Non-aqueous electrolyte for secondary battery, secondary battery and electronic device
By using specific compounds in non-aqueous electrolytes in secondary batteries, a synergistic effect is formed to enhance the stability of the positive and negative electrode interfaces, solving the problems of insufficient high-temperature impedance growth rate and cycle performance of secondary batteries in the existing technology, and achieving Better cycle performance and high temperature storage performance.
Patent Information
- Application Number
- CN202410798008.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-15
AI Technical Summary
Existing secondary batteries have deficiencies in resistance growth rate and cycle performance under high temperature conditions, especially due to excessive viscosity or high film formation resistance caused by additives, which reduces low-temperature discharge performance and cycle performance.
Using a non-aqueous electrolyte containing specific compounds such as cyano or fluorine-substituted alkyl compounds, by adjusting their content in the electrolyte, a synergistic effect is formed to enhance the stability of the positive and negative electrode interfaces and reduce the decomposition of the electrolyte. Improves cycling performance and high-temperature storage performance.
It effectively improves the cycle performance and high-temperature storage performance of lithium-ion batteries. By stabilizing the interface and reducing electrolyte decomposition, it moderates the viscosity of the electrolyte and improves the overall performance of the battery.
Smart Images

Figure CN118782901A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of electrochemical technology, and in particular to a non-aqueous electrolyte for a secondary battery, a secondary battery and an electronic device. Background Art
[0002] With the widespread application of secondary batteries in various electronic products, users have also put forward higher and higher requirements for the performance of secondary batteries, especially the high-temperature impedance growth rate and cycle performance. In related technologies, electrolyte additives are mostly used to improve the high-temperature impedance growth rate and cycle performance of secondary batteries. However, most additives improve the high-temperature impedance growth rate by forming a film on the positive electrode, but often because of too high viscosity or too large film impedance, the low-temperature discharge performance and cycle performance of the secondary battery are reduced. And some additives with lower film impedance often increase the high-temperature impedance growth rate of secondary batteries. Therefore, it is urgent to develop an electrolyte that can effectively improve the high-temperature impedance growth rate and cycle performance of secondary batteries. Summary of the invention
[0003] The purpose of this application is to provide a non-aqueous electrolyte for a secondary battery, a secondary battery and an electronic device to improve the cycle performance and high-temperature storage performance of the secondary battery. The specific technical solution is as follows:
[0004] It should be noted that in the invention content of the present application, a lithium-ion battery is used as an example of a secondary battery to explain the present application, but the secondary battery of the present application is not limited to a lithium-ion battery.
[0005] The first aspect of the present application provides a non-aqueous electrolyte for a secondary battery, which comprises a compound of formula I:
[0006]
[0007] Among them, A 1 Independently selected from cyano or Represents the binding site with the adjacent atom, R 1 is selected from a hydrogen atom, a C1 to C5 alkyl group, a C1 to C5 alkyl group substituted with a cyano group, a C1 to C5 alkyl group substituted with a fluorine group, a C1 to C5 alkoxy group, or a C1 to C5 alkoxy group substituted with a fluorine group; wherein the substitution may be full substitution or partial substitution; based on the total mass of the non-aqueous electrolyte for a secondary battery, the mass percentage of the compound of formula I is W I The compound of formula I can increase the stability of the positive electrode interface and the negative electrode interface, reduce the continuous decomposition of the electrolyte, and thus improve the cycle performance and high temperature storage performance of the lithium ion battery.
[0008] In one embodiment of the present application, the compound of formula I includes at least one of the following compounds:
[0009]
[0010] In one embodiment of the present application, the non-aqueous electrolyte for secondary batteries further comprises a compound of formula II:
[0011]
[0012] Wherein n is an integer selected from 0 to 4. When n=0, the fragment is regarded as a covalent single bond. 23 and R 24 Connected; A 2 Selected from R 21 , R 22 , R 23 , R 24 independently selected from a covalent single bond, a C1 to C5 alkylene group, a C2 to C4 alkenylene group or R 25 Selected from hydrogen, cyano, C 1 To C 3 or a C1 to C3 alkyl group substituted with a cyano group; R 26 , R 27 are independently selected from a covalent single bond or C 1 To C 3 Alkylene; substitution may be full substitution or partial substitution; based on the total mass of the non-aqueous electrolyte for secondary batteries, the mass percentage content of the compound of formula II W II The compound of formula II can form a synergistic effect with the compound of formula I in the electrolyte, which can play a stronger protective role on the positive electrode interface and the negative electrode interface, further reduce the decomposition of the electrolyte, and thus further improve the cycle performance of the secondary battery.
