High-strength and high-conductivity composite bipolar plate and preparation method thereof
By combining graphite, carbon black, and carbon fiber compositions with specific particle sizes and lengths with polytetrafluoroethylene resin and powdered phenolic resin, the problem of insufficient strength and conductive properties of the composite bipolar plate is solved, and efficient conductivity and mechanical properties are achieved. Improved strength, suitable for high temperature environments and mass production.
Patent Information
- Application Number
- CN202410975384.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing composite bipolar plates have insufficient strength and conductive properties, resulting in short service life and high cost in high temperature environments, which limits their industrial application in the field of fuel cells.
Graphite of a specific particle size, conductive carbon black and carbon fiber of a specific length are used as the conductive composition, and through the combination of polytetrafluoroethylene resin and powdered phenolic resin, a dense and orderly conductive path is formed through shearing and rolling processes. Improve the electrical conductivity and mechanical strength of bipolar plates.
A composite bipolar plate with excellent conductivity and strength in high-temperature environments has been achieved, which reduces production costs, is suitable for mass production, and extends service life.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fuel cells, and in particular to a high-strength and high-conductivity composite bipolar plate and a preparation method thereof. Background Art
[0002] Bipolar plates are a core component of fuel cells. There are many types of bipolar plates on the market, such as metal bipolar plates, graphite bipolar plates, and graphite composite bipolar plates. At present, the preparation technology of metal plate and graphite plate stacks is relatively mature and has been widely used. Graphite bipolar plates have good conductivity but poor strength and short service life. Metal bipolar plates have good conductivity and high strength but poor corrosion resistance. Graphite composite bipolar plates combine the advantages of the former two and have the most balanced performance. They are one of the future development directions of bipolar plates. However, composite bipolar plates have not yet been put into mass production because their strength and conductivity do not meet the requirements, and some process preparations require multiple modification reactions, which are cumbersome and costly. Therefore, improving mechanical and conductive properties is of great significance to the industrial production of composite bipolar plates.
[0003] Therefore, there is an urgent need for a composite bipolar plate and a preparation method thereof to solve the deficiencies of the existing technical problems. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides a high-strength and high-conductivity composite bipolar plate and a preparation method thereof to solve the problems of strength and conductivity of the composite bipolar plate in the prior art. To achieve the above purpose, the present invention provides a composite bipolar plate and a preparation method thereof.
[0005] In one aspect, the present application provides a high-strength and high-conductivity composite bipolar plate, wherein the raw materials for preparing the composite bipolar plate include: 80-98% conductive composition; 0.5-5% polytetrafluoroethylene resin; 1-20% powdered phenolic resin; The conductive composition comprises graphite, carbon fiber and conductive carbon black; the average particle size of the graphite is 20 μm-200 μm; the carbon fiber is chopped carbon fiber with an average diameter of 5 μm-20 μm and a length of 2 mm-20 mm; the particle size of the conductive carbon black is 8-20 μm.
[0006] Graphite has excellent high temperature resistance and electrical conductivity, and maintains good strength at high temperatures. As a conductive material, it gives the bipolar sheet good conductivity and strength, and can be used in high temperature environments. Graphite has good lubricity and toughness, and can be mixed with other components to facilitate the formation of sheets through roller molding. Carbon fiber and conductive carbon black are also commonly used conductive materials. Carbon fiber also has high temperature resistance and corrosion resistance. The excellent orientation of carbon fiber in the fiber axis makes it have high strength in the fiber axis direction. Conductive carbon black also has good high temperature resistance and corrosion resistance.
