Ru) target and an optional target of other metals or metalloids other than ruthenium (Ru), particularly a niobium (Nb) target, a zirconium (Zr) target, a titanium (Ti) target, a chromium (Cr) target or a silicon (Si) target as a target, and using a rare gas such as helium (He) gas, argon (Ar) gas, krypton (Kr) gas and xenon (Xe) gas as a sputtering gas. Sputtering is preferably magnetron sputtering.

[0074] In the reflective mask, the absorber film is a film that absorbs exposure light and reduces reflectivity. The absorber film is formed in contact with the protective film. The absorber film is a film that reduces the reflectivity of the exposure light by absorbing EUV light as the exposure light. In the reflective mask, the transfer pattern is formed by the difference in reflectivity between the portion where the absorber film is formed and the portion where the absorber film is not formed.

[0075] The absorber film is composed of a material that can absorb EUV light and can be processed into a pattern and a material containing tantalum (Ta). The material containing tantalum (Ta) may contain oxygen (O), nitrogen (N), carbon (C), boron (B) or other elements. Examples of the material of the absorber film include, for example, a material containing tantalum (Ta). In particular, examples of the material include a simple substance of Ta and a tantalum (Ta) compound, such as TaO, TaN, TaON, TaC, TaCO, TaCN, TaCON, TaB, TaOB, TaNB, TaONB, TaCB, TaCOB, TaCNB and TaCONB.

[0076] In particular, a material containing tantalum (Ta) and nitrogen (N) is preferred. In dry etching using a gas containing chlorine and not containing oxygen, since both the etching selectivity for a protective film composed of a material containing ruthenium (Ru) and the etching selectivity for a hard mask film composed of a material containing chromium (Cr) are high, the material imparts good processability in pattern formation of an absorber film. On the other hand, compared with a material containing tantalum (Ta) and nitrogen (N), a material containing tantalum (Ta) and not containing nitrogen (N) is difficult to etch by dry etching using a gas containing chlorine and oxygen.

[0077] The absorber film preferably has a microcrystalline structure or an amorphous structure. The absorber film may contain at least one element selected from the group consisting of hydrogen (H), boron (B), carbon (C), silicon (Si), molybdenum (Mo), zirconium (Zr), chromium (Cr), germanium (Ge) and aluminum (Al), in particular one or both of carbon (C) and boron (B), as long as the total content of the elements is not more than 20 atomic %.

[0078] The absorber film may be composed of two layers, which are the first layer and the second layer from the substrate side. In the case of an absorber film having a two-layer structure, the first layer preferably has a composition containing tantalum (Ta) and no nitrogen (N), and the second layer preferably has a composition containing tantalum (Ta) and nitrogen (N).

[0079] The first layer preferably contains oxygen (O). In the case where the first layer contains oxygen (O), although it has high resistance to dry etching using a gas containing chlorine and oxygen, it is advantageous that even if a small amount of the absorber film remains on the protective film in an area other than the pattern of the absorber film, it can be removed by cleaning with a sulfuric acid-hydrogen peroxide mixture (SPM). In the case where the first layer contains oxygen (O), the first layer has an oxygen (O) content of preferably not less than 5 atomic%, more preferably not less than 20 atomic%, and even more preferably not less than 50 atomic%. The content of oxygen (O) preferably has an upper limit of not more than 71.4 atomic%, but is not limited thereto.

[0080] The first layer has a thickness of preferably not more than 2 nm, and preferably not less than 0.5 nm, and more preferably not less than 1 nm. When the first layer is too thick, when forming the pattern of the absorber film, the absorber film may remain in the area other than the pattern of the absorber film on the protective film, thereby reducing the reflectivity of the reflective mask.

[0081] Preferably, the second layer is easily etched by dry etching using a gas containing chlorine and no oxygen. Therefore, the second layer has a nitrogen (N) content of preferably not less than 10 atomic%, more preferably not less than 15 atomic%, and even more preferably not less than 30 atomic%. The nitrogen (N) content has an upper limit of preferably not more than 60 atomic%, more preferably not more than 45 atomic%. In addition, the second layer preferably has an oxygen (O) content of not more than 5 atomic%, and more preferably the second layer does not contain oxygen (O). On the other hand, the second layer has a tantalum (Ta) content of preferably not less than 40 atomic%, more preferably not less than 55 atomic%, preferably not more than 90 atomic%, and more preferably not more than 70 atomic%.