[0013] In one embodiment of the present application, the compound of formula II includes at least one of the following compounds:
[0014]
[0015]
[0016] In one embodiment of the present application, the ratio of the mass percentage of the compound of formula I to the mass percentage of the compound of formula II is W I / W II W is 0.016 to 5, preferably 0.016 to 0.5. I / W IIWhen within the above range, it is beneficial for the compound of formula II to form a synergistic effect with the compound of formula I in the electrolyte, which can provide a stronger protective effect on the positive electrode interface and the negative electrode interface, further inhibit the decomposition of the electrolyte, and at the same time make the viscosity of the electrolyte moderate, thereby further improving the cycle performance of the secondary battery.
[0017] In one embodiment of the present application, the non-aqueous electrolyte for a secondary battery includes a fluorinated compound, the fluorinated compound includes at least one of fluoroethylene carbonate, 2,2-difluoroethyl acetate, 2,2,2-trifluoroethyl acetate, 2,2-difluoroethyl propionate, 2,2,2-trifluoroethyl propionate, ethylsulfonyl fluoride, 2,2,2-trifluoroethyl methanesulfonate or 2,2,2-trifluoroethyl trifluoromethanesulfonate; based on the total mass of the non-aqueous electrolyte for a secondary battery, the mass percentage of the fluorinated compound is W F The fluorinated compound can improve the stability of the positive electrode interface, reduce the decomposition of the electrolyte, further enhance the stability of the interface, and can be used in combination with the compound of formula I to further improve the cycle performance and high temperature storage performance of the secondary battery.
[0018] In one embodiment of the present application, the mass percentage of the compound of formula I is W I Mass percentage of fluorinated compounds W F The ratio x is 0.001 to 0.2. When the value of x is within the above range, the stability of the positive electrode interface and the negative electrode interface of the secondary battery is high, which can further improve the cycle performance and high temperature storage performance of the secondary battery.
[0019] In one embodiment of the present application, the non-aqueous electrolyte for a secondary battery includes a compound of formula III:
[0020]
[0021] Among them, A 31 and A 32 Each independently selected Represents the binding site with the adjacent atom, m is selected from 0 or 1. When m = 0, the fragment is regarded as a covalent single bond, R 31 and R 32 Connected; R 31 , R 32 Each is independently selected from a covalent single bond, a substituted or unsubstituted C1 to C5 alkylene, a substituted or unsubstituted C2 to C5 alkenylene, when substituted, the substituent is a F atom, and the substitution may be full substitution or partial substitution. Based on the total mass of the non-aqueous electrolyte for secondary batteries, the mass percentage of the compound of formula III is 0.08% to 5%. The compound of formula III can improve the stability of the positive electrode interface, reduce the decomposition of the electrolyte, and further improve the cycle performance of the secondary battery.
[0022] In one embodiment of the present application, the compound of formula III includes at least one of the following compounds:
[0023]
[0024] In one embodiment of the present application, the non-aqueous electrolyte for secondary batteries further comprises a compound of formula IV:
[0025]
[0026] Among them, R 41 The compound of formula IV is selected from substituted C1 to C6 alkylene, substituted or unsubstituted C2 to C6 alkenylene, and when substituted, the substituent is selected from C2 to C6 alkenyl; the substitution may be full substitution or partial substitution; based on the total mass of the non-aqueous electrolyte for secondary batteries, the mass percentage of the compound of formula IV is 0.1% to 2%. The compound of formula IV can assist in enhancing the film formation stability of the solid electrolyte interface film (SEI film), reduce the decomposition of the SEI film during the charge and discharge process, reduce the impedance generated by the accumulation of byproducts during the cycle, and improve the cycle performance of the secondary battery.
[0027] In one embodiment of the present application, the compound of formula IV includes at least one of the following compounds:
[0028]
[0029] In one embodiment of the present application, the non-aqueous electrolyte for secondary batteries further comprises a boron lithium salt, which comprises at least one of lithium tetrafluoroborate, lithium dioxalate borate or lithium difluorooxalate borate; based on the total mass of the non-aqueous electrolyte for secondary batteries, the mass percentage of the boron lithium salt is 0.01% to 1%. The boron lithium salt can form a film on the positive electrode interface, protect the positive electrode interface, and produce a synergistic effect with the compound of formula I, which can further improve the cycle performance of the secondary battery.