[0007] The applicant tried to use the above three conductive components as a conductive mixture when seeking to prepare a bipolar plate with better conductivity and strength. At the same time, it was found that by selecting graphite of a specific particle size and conductive carbon black of a specific particle size, and selecting millimeter-level carbon fibers of a specific range of length as the conductive composition, satisfactory conductivity and mechanical strength were obtained. This may be because within the above particle size range, graphite undergoes interlayer sliding after rolling due to its lamellar structure, while carbon black has a similar mesh plane, and its interlayer spacing is slightly larger than that of graphite, and the carbon between the two layers is randomly arranged. The interlayer stacking of the two is achieved through common rolling and high-temperature pressing. The carbon black presents an orderly arrangement on the graphite surface layer, which improves the interaction force and density of the two, and has better conductivity. The conductive carbon black particle size is relatively large and has poor stacking on the graphite surface, while the conductive carbon black particle size is relatively small and is not conducive to forming an orderly arrangement structure. In addition, when carbon fibers of a specific length participate in the co-pressing molding, they act as medium-long chains in the conductive network, further overlapping the carbon black and graphite to form a The network pathway is formed to improve the conductivity. After pressing, the pores between graphite and carbon black become smaller and the longitudinal strength is increased. The carbon fiber improves the lateral strength of the material due to its axial strength effect. The three work together to give the bipolar plate better strength. Under the graphene particle size and carbon black particle size of the present application, the effect achieved when the carbon fiber length is within the above range is better. If the carbon fiber is too long, the longitudinal orientation is more obvious, which is not conducive to building more conductive pathways between graphite and carbon black when they are pressed together. If the length of the carbon fiber is too short, its strength is slightly poor and it is not conducive to forming a continuous conductive pathway. By selecting the above-mentioned length of carbon fiber and matching graphite and carbon black with corresponding particle sizes, it is possible to achieve both bipolar plate strength and conductivity.
[0008] Polytetrafluoroethylene resin has excellent high temperature resistance and chemical resistance. As a resin added to the bipolar plate, it can further improve the high temperature resistance. Compared with the conventional composite bipolar plate, the resin on the surface of the conductive filler after pressing is bonded to each other and solidified into a whole. The polytetrafluoroethylene of this application is adhered to the surface of the conductive composition after shearing, and the initial bonding of the components of the bipolar plate is achieved. The particles are arranged in an orderly manner and the conductive composition is avoided from being completely coated, thereby improving the conductivity of the bipolar plate. In addition, phenolic resin also has excellent high temperature resistance and corrosion resistance. The phenolic resin is added and pressed and solidified at high temperature. The powdered phenolic resin melted at high temperature can fill the gaps between the conductive fillers, while increasing the strength and air tightness of the product. The inventors achieved a dense and orderly arrangement by selecting conductive fillers of specific particle size and length as the conductive composition, forming a more effective conductive path. At the same time, the combination of particle size and length takes into account both strength and conductivity. On the basis of the above conductive composition, polytetrafluoroethylene is used for bonding and phenolic resin is melt-filled and solidified to make the combination arrangement more orderly and dense. The obtained two-stage board has excellent strength and conductivity, and is also resistant to high temperature and corrosion, and can be used in high temperature environments.
[0009] Preferably, the average particle size of the graphite is 50μm-150μm; more preferably 60μm-120μm; more preferably 80μm-100μm; preferably, the average diameter of the chopped carbon fiber is 8μm-15μm, the length is 5mm-10mm, more preferably the length is 6mm-8mm; preferably, the particle size of the conductive carbon black is 10-20μm.
[0010] Preferably, the mass ratio of the graphite, carbon fiber and conductive carbon black is (30-50):(1-3):(30-50).
[0011] Formulating the conductive mixture within the above range is conducive to forming continuous and more conductive paths and improving conductivity.
[0012] Preferably, the average particle size of the polytetrafluoroethylene resin is 0.1 μm-1000 μm; the average particle size of the powdered phenolic resin is 10 μm-150 μm; more preferably, the average particle size of the polytetrafluoroethylene resin is 0.1 μm-700 μm; the average particle size of the powdered phenolic resin is 10 μm-100 μm.
[0013] The particle size selection of the powdered phenolic resin has an impact on the performance of the bipolar plate. The powdered phenolic resin is more conducive to melt filling at the above particle size, thereby improving the density of the bipolar plate and reducing the pores.
[0014] Preferably, the mass ratio of the conductive composition to the polytetrafluoroethylene resin is 30:150:1; the mass ratio of the polytetrafluoroethylene resin to the powdered phenolic resin is 1:4-1:8.
[0015] Adjusting the amount of polytetrafluoroethylene and phenolic resin is conducive to achieving better bonding and sorting of the conductive composition. Under the above ratio, polytetrafluoroethylene shows better conductivity and strength. When it is lower than the above range, it is not conducive to rolling to form an orderly arrangement. When it is higher than the above range, the final wrapping of the conductive composition increases, resulting in a decrease in conductivity. In addition, the content of phenolic resin will increase the final structural strength, but the increased strength is limited, and the increase of phenolic resin will reduce a certain degree of conductivity.
[0016] Preferably, the graphite is a mixed graphite with a mass ratio of worm graphite to flake graphite of 1:(6-10).