[0082] The first layer and the second layer have a total thickness (the sum of the thicknesses of the first layer and the second layer) of preferably not less than 50 nm, more preferably not less than 55 nm, and preferably not more than 80 nm, more preferably not more than 70 nm. The first layer and the second layer can be etched by dry etching using a gas containing chlorine and not containing oxygen.

[0083] The absorber film may have a two-layer structure, but, in the absorber film, when the portion farthest from the protective film contains oxygen, the reflectivity at the inspection wavelength used for defect inspection in mask processing decreases. Therefore, the third layer may be provided as the layer farthest from the protective film in the absorber film, and the absorber film may be composed of three layers, which are the first layer, the second layer, and the third layer from the substrate side. In this case, the third layer preferably has a composition containing tantalum (Ta), nitrogen (N), and oxygen (O).

[0084] The third layer has an oxygen (O) content of preferably not less than 30 atomic %, more preferably not less than 50 atomic % and preferably not more than 70 atomic %. The third layer has a tantalum (Ta) content of preferably not less than 30 atomic %, more preferably not less than 40 atomic % and preferably not more than 70 atomic %, more preferably not more than 60 atomic %. On the other hand, the third layer has a nitrogen (N) content of preferably not more than 50 atomic %, more preferably not more than 40 atomic %. The content of nitrogen (N) has a lower limit of preferably not less than 5 atomic %, more preferably not less than 10 atomic %, but is not limited thereto.

[0085] The third layer has a thickness of preferably not more than 20 nm, more preferably not more than 10 nm, and even more preferably not more than 5 nm. The thickness of the third layer has a lower limit of preferably not less than 1 nm, more preferably not less than 3 nm, but is not limited thereto. The third layer can be etched by dry etching using a fluorine-based gas (fluorine-based dry etching).

[0086] The absorber film preferably has a value not greater than 1×10 6 Ω / square, more preferably not more than 1×10 5 The absorption film has a surface roughness Sq of preferably not more than 0.8 nm, more preferably not more than 0.6 nm.

[0087] The absorber film (each layer constituting the absorber film) can be formed by sputtering, and the sputtering is preferably magnetron sputtering. In particular, the absorber film can be formed by sputtering using a target such as a tantalum (Ta) target, a tantalum (Ta) compound target (a target containing tantalum (Ta) and at least one element selected from the group consisting of oxygen (O), nitrogen (N), carbon (C), boron (B) and other elements) and using a rare gas such as helium (He) gas, neon (Ne) gas, argon (Ar) gas, krypton (Kr) gas and xenon (Xe) gas as a sputtering gas, or by using a reactive gas as a sputtering gas (such as an oxygen-containing gas, a nitrogen-containing gas and a carbon-containing gas, especially an oxygen (O 2 ) gas, nitrogen (N 2 ) gas, nitrogen oxides (N 2 O, NO, NO 2 ) gases and carbon oxides (CO, CO2 ) gas) and a rare gas by reactive sputtering.

[0088] Among the layers constituting the absorber film, the third layer may be a layer containing oxygen (O 2 ) gas atmosphere, such as the portion of the second layer farthest from the protective film is in the air, and is formed by natural oxidation. Alternatively, the third layer can be formed by 2 ) gas atmosphere, such as the portion of the second layer that is formed by heat treatment in air that is farthest from the protective film.

[0089] A hard mask film (etching mask film for the absorber film) having etching characteristics different from those of the absorber film may be provided on the absorber film on the side farthest from the substrate. The hard mask film serves as an etching mask in dry etching of the absorber film. The hard mask film is formed in contact with the absorber film.

[0090] Examples of materials for the hard mask film include materials containing chromium (Cr). When processing an absorber film composed of a material containing tantalum (Ta), the material containing chromium (Cr) has different etching characteristics. The hard mask film composed of a material containing chromium (Cr) acts as an etching mask when dry etching the absorber film, and therefore, the hard mask film is suitable. Therefore, the hard mask film preferably does not contain tantalum (Ta).