[0030] The second aspect of the present application provides a secondary battery, which includes a positive electrode plate, a separator, a negative electrode plate and the non-aqueous electrolyte for the secondary battery provided in the first aspect of the present application.
[0031] A third aspect of the present application provides an electronic device, wherein the electronic device includes the secondary battery provided by the second aspect of the present application.
[0032] Beneficial effects of this application:
[0033] The present application provides a non-aqueous electrolyte for a secondary battery, a secondary battery and an electronic device. The secondary battery comprises a positive electrode sheet, a negative electrode sheet and a non-aqueous electrolyte for a secondary battery, wherein the non-aqueous electrolyte for a secondary battery contains a compound of formula I, the compound of formula I can be reduced at the negative electrode to form an interface protection layer, and in addition, the nitrogen atom in the compound of formula I can stabilize the high-valent transition metal, and these two properties jointly stabilize the positive and negative electrode interfaces, inhibit the continuous decomposition of the electrolyte, thereby improving the cycle performance and high-temperature storage performance of the lithium-ion battery. DETAILED DESCRIPTION
[0034] The technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by those skilled in the art based on the present application belong to the scope of protection of the present application.
[0035] It should be noted that in the specific implementation manner of the present application, the present application is explained by taking a lithium-ion battery as an example of a secondary battery, but the secondary battery of the present application is not limited to a lithium-ion battery.
[0036] The first aspect of the present application provides a non-aqueous electrolyte for a secondary battery, which comprises a compound of formula I:
[0037]
[0038] Among them, A 1 Independently selected from cyano or Represents the binding site with the adjacent atom, R 1 is selected from a hydrogen atom, a C1 to C5 alkyl group, a C1 to C5 alkyl group substituted with a cyano group, a C1 to C5 alkyl group substituted with a fluorine group, a C1 to C5 alkoxy group, or a C1 to C5 alkoxy group substituted with a fluorine group; the substitution may be full substitution or partial substitution; based on the total mass of the non-aqueous electrolyte for a secondary battery, the mass percentage of the compound of formula I is W I0.08% to 1%. For example, the mass percentage of the compound of formula I can be 0.08%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1% or a range consisting of any two of the values. When the mass percentage of the compound of formula I is too high, for example, higher than the upper limit of the present application, the cycle performance of the secondary battery is not significantly improved, but the electrolyte viscosity is too large, so that the dynamic performance of the secondary battery decreases; when the mass percentage of the compound of formula I is too low, for example, lower than the lower limit of the present application, the effect of improving the cycle performance of the secondary battery is relatively limited. Without being limited to any theory, the inventors of the present application have found that when the mass percentage of the compound of formula I is within the above range, the compound of formula I can be reduced at the negative electrode to form an interface protection layer. In addition, the nitrogen atoms in the compound of formula I can stabilize high-valent transition metals. These two properties jointly stabilize the positive electrode interface and the negative electrode interface, and can reduce the continuous decomposition of the electrolyte, thereby improving the cycle performance and high-temperature storage performance of the lithium-ion battery.
[0039] In one embodiment of the present application, the compound of formula I includes at least one of the following compounds:
[0040]
[0041] When the compound of formula I is selected from the compounds within the above range, the compound of formula I can be reduced at the negative electrode to form an interface protection layer. In addition, the nitrogen atom in the compound of formula I can stabilize the high-valent transition metal. These two properties jointly stabilize the positive electrode interface and the negative electrode interface, inhibit the continuous decomposition of the electrolyte, thereby improving the cycle performance and high-temperature storage performance of the lithium-ion battery.
[0042] In one embodiment of the present application, the non-aqueous electrolyte for secondary batteries further comprises a compound of formula II:
[0043]
[0044] Wherein n is an integer selected from 0 to 4. When n=0, the fragment is regarded as a covalent single bond. 23 and R 24 Connected; A 2 Selected from R 21 , R 22 , R 23 , R 24 are independently selected from a covalent single bond, C 1 To C 5 Alkylene, C 2 To C 4 Alkenylene or R 25 Selected from hydrogen, cyano, C 1 To C3 Alkyl or cyano-substituted C 1 To C 3 Alkyl; R 26 , R 27 are independently selected from a covalent single bond or C 1 To C 3 Alkylene; substitution may be full substitution or partial substitution; based on the total mass of the non-aqueous electrolyte for secondary batteries, the mass percentage content of the compound of formula II W II The mass percentage of the compound of formula II can be 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, or a range consisting of any two of the values. By regulating the