[0017] The addition of a small amount of worm graphite can improve plasticity, and the intercalation effect of the worm graphite itself is conducive to the accumulation of carbon fiber and conductive carbon black, enriching the conductive pathway between carbon fiber, conductive carbon black and graphite. However, the addition of too much worm graphite is not conducive to the compaction of the material and the reduction of the pores between particles, which affects the performance of the bipolar plate.
[0018] On the other hand, the present application provides a method for preparing a high-strength and high-conductivity composite bipolar plate, comprising the following steps: Step 1: Weigh the raw materials according to the ratio; Step 2: Shearing and mixing the conductive composition at a shearing speed of 10-20 m / s and a mixing time of 5-15 min to form a first mixture; Step 3: adding polytetrafluoroethylene resin to the first mixture, performing high-speed shearing, with a shearing line speed of 40-60 m / s and a shearing time of 15-25 min, to form a second mixture; Step 4: adding the powdered phenolic resin to the second mixture and performing shear mixing at a shear line speed of 10-20 m / s and a mixing time of 5-15 min to form a third mixture; Step 5: compressing the third mixture into blocks, and then continuously rolling to form a sheet; preferably, forming a sheet with a density of 1.5-1.6 g / cm3; Step 6: The sheet material in step 5 is subjected to hot pressing at a temperature of 240-280° C. and a pressure of 50-70 MPa for 15-25 min to obtain a composite bipolar plate.
[0019] In the traditional composite bipolar plate process, a layer of resin is first coated on the surface of the conductive filler, and then the resin on the surface of the conductive filler is bonded and solidified into a whole through high-temperature molding. The conductive filler coated with resin will significantly reduce the conductivity. In the present invention, a small amount of polytetrafluoroethylene filaments are adhered to the surface of the conductive filler composition by shearing the raw materials and continuous rolling. The surface of the conductive filler will not be completely coated with the resin, and the orderly arrangement between the conductive compositions increases the density. In addition, the conductive material after rolling is also denser, with more conductive pathways, lower contact resistance between the conductive materials, and better conductivity. On this basis, high temperature and high pressure pressing is performed, and the powdered phenolic resin melted at high temperature can fill the gaps between the conductive fillers, while increasing the strength and air tightness of the product.
[0020] Compared with the existing process, the present application does not require complicated modification processes and achieves higher conductivity and strength, has low cost, and is conducive to large-scale production.
[0021] In summary, this application has at least the following beneficial effects: 1. By selecting graphite of a specific particle size, conductive carbon black and carbon fiber of a specific particle size length as the conductive composition to achieve a dense and orderly arrangement, a more effective conductive path is formed, taking into account both strength and conductivity. On the basis of the above conductive composition, polytetrafluoroethylene is bonded and phenolic resin is melted, filled and solidified to make the combination arrangement more orderly and dense. The obtained bipolar plate has excellent strength and conductivity, and is resistant to high temperature and corrosion, and can be used in high temperature environments. At the same time, regulating the particle size of the powdered phenolic resin is more conducive to melt filling, improving the density of the bipolar plate and reducing pores; 2. The bipolar plates prepared by regulating the content of polytetrafluoroethylene show better conductivity and strength. If the content is lower than the above range, the adhesion is reduced, which is not conducive to rolling to form an orderly arrangement. If the content is higher than the above range, the wrapping of the conductive composition will increase, resulting in a decrease in conductivity. The content of phenolic resin is regulated so that the final structural strength has both excellent conductivity and strength; 3. The plasticity is improved by adding a small amount of worm graphite, and the intercalation effect of worm graphite itself is conducive to the accumulation of carbon fiber and conductive carbon black, enriching the conductive path between carbon fiber, conductive carbon black and graphite, taking into account the compaction of the material and reducing the pores between particles, thereby improving the strength and conductivity of the bipolar plate.
[0022] 4. Through raw material shearing and continuous rolling, a small amount of polytetrafluoroethylene filaments adhere to the surface of the conductive filler composition, and the surface of the conductive filler will not be completely covered by the resin, which promotes the effective horizontal arrangement of conductivity and increases the density. Then, the powdered phenolic resin is melted at high temperature to fill the gaps between the conductive fillers, thereby increasing the strength and air tightness of the product. DETAILED DESCRIPTION
[0023] The present application is further described in detail below in conjunction with the examples. The particle size of polytetrafluoroethylene in the examples or comparative examples is 500 μm; the experimental reagents in the examples or comparative examples, unless otherwise specified, are conventional commercial brands or obtained through conventional preparation processes.