[0091] Examples of materials containing chromium (Cr) include CrO, CrN, CrON, CrC, CrOC, CoNC, and CrONC. A hard mask film composed of a material containing chromium (Cr) is generally removed by dry etching using a gas containing chlorine and oxygen during the manufacturing process of a reflective mask. Therefore, in such dry etching, it is preferred that the hard mask film has a high etching rate, and from this point of view, CrONC is preferred as the material containing chromium (Cr). The hard mask film composed of a material containing chromium (Cr) has a chromium (Cr) content of preferably not more than 60 atomic %, more preferably not more than 50 atomic %, preferably not less than 30 atomic %, more preferably not less than 40 atomic %.

[0092] After forming the pattern of the absorber film, the hard mask film may remain in the reflective mask, for example, as a reflectivity-reducing film for reducing the reflectivity at the wavelength of light used in inspection such as pattern inspection, or may be removed so as not to exist on the reflective mask. In particular, in the case where the absorber film is composed of a material containing tantalum (Ta) and not containing chromium (Cr), a hard mask film composed of a material containing chromium (Cr) is preferred.

[0093] The hard mask film may be formed on the second layer of the absorber film. In the case where the absorber film includes a third layer having a function of reducing the reflectivity at the wavelength of light used for inspection such as pattern inspection, the hard mask film may be formed on the third layer of the absorber film. The hard mask film may be formed by, for example, a magnetron sputtering method. When the hard mask film is too thin, the hard mask film may not function as an etching mask, and when the hard mask film is too thick, the processing properties may deteriorate. Therefore, the hard mask film has a thickness of preferably not less than 5 nm, preferably not more than 20 nm, and more preferably not more than 10 nm, but is not limited thereto.

[0094] The hard mask film can be formed by sputtering, and the sputtering is preferably magnetron sputtering. In particular, the hard mask film can be formed by sputtering using a target such as a chromium (Cr) target, a chromium compound target (a target containing Cr and at least one element selected from the group consisting of oxygen (O), nitrogen (N), carbon (C), boron (B) and other elements), and using a rare gas such as helium (He) gas, argon (Ar) gas, krypton (Kr) gas and xenon (Xe) gas as a sputtering gas, or by using a reactive gas as a sputtering gas (such as an oxygen-containing gas, a nitrogen-containing gas and a carbon-containing gas, especially oxygen (O 2 ) gas, nitrogen (N 2 ) gas, nitrogen oxides (N 2 O, NO, NO 2 ) gases and carbon oxides (CO, CO 2 ) gas) and a rare gas by reactive sputtering.

[0095] A conductive film for electrostatic adsorption to attach the reflective mask to an exposure device may be formed on the other main surface (back side surface) on the opposite side of the one main surface of the substrate, preferably in contact with the other main surface.

[0096] The conductive film preferably has a sheet resistance of not more than 100Ω / square, and the material of the conductive film is not limited. Examples of materials for the conductive film include, for example, materials containing tantalum (Ta) or chromium (Cr). Materials containing tantalum (Ta) or chromium (Cr) may contain oxygen (O), nitrogen (N), carbon (C), boron (B) or other elements. Examples of materials containing tantalum (Ta) include, for example, simple substances of Ta and tantalum (Ta) compounds, such as TaO, TaN, TaON, TaC, TaCN, TaCO, TaCON, TaB, TaOB, TaNB, TaONB, TaCB, TaCNB, TaCOB and TaCONB. Examples of materials containing chromium (Cr) include, for example, simple substances of Cr and chromium (Cr) compounds, such as CrO, CrN, CrON, CrC, CrCN, CrCO, CrCON, CrB, CrOB, CrNB, CrONB, CrCB, CrCNB, CrCOB and CrCONB.