[0024] Embodiment 1: The composite bipolar plate was prepared according to the following steps: Step 1: weigh the raw materials according to the ratio: 4 kg of graphite with a particle size of 100 μm, 4 kg of conductive carbon black with a particle size of 20 μm, 0.2 kg of carbon fiber with a diameter of 10 μm and a length of 6 mm, 0.2 kg of polytetrafluoroethylene resin, and 1 kg of powdered phenolic resin with a particle size of 100 μm; the graphite is flake graphite; Step 2: Shear-mixing graphite, conductive carbon black and carbon fiber at a shearing speed of 15 m / s and a mixing time of 10 min to form a first mixture; Step 3: adding polytetrafluoroethylene resin to the first mixture, performing high-speed shearing, with a shearing line speed of 50 m / s and a shearing time of 20 min, to form a second mixture; Step 4: adding the powdered phenolic resin to the second mixture and performing shear mixing at a shear speed of 15 m / s and a mixing time of 10 min to form a third mixture; Step 5: compressing the third mixture into blocks, and then continuously rolling to form a sheet; Step 6: The sheet material described in step 5 is hot-pressed at a temperature of 260° C. and a pressure of 60 MPa for 20 min to obtain a composite bipolar plate.
[0025] Embodiment 2: Prepare the composite bipolar plate according to the following steps: Step 1: weigh the raw materials according to the ratio: 5 kg of graphite with a particle size of 100 μm, 3 kg of conductive carbon black with a particle size of 20 μm, 0.2 kg of carbon fiber with a diameter of 10 μm and a length of 6 mm, 0.2 kg of polytetrafluoroethylene resin, and 1 kg of powdered phenolic resin with a particle size of 100 μm; the graphite is flake graphite; Step 2: Shear-mixing graphite, conductive carbon black and carbon fiber at a shearing speed of 15 m / s and a mixing time of 10 min to form a first mixture; Step 3: adding polytetrafluoroethylene resin to the first mixture, performing high-speed shearing, with a shearing line speed of 50 m / s and a shearing time of 20 min, to form a second mixture; Step 4: adding the powdered phenolic resin to the second mixture and performing shear mixing at a shear speed of 15 m / s and a mixing time of 10 min to form a third mixture; Step 5: compressing the third mixture into blocks, and then continuously rolling to form a sheet; Step 6: The sheet material described in step 5 is hot-pressed at a temperature of 260° C. and a pressure of 60 MPa for 20 min to obtain a composite bipolar plate.
[0026] Embodiment 3: Prepare the composite bipolar plate according to the following steps: Step 1: weigh the raw materials according to the ratio: 4 kg of graphite with a particle size of 100 μm, 4 kg of conductive carbon black with a particle size of 20 μm, 0.2 kg of carbon fiber with a diameter of 10 μm and a length of 6 mm, 0.4 kg of polytetrafluoroethylene resin, and 0.8 kg of powdered phenolic resin with a particle size of 100 μm; the graphite is flake graphite; Step 2: Shear-mixing graphite, conductive carbon black and carbon fiber at a shearing speed of 15 m / s and a mixing time of 10 min to form a first mixture; Step 3: adding polytetrafluoroethylene resin to the first mixture, performing high-speed shearing, with a shearing line speed of 50 m / s and a shearing time of 20 min, to form a second mixture; Step 4: adding the powdered phenolic resin to the second mixture and performing shear mixing at a shear speed of 15 m / s and a mixing time of 10 min to form a third mixture; Step 5: compressing the third mixture into blocks, and then continuously rolling to form a sheet; Step 6: The sheet material described in step 5 is hot-pressed at a temperature of 260° C. and a pressure of 60 MPa for 20 min to obtain a composite bipolar plate.
[0027] Embodiment 4: Prepare the composite bipolar plate according to the following steps: Step 1: weigh the raw materials according to the ratio: 4 kg of graphite with a particle size of 50 μm, 4 kg of conductive carbon black with a particle size of 10 μm, 0.2 kg of carbon fiber with a diameter of 10 μm and a length of 6 mm, 0.2 kg of polytetrafluoroethylene resin, and 1 kg of powdered phenolic resin with a particle size of 100 μm; the graphite is flake graphite; Step 2: Shear-mixing graphite, conductive carbon black and carbon fiber at a shearing speed of 15 m / s and a mixing time of 10 min to form a first mixture; Step 3: adding polytetrafluoroethylene resin to the first mixture, performing high-speed shearing, with a shearing line speed of 50 m / s and a shearing time of 20 min, to form a second mixture; Step 4: adding the powdered phenolic resin to the second mixture and performing shear mixing at a shear speed of 15 m / s and a mixing time of 10 min to form a third mixture; Step 5: compressing the third mixture into blocks, and then continuously rolling to form a sheet; Step 6: The sheet material described in step 5 is hot-pressed at a temperature of 260° C. and a pressure of 60 MPa for 20 min to obtain a composite bipolar plate.
[0028] Embodiment 5: Prepare the composite bipolar plate according to the following steps: Step 1: weigh the raw materials according to the ratio: 4 kg of graphite with a particle size of 100 μm, 4 kg of conductive carbon black with a particle size of 20 μm, 0.2 kg of carbon fiber with a diameter of 10 μm and a length of 20 mm, 0.2 kg of polytetrafluoroethylene resin, and 1 kg of powdered phenolic resin with a particle size of 100 μm; the graphite is flake graphite; Step 2: Shear-mixing graphite, conductive carbon black and carbon fiber at a shearing speed of 15 m / s and a mixing time of 10 min to form a first mixture; Step 3: adding polytetrafluoroethylene resin to the first mixture, performing high-speed shearing, with a shearing line speed of 50 m / s and a shearing time of 20 min, to form a second mixture; Step 4: adding the powdered phenolic resin to the second mixture and performing shear mixing at a shear speed of 15 m / s and a mixing time of 10 min to form a third mixture; Step 5: compressing the third mixture into blocks, and then continuously rolling to form a sheet; Step 6: The sheet material described in step 5 is hot-pressed at a temperature of 260° C. and a pressure of 60 MPa for 20 min to obtain a composite bipolar plate.
[0029] Embodiment 6: Prepare the composite bipolar plate according to the following steps: Step 1: weigh the raw materials according to the ratio: 4 kg of graphite with a particle size of 100 μm, 4 kg of conductive carbon black with a particle size of 20 μm, 0.2 kg of carbon fiber with a diameter of 10 μm and a length of 6 mm, 0.2 kg of polytetrafluoroethylene resin, and 1 kg of powdered phenolic resin with a particle size of 100 μm; the graphite is 0.4 kg of worm graphite and 3.6 kg of flake graphite; Step 2: Shear-mixing graphite, conductive carbon black and carbon fiber at a shearing speed of 15 m / s and a mixing time of 10 min to form a first mixture; Step 3: adding polytetrafluoroethylene resin to the first mixture, performing high-speed shearing, with a shearing line speed of 50 m / s and a shearing time of 20 min, to form a second mixture; Step 4: adding the powdered phenolic resin to the second mixture and performing shear mixing at a shear speed of 15 m / s and a mixing time of 10 min to form a third mixture; Step 5: compressing the third mixture into blocks, and then continuously rolling to form a sheet; Step 6: The sheet material described in step 5 is hot-pressed at a temperature of 260° C. and a pressure of 60 MPa for 20 min to obtain a composite bipolar plate.
[0030] Embodiment 7: Prepare the composite bipolar plate according to the following steps: Step 1: weigh the raw materials according to the ratio: 4 kg of graphite with a particle size of 100 μm, 4 kg of conductive carbon black with a particle size of 20 μm, 0.2 kg of carbon fiber with a diameter of 10 μm and a length of 6 mm, 0.2 kg of polytetrafluoroethylene resin, and 1 kg of powdered phenolic resin with a particle size of 100 μm; the graphite is 1 kg of worm graphite and 3 kg of flake graphite; Step 2: Shear-mixing graphite, conductive carbon black and carbon fiber at a shearing speed of 15 m / s and a mixing time of 10 min to form a first mixture; Step 3: adding polytetrafluoroethylene resin to the first mixture, performing high-speed shearing, with a shearing line speed of 50 m / s and a shearing time of 20 min, to form a second mixture; Step 4: adding the powdered phenolic resin to the second mixture and performing shear mixing at a shear speed of 15 m / s and a mixing time of 10 min to form a third mixture; Step 5: compressing the third mixture into blocks, and then continuously rolling to form a sheet; Step 6: The sheet material described in step 5 is hot-pressed at a temperature of 260° C. and a pressure of 60 MPa for 20 min to obtain a composite bipolar plate.