[0097] The conductive film has a thickness of generally about 20 to 300 nm, but is not particularly limited thereto, as long as the thickness is sufficient for electrostatic adsorption purposes. The conductive film is preferably formed to have a thickness that satisfies the film stress balance between the conductive film and the patterns of the multilayer reflective film, the protective film, and the absorber film after obtaining the reflective mask, i.e., after forming the pattern of the absorber film. The conductive film may be formed before forming the multilayer reflective film, or after forming all films on the substrate on the multilayer reflective film side. After forming a portion of the film on the substrate on the multilayer reflective film side, the conductive film may be formed, and then the remaining films on the multilayer reflective film side may be formed on the substrate. The conductive film may be formed by, for example, a magnetron sputtering method.

[0098] The reflective mask blank may include a resist film formed on a side farthest from the substrate. The resist film is preferably an electron beam (EB) resist.

[0099] For example, a reflective mask including a substrate, a multilayer reflective film formed on one main surface of the substrate, a protective film formed in contact with the multilayer reflective film, and an absorber pattern (absorber film pattern) formed by patterning an absorber film and in contact with the protective film can be manufactured from a reflective mask blank. In the reflective mask, a transfer pattern is formed by a reflectivity difference between a portion where the absorber film is formed and a portion where the absorber film is not formed.

[0100] In the case of a hard mask film composed of a material containing chromium (Cr), a pattern of the hard mask film (hard mask pattern) can be formed by dry etching using a gas containing chlorine and oxygen. In the case of an absorber film composed of a material containing tantalum (Ta), a pattern of the absorber film (absorber pattern) can be formed by dry etching using a gas containing chlorine and no oxygen. The pattern of the hard mask film acts as an etching mask during the dry etching. After the absorber pattern is formed, the hard mask pattern can be removed by dry etching using a gas containing chlorine and oxygen. After removing the hard mask pattern, the absorber film remaining in the area other than the absorber pattern and / or the exposed protective film can be subjected to a treatment in contact with a sulfuric acid-hydrogen peroxide mixture (SPM), for example, by cleaning with a sulfuric acid-hydrogen peroxide mixture (SPM).

[0101] In particular, the reflective mask of the present invention can be manufactured by a method comprising the following steps:

[0102] (A) preparing a reflective mask blank,

[0103] (B) forming a resist pattern on the hard mask film,

[0104] (C) forming a pattern of the hard mask film by dry etching the hard mask film using a gas containing chlorine and oxygen and utilizing the resist pattern as an etching mask,

[0105] (D) forming patterns of the first and second layers in the absorber film by dry etching the first and second layers in the absorber film using a gas containing chlorine and not containing oxygen and utilizing the pattern of the hard mask film as an etching mask,

[0106] (E) after step (C) or (D), removing the resist pattern, and

[0107] (F) The pattern of the hard mask film is removed by dry etching using a gas containing chlorine and oxygen.

[0108] In step (D), dry etching may be performed to expose the protective film. In step (D), dry etching may be performed to leave part of the absorber film, preferably part or all of the first layer without exposing the protective film, and in step (F), dry etching may be performed to expose the protective film.

[0109] The method for manufacturing the reflective mask of the present invention may further comprise the following steps:

[0110] (G) After step (F), a treatment step comprising contacting the exposed absorber film with a sulfuric acid-hydrogen peroxide mixture (SPM).

[0111] When the method for manufacturing a reflective mask of the present invention includes step (G), in steps (D) and (F), dry etching can be performed to leave part of the absorber film without exposing the protective film, and in step (G), dry etching can be performed to expose the protective film.

[0112] When the absorber film consists of a first layer, a second layer and a third layer starting from the substrate side, preferably, the method further comprises the following steps:

[0113] (C-1) After step (C) and before step (D), the pattern of the third layer in the absorber film is formed by dry etching the third layer in the absorber film using a fluorine-based gas and utilizing the pattern of the hard mask film.

[0114] Example

[0115] Examples of the invention are given below by way of illustration and not by way of limitation.

[0116] Experimental Example 1

[0117] As a protective film (thickness: 3.9 nm), a low thermal expansion substrate (SiO 2 -TiO 2A RuNb film (Ru:Nb=82:18 (atomic ratio)) was formed on the main surface of a substrate (based glass substrate). The RuNb film was formed using a multi-cathode sputtering device with a Ru target and a Nb target attached, a low thermal expansion substrate was placed in a chamber, and the RuNb film was formed by DC pulse magnetron sputtering while rotating the substrate. The RuNb film was formed by supplying Ar gas (flow rate: 10 sccm) into the chamber at a pressure in the chamber of 0.016 Pa, and applying an electric power of 400 W to the Ru target and an electric power of 200 W to the Nb target.