[0031] Embodiment 8: Prepare the composite bipolar plate according to the following steps: Step 1: weigh the raw materials according to the ratio: 4 kg of graphite with a particle size of 100 μm, 4 kg of conductive carbon black with a particle size of 20 μm, 0.2 kg of carbon fiber with a diameter of 10 μm and a length of 6 mm, 0.2 kg of polytetrafluoroethylene resin, and 1 kg of powdered phenolic resin with a particle size of 100 μm; the graphite is flake graphite; Step 2: Shear-mixing graphite, conductive carbon black and carbon fiber at a shearing speed of 15 m / s and a mixing time of 10 min to form a first mixture; Step 3: adding polytetrafluoroethylene resin to the first mixture, performing high-speed shearing, with a shearing line speed of 50 m / s and a shearing time of 20 min, to form a second mixture; Step 4: adding the powdered phenolic resin to the second mixture and performing shear mixing at a shear speed of 15 m / s and a mixing time of 10 min to form a third mixture; Step 5: The third mixture described in step 4 is subjected to high temperature and high pressure lamination and shaping at a temperature of 260° C. and a pressure of 60 MPa for 20 min to obtain a composite bipolar plate.
[0032] Comparative Example 1: Prepare the composite bipolar plate according to the following steps: Step 1: weigh the raw materials according to the ratio: 4 kg of graphite with a particle size of 100 μm, 4 kg of conductive carbon black with a particle size of 20 μm, 0.2 kg of carbon fiber with a diameter of 10 μm and a length of 6 mm, 0.03 kg of polytetrafluoroethylene resin, and 1.17 kg of powdered phenolic resin with a particle size of 100 μm; the graphite is flake graphite; Step 2: Shear-mixing graphite, conductive carbon black and carbon fiber at a shearing speed of 15 m / s and a mixing time of 10 min to form a first mixture; Step 3: adding polytetrafluoroethylene resin to the first mixture, performing high-speed shearing, with a shearing line speed of 50 m / s and a shearing time of 20 min, to form a second mixture; Step 4: adding the powdered phenolic resin to the second mixture and performing shear mixing at a shear speed of 15 m / s and a mixing time of 10 min to form a third mixture; Step 5: compressing the third mixture into blocks, and then continuously rolling to form a sheet; Step 6: The sheet material described in step 5 is hot-pressed at a temperature of 260° C. and a pressure of 60 MPa for 20 min to obtain a composite bipolar plate.
[0033] Comparative Example 2: Prepare the composite bipolar plate according to the following steps: Step 1: weigh the raw materials according to the ratio: 4 kg of graphite with a particle size of 100 μm, 4 kg of conductive carbon black with a particle size of 20 μm, 0.2 kg of carbon fiber with a diameter of 10 μm and a length of 6 mm, 0.7 kg of polytetrafluoroethylene resin, and 0.5 kg of powdered phenolic resin with a particle size of 100 μm; the graphite is flake graphite; Step 2: Shear-mixing graphite, conductive carbon black and carbon fiber at a shearing speed of 15 m / s and a mixing time of 10 min to form a first mixture; Step 3: adding polytetrafluoroethylene resin to the first mixture, performing high-speed shearing, with a shearing line speed of 50 m / s and a shearing time of 20 min, to form a second mixture; Step 4: adding the powdered phenolic resin to the second mixture and performing shear mixing at a shear speed of 15 m / s and a mixing time of 10 min to form a third mixture; Step 5: compressing the third mixture into blocks, and then continuously rolling to form a sheet; Step 6: The sheet material described in step 5 is hot-pressed at a temperature of 260° C. and a pressure of 60 MPa for 20 min to obtain a composite bipolar plate.
[0034] Comparative Example 3: Prepare the composite bipolar plate according to the following steps: Step 1: weigh the raw materials according to the ratio: 4 kg of graphite with a particle size of 100 μm, 4 kg of conductive carbon black with a particle size of 2 μm, 0.2 kg of carbon fiber with a diameter of 10 μm and a length of 6 mm, 0.2 kg of polytetrafluoroethylene resin, and 1 kg of powdered phenolic resin with a particle size of 100 μm; the graphite is flake graphite; Step 2: Shear-mixing graphite, conductive carbon black and carbon fiber at a shearing speed of 15 m / s and a mixing time of 10 min to form a first mixture; Step 3: adding polytetrafluoroethylene resin to the first mixture, performing high-speed shearing, with a shearing line speed of 50 m / s and a shearing time of 20 min, to form a second mixture; Step 4: adding the powdered phenolic resin to the second mixture and performing shear mixing at a shear speed of 15 m / s and a mixing time of 10 min to form a third mixture; Step 5: compressing the third mixture into blocks, and then continuously rolling to form a sheet; Step 6: The sheet material described in step 5 is hot-pressed at a temperature of 260° C. and a pressure of 60 MPa for 20 min to obtain a composite bipolar plate.
[0035] Comparative Example 4: Prepare the composite bipolar plate according to the following steps: Step 1: weigh the raw materials according to the ratio: 4 kg of graphite with a particle size of 100 μm, 4 kg of conductive carbon black with a particle size of 30 μm, 0.2 kg of carbon fiber with a diameter of 10 μm and a length of 6 mm, 0.2 kg of polytetrafluoroethylene resin, and 1 kg of powdered phenolic resin with a particle size of 100 μm; the graphite is flake graphite; Step 2: Shear-mixing graphite, conductive carbon black and carbon fiber at a shearing speed of 15 m / s and a mixing time of 10 min to form a first mixture; Step 3: adding polytetrafluoroethylene resin to the first mixture, performing high-speed shearing, with a shearing line speed of 50 m / s and a shearing time of 20 min, to form a second mixture; Step 4: adding the powdered phenolic resin to the second mixture and performing shear mixing at a shear speed of 15 m / s and a mixing time of 10 min to form a third mixture; Step 5: compressing the third mixture into blocks, and then continuously rolling to form a sheet; Step 6: The sheet material described in step 5 is hot-pressed at a temperature of 260° C. and a pressure of 60 MPa for 20 min to obtain a composite bipolar plate.
[0036] Comparative Example 5: Prepare the composite bipolar plate according to the following steps: Step 1: weigh the raw materials according to the ratio: 4 kg of graphite with a particle size of 100 μm, 4 kg of conductive carbon black with a particle size of 20 μm, 0.2 kg of carbon fiber with a diameter of 10 μm and a length of 1 mm, 0.2 kg of polytetrafluoroethylene resin, and 1 kg of powdered phenolic resin with a particle size of 100 μm; the graphite is flake graphite; Step 2: Shear-mixing graphite, conductive carbon black and carbon fiber at a shearing speed of 15 m / s and a mixing time of 10 min to form a first mixture; Step 3: adding polytetrafluoroethylene resin to the first mixture, performing high-speed shearing, with a shearing line speed of 50 m / s and a shearing time of 20 min, to form a second mixture; Step 4: adding the powdered phenolic resin to the second mixture and performing shear mixing at a shear speed of 15 m / s and a mixing time of 10 min to form a third mixture; Step 5: compressing the third mixture into blocks, and then continuously rolling to form a sheet; Step 6: The sheet material described in step 5 is hot-pressed at a temperature of 260° C. and a pressure of 60 MPa for 20 min to obtain a composite bipolar plate.
[0037] Comparative Example 6: Prepare the composite bipolar plate according to the following steps: Step 1: weigh the raw materials according to the ratio: 4 kg of graphite with a particle size of 100 μm, 4 kg of conductive carbon black with a particle size of 20 μm, 0.2 kg of carbon fiber with a diameter of 10 μm and a length of 30 mm, 0.2 kg of polytetrafluoroethylene resin, and 1 kg of powdered phenolic resin with a particle size of 100 μm; the graphite is flake graphite; Step 2: Shear-mixing graphite, conductive carbon black and carbon fiber at a shearing speed of 15 m / s and a mixing time of 10 min to form a first mixture; Step 3: adding polytetrafluoroethylene resin to the first mixture, performing high-speed shearing, with a shearing line speed of 50 m / s and a shearing time of 20 min, to form a second mixture; Step 4: adding the powdered phenolic resin to the second mixture and performing shear mixing at a shear speed of 15 m / s and a mixing time of 10 min to form a third mixture; Step 5: compressing the third mixture into blocks, and then continuously rolling to form a sheet; Step 6: The sheet material described in step 5 is hot-pressed at a temperature of 260° C. and a pressure of 60 MPa for 20 min to obtain a composite bipolar plate.