[0118] Next, as an absorber film (thickness: 60.0 nm), a TaO layer (Ta:O=70:30 (atomic ratio)) with a thickness of 1.0 nm and a TaN layer (Ta:N=57:43 (atomic ratio)) with a thickness of 59.0 nm were sequentially formed on the RuNb film to obtain a substrate with a film for evaluation. Another sputtering device with a Ta target attached was used to form the TaO layer and the TaN layer, and the substrate on which the RuNb film was formed was placed in a chamber, and the TaO layer and the TaN layer were formed by DC pulsed magnetron sputtering while rotating the substrate. By mixing Ar gas (flow rate: 40 sccm) and O 2 Ar gas (flow rate: 70 sccm) and N 2 Gas (flow rate: 120 sccm) was supplied into the chamber at a pressure in the chamber of 0.48 Pa, and an electric power of 1,800 W was applied to the Ta target to form a TaN layer.

[0119] The obtained substrate in which the protective film and the absorber film were formed was taken out of the chamber into the atmosphere. As a result, it was confirmed that a TaON layer (Ta:O:N=40:30:30 (atomic ratio)) with a thickness of 1.0 nm was formed by natural oxidation on the surface portion of the TaN layer farthest from the protective film.

[0120] Experimental Example 2

[0121] A substrate with a film for evaluation was obtained in the same manner as in Experimental Example 1 except that a TaO layer (Ta:O=80:20 (atomic ratio)) having a thickness of 1.5 nm and a TaN layer having a thickness of 58.5 nm were formed. 2 Gas (flow rate: 30 sccm) was supplied into the chamber at a pressure in the chamber of 0.14 Pa, and an electric power of 1,800 W was applied to the Ta target to form a TaO layer.

[0122] The obtained substrate in which the protective film and the absorber film were formed was taken out of the chamber into the atmosphere. As a result, it was confirmed that a TaON layer (Ta:O:N=40:30:30 (atomic ratio)) with a thickness of 1.0 nm was formed by natural oxidation on the surface portion of the TaN layer farthest from the protective film.

[0123] Experimental Example 3

[0124] Except that a Ta layer having a thickness of 1.5 nm was formed instead of the TaO layer, a substrate with a film for evaluation was obtained in the same manner as in Experimental Example 2. The Ta layer was formed by supplying Ar gas (flow rate: 18 sccm) into the chamber at a pressure in the chamber of 0.07 Pa and applying an electric power of 500 W to the Ta target.

[0125] The obtained substrate in which the protective film and the absorber film were formed was taken out of the chamber into the atmosphere. As a result, it was confirmed that a TaON layer (Ta:O:N=40:30:30 (atomic ratio)) with a thickness of 1.0 nm was formed by natural oxidation on the surface portion of the TaN layer farthest from the protective film.

[0126] Comparative Experiment Example 1

[0127] A substrate with a film for evaluation was obtained in the same manner as in Experimental Example 1, except that a TaN layer having a thickness of 60.0 nm was formed without forming a TaO layer.

[0128] The obtained substrate in which the protective film and the absorber film were formed was taken out of the chamber into the atmosphere. As a result, it was confirmed that a TaON layer (Ta:O:N=40:30:30 (atomic ratio)) with a thickness of 1.0 nm was formed by natural oxidation at the surface portion of the TaN layer farthest from the protective film.

[0129] Experimental Example 4

[0130] As a protective film (thickness: 3.9 nm), a low thermal expansion substrate (SiO 2 -TiO 2 The Ru film was formed on the main surface of a base glass substrate. The Ru film was formed using a sputtering device with a Ru target attached, a low thermal expansion substrate was placed in a chamber, and the Ru film was formed by DC pulse magnetron sputtering while rotating the substrate. The Ru film was formed by supplying Ar gas (flow rate: 10 sccm) into the chamber at a pressure in the chamber of 0.016 Pa and applying an electric power of 400 W to the Ru target.

[0131] Next, as an absorber film (thickness: 60.0 nm), a TaO layer (Ta:O=60:40 (atomic ratio)) with a thickness of 2.0 nm and a TaN layer (Ta:N=57:43 (atomic ratio)) with a thickness of 58.0 nm were sequentially formed on the Ru film to obtain a substrate with a film for evaluation. Another sputtering device with a Ta target attached was used to form the TaO layer and the TaN layer, and the substrate on which the Ru film was formed was placed in a chamber, and the TaO layer and the TaN layer were formed by DC pulsed magnetron sputtering while rotating the substrate. By mixing Ar gas (flow rate: 15 sccm) and O 2 Ar gas (flow rate: 70 sccm) and N 2 Gas (flow rate: 120 sccm) was supplied into the chamber at a pressure in the chamber of 0.48 Pa, and an electric power of 1,800 W was applied to the Ta target to form a TaN layer.

[0132] The obtained substrate in which the protective film and the absorber film were formed was taken out of the chamber into the atmosphere. As a result, it was confirmed that a TaON layer (Ta:O:N=40:30:30 (atomic ratio)) with a thickness of 1.0 nm was formed by natural oxidation on the surface portion of the TaN layer farthest from the protective film.

[0133] Comparative Experiment Example 2

[0134] A substrate with a film for evaluation was obtained in the same manner as in Experimental Example 4, except that a TaN layer having a thickness of 60.0 nm was formed without forming a TaO layer.

[0135] The obtained substrate in which the protective film and the absorber film were formed was taken out of the chamber into the atmosphere. As a result, it was confirmed that a TaON layer (Ta:O:N=40:30:30 (atomic ratio)) with a thickness of 1.0 nm was formed by natural oxidation on the surface portion of the TaN layer farthest from the protective film.

[0136] <Evaluation of protective film and absorbent film>

[0137] Using each of the substrates with films obtained for evaluation in the experimental examples and the comparative experimental examples, the following treatments (i) to (iii) were performed in sequence, and the thickness of the film remaining on the substrate was measured after each of the treatments (i), (ii), and (iii). The thickness of the film was measured by an X-ray diffractometer (SmartLab, manufactured by Rigaku Corporation). The results are shown in Table 1.

[0138] First, dry etching is performed using a fluorine-based gas to remove the TaON layer.

[0139] pass Figure 3 The etching apparatus shown in performs dry etching under the following conditions. Figure 3 1 is a schematic diagram of a dry etching apparatus for dry etching (also applied to the following dry etching). The dry etching apparatus 100 includes a chamber 101, a ground 102, a lower electrode 103, an antenna coil 104, and high-frequency power supplies RF1 and RF2. In this case, a substrate to be processed (a substrate with a film for evaluation) 105 is placed on the lower electrode 103.

[0140] <Conditions for dry etching using fluorine-based gas>

[0141] RF1 (RIE: Reactive Ion Etching): CW (Continuous Discharge) 54W

[0142] RF2 (ICP: Inductively Coupled Plasma): CW (Continuous Discharge) 325W

[0143] Pressure: 5mTorr (0.67Pa)

[0144] SF 6 :18sccm

[0145] He: 130sccm

[0146] Processing time: 10 seconds

[0147] Process (i): Dry etching using a chlorine-containing and oxygen-free gas

[0148] pass Figure 3 The etching device shown in performs dry etching under the following conditions. During etching, the emission spectrum from the plasma is measured by an optical emission spectrometer (OES) equipped in the etching device, the intensity of the emission light originating from nitrogen (N) is monitored, and the point where the intensity of the emission light originating from nitrogen (N) begins to decrease is automatically detected as the end point. 20% of the time (t) from the start of etching to the end point is added to the time (t) as the over-etching time, and the time corresponding to 120% of the time (t) is set as the processing time. The processing time is shown in Table 1.

[0149] <Etching Conditions of Treatment (i)>

[0150] RF1 (RIE: Reactive Ion Etching): CW (Continuous Discharge) 625W

[0151] RF2 (ICP: Inductively Coupled Plasma): CW (Continuous Discharge) 300W

[0152] Pressure: 5mTorr (0.67Pa)

[0153] Cl 2 :150sccm

[0154] He: 10 sccm

[0155] Process (ii): Dry etching using a gas containing chlorine and oxygen

[0156] By showing Figure 3 The etching apparatus in the dry etching was carried out under the following conditions.