[0038] Performance testing: The bipolar plates prepared in Examples 1-8 and Comparative Examples 1-6 were tested, and the test results are shown in Table 1: Tensile strength(MPa) <![CDATA[Conductivity (S.cm -1 )]]> Density(g / cm3) Example 1 30 268 1.96 Example 2 33 280 1.98 Example 3 27 274 1.91 Example 4 31 263 1.93 Example 5 35 292 1.94 Example 6 34 274 1.92 Example 7 28 262 1.90 Example 8 18 230 1.74 Comparative Example 1 21 172 1.92 Comparative Example 2 20 190 1.87 Comparative Example 3 28 220 1.94 Comparative Example 4 27 204 1.92 Comparative Example 5 24 235 1.95 Comparative Example 6 26 230 1.91 It can be seen from Examples 1-5 of the present application that the bipolar plate prepared by the present application through the graphite of specific particle size, conductive carbon black, carbon fiber of specific diameter and length combined with corresponding content of polytetrafluoroethylene resin and powdered phenolic resin has excellent conductivity and tensile strength, and its conductivity reaches 230-300S.cm -1 , the tensile strength can reach 27-35MPa.
[0039] It can be seen from Example 1 and Comparative Examples 1-2 that the conductivity and tensile strength are poor when the content of polytetrafluoroethylene resin is too much or too little. Combining Example 1 and Comparative Examples 3-6, it can be seen that the carbon black particle size and carbon fiber length parameters both affect the conductivity. Appropriate parameter selection is conducive to the orderly arrangement and stacking of particles, reduces the particle pores, and can construct more conductive pathways, thereby greatly improving the conductivity and strength of the bipolar plate.
[0040] It can be seen from Example 1 and Examples 6-7 that the addition of a small amount of worm graphite can improve strength and conductivity, and the performance improvement is more obvious when the added content is controlled within a reasonable range.
[0041] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A high-strength and high-conductivity composite bipolar plate, characterized in that: The raw materials for preparing the composite bipolar plate include: 80-98% conductive composition; 5~5% polytetrafluoroethylene resin; 1-20% powdered phenolic resin; The conductive composition comprises graphite, carbon fiber and conductive carbon black; the average particle size of the graphite is 20 μm-200 μm; the carbon fiber is chopped carbon fiber with an average diameter of 5 μm-20 μm and a length of 2 mm-20 mm; the particle size of the conductive carbon black is 8-20 μm.
2. The high-strength and high-conductivity composite bipolar plate according to claim 1, characterized in that: The average particle size of the graphite is 50 μm-150 μm; the average diameter of the chopped carbon fiber is 8 μm-15 μm, and the length is 5 mm-10 mm; the particle size of the conductive carbon black is 10-20 μm.
3. The high-strength and high-conductivity composite bipolar plate according to claim 1, characterized in that: The mass ratio of the graphite, carbon fiber and conductive carbon black is (30-50):(1-3):(30-50).
4. The high-strength and high-conductivity composite bipolar plate according to claim 1, characterized in that: The average particle size of the polytetrafluoroethylene resin is 0.1 μm-1000 μm; the average particle size of the powdered phenolic resin is 10 μm-150 μm.
5. The high-strength and high-conductivity composite bipolar plate according to claim 4, characterized in that: The average particle size of the polytetrafluoroethylene resin is 0.1 μm-700 μm; the average particle size of the powdered phenolic resin is 10 μm-100 μm.
6. The high-strength and high-conductivity composite bipolar plate according to claim 1, characterized in that: The mass ratio of the conductive composition to the polytetrafluoroethylene resin is 30:150:
1.
7. The high-strength and high-conductivity composite bipolar plate according to claim 1, characterized in that: The mass ratio of the polytetrafluoroethylene resin to the powdered phenolic resin is 1:4-1:
8.
8. The high-strength and high-conductivity composite bipolar plate according to claim 1, characterized in that: The graphite is a mixed graphite with a mass ratio of worm graphite to flake graphite of 1:(6-10).
9. A method for preparing a high-strength and high-conductivity composite bipolar plate according to any one of claims 1 to 8, characterized in that: The steps include: Step 1: Weigh the raw materials according to the ratio; Step 2: Shearing and mixing the conductive composition at a shearing speed of 10-20 m / s and a mixing time of 5-15 min to form a first mixture; Step 3: adding polytetrafluoroethylene resin to the first mixture, performing high-speed shearing, with a shearing line speed of 40-60 m / s and a shearing time of 15-25 min, to form a second mixture; Step 4: adding the powdered phenolic resin to the second mixture and performing shear mixing at a shear line speed of 10-20 m / s and a mixing time of 5-15 min to form a third mixture; Step 5: compressing the third mixture into blocks, and then continuously rolling to form a sheet; Step 6: The sheet material described in step 5 is subjected to hot pressing at a temperature of 240-280° C. and a pressure of 50-70 MPa for 15-25 min to obtain a composite bipolar plate.
Citation Information
Cited By
Bipolar plate, preparation method and flow battery
CN120149445A