[0157] <Etching Conditions of Treatment (ii)>

[0158] RF1 (RIE: Reactive Ion Etching): CW (Continuous Discharge) 625W

[0159] RF2 (ICP: Inductively Coupled Plasma): CW (Continuous Discharge) 300W

[0160] Pressure: 5mTorr (0.67Pa)

[0161] Cl 2 :150sccm

[0162] O 2 :30sccm

[0163] He: 10 sccm

[0164] Processing time: 20 seconds

[0165] Treatment (iii): Cleaning using sulfuric acid-hydrogen peroxide mixture (SPM)

[0166] The substrate with the film for evaluation was immersed in a sulfuric acid-hydrogen peroxide mixture (SPM) of 90 wt % aqueous sulfuric acid solution and 30 wt % hydrogen peroxide solution (aqueous sulfuric acid solution:hydrogen peroxide solution=3:1 (volume ratio)) at room temperature (25° C.) for 6 minutes.

[0167] Table 1

[0168]

[0169] In the substrate with film for evaluation not including the first layer (Comparative Experimental Examples 1 and 2), the thickness of the protective film after treatment (i) was reduced. On the other hand, in the substrate with film for evaluation including the first layer (Experimental Examples 1 to 4), the thickness of the protective film after treatment (i) maintained almost the same thickness as the formed thickness.

[0170] The treatment time of treatment (i) of the substrate with a film for evaluation (Experimental Examples 1, 2, and 4) including a TaO layer as the first layer of the absorber film was long compared to the substrate with a film for evaluation (Comparative Experimental Examples 1 and 2) not including the first layer. It is considered that the detection of the etching endpoint was delayed because nitrogen (N) diffused from the TaN layer to form a TaON layer at the interface portion between the TaO layer and the TaN layer.

[0171] In the substrates with films for evaluation including the first layer (Experimental Examples 1 to 4), the thickness reduction due to treatment (i) was less than that of the substrates with films for evaluation not including the first layer (Comparative Experimental Examples 1 and 2). In particular, in Experimental Examples 2 to 4, a portion of the absorber film (a portion of the first layer) remained after treatment (i).

[0172] In the substrates with films for evaluation in which the protective film was a RuNb film (Experimental Examples 1 to 3 and Comparative Experimental Example 1), the thickness was not reduced by the treatment (ii) in Experimental Examples 1 to 3. In contrast, in Experimental Example 1 and Comparative Experimental Example 1 in which the protective film (RuNb film) was exposed after the treatment (i), the thickness reduction due to the treatment (iii) was large compared to Experimental Examples 2 to 4 in which a portion of the absorber film (a portion of the first layer) remained after the treatment (i).

[0173] In the substrates with films for evaluation in which the protective film was a Ru film (Experimental Example 4 and Comparative Experimental Example 2), the thickness was not reduced by the treatment (ii) in Experimental Example 4 in which a portion of the absorber film (a portion of the first layer) remained after the treatment (i). In contrast, in Comparative Example 2 in which the protective film (Ru film) was exposed after the treatment (i), the thickness reduction due to the treatment (ii) was significantly large.

[0174] In the substrate with a film for evaluation (Experimental Example 1 and Comparative Experimental Example 1) in which the protective film was a RuNb film and the protective film (RuNb film) was exposed after treatment (i), the thickness reduction due to treatment (iii) was large compared to Comparative Experimental Example 2 in which the protective film was a Ru film and the protective film (Ru film) was exposed after treatment (i). Even when the substrate with a film for evaluation included a protective film of a RuNb film, in Experimental Examples 2 to 4 in which a portion of the absorber film (a portion of the first layer) remained after treatment (i), the thickness reduction due to treatment (iii) was small.

Claims

1. A reflective mask blank comprising a substrate, a multilayer reflective film formed on one main surface of the substrate and reflecting exposure light, a protective film formed on and in contact with the multilayer reflective film, an absorber film formed on and in contact with the protective film and absorbing exposure light, and a hard mask film formed on and in contact with the absorber film and serving as an etching mask in dry etching of the absorber film, the reflective mask blank being a material for a reflective mask in EUV lithography using EUV light as exposure light, wherein: The protective film is composed of a material containing ruthenium (Ru) and has a thickness of not less than 2 nm and not more than 5 nm, The absorber film is composed of a material containing tantalum (Ta) and is composed of a first layer and a second layer, or a first layer, a second layer, and a third layer from the substrate side, The first layer has a composition containing tantalum (Ta) and no nitrogen (N), and has a thickness of not less than 0.5 nm and not more than 2 nm, the second layer has a composition including tantalum (Ta) and nitrogen (N), and the composition has a nitrogen (N) content of not less than 10 atomic % and an oxygen (O) content of not more than 5 atomic %, The first layer and the second layer have a total thickness of not less than 50 nm and not more than 80 nm, The third layer has a composition including tantalum (Ta), nitrogen (N) and oxygen (O) and has a thickness of not more than 20 nm, and the composition has an oxygen (O) content of not less than 30 atomic % and not more than 70 atomic %, and The hard mask film is composed of a material including chromium (Cr) and has a thickness of not less than 5 nm and not more than 20 nm. 2 . The reflective mask blank according to claim 1 , wherein the composition of the first layer further comprises oxygen (O). 3 . The reflective mask blank according to claim 2 , wherein the composition of the first layer has an oxygen (O) content of not less than 5 atomic %.

4. The reflective mask blank according to any one of claims 1 to 3, wherein the composition of the second layer has a tantalum (Ta) content of not less than 55 atomic % and not more than 70 atomic % and a nitrogen (N) content of not less than 30 atomic % and not more than 45 atomic %. 5 . The reflective mask blank according to claim 1 , wherein the material containing ruthenium (Ru) is a simple substance of ruthenium (Ru) or an alloy consisting of ruthenium (Ru) and niobium (Nb). 6 . The reflective mask blank according to claim 5 , wherein the alloy composed of ruthenium (Ru) and niobium (Nb) has a niobium (Nb) content of not more than 30 atomic % on average with respect to the entire protective film.

7. A method for manufacturing a reflective mask, comprising the steps of: (A) preparing a reflective mask blank according to any one of claims 1 to 6, (B) forming a resist pattern on the hard mask film, (C) dry etching the hard mask film by using a gas containing chlorine and oxygen and utilizing the resist pattern as an etching mask to form a pattern of the hard mask film, (D) forming patterns of the first and second layers in the absorber film by dry etching the first and second layers in the absorber film using a gas containing chlorine and not containing oxygen and utilizing the pattern of the hard mask film as an etching mask, (E) after step (C) or (D), removing the resist pattern, and (F) Removing the pattern of the hard mask film by dry etching using a gas containing chlorine and oxygen.

8. The method according to claim 7, wherein dry etching is performed in step (D) to expose the protective film.

9. The method according to claim 7, wherein In step (D), dry etching is performed so that a portion of the absorber film remains without exposing the protective film, and In step (F), dry etching is performed to expose the protective film.

10. The method according to claim 8 or 9, further comprising (G) A treatment step subsequent to step (F) comprising contacting the exposed absorber film with a sulfuric acid-hydrogen peroxide mixture (SPM).

11. The method according to claim 7, further comprising (G) a treatment step after step (F) comprising contacting the exposed absorber film with a sulfuric acid-hydrogen peroxide mixture (SPM), wherein In steps (D) and (F), dry etching is performed so that a portion of the absorber film remains without exposing the protective film, and In step (G), dry etching is performed to expose the protective film.

12. The method according to any one of claims 7 to 11, wherein the absorber film consists of a first layer, a second layer and a third layer starting from the substrate side, and The method further comprises the following steps: (C-1) After step (C) and before step (D), the pattern of the third layer in the absorber film is formed by dry etching the third layer in the absorber film using a fluorine-based gas and utilizing the pattern of the hard mask film.

Citation Information

Patent Citations

  • Reflective photomask

    JP2002122981A

  • Reflecting type exposure mask, its manufacturing method and semiconductor element

    JP2002246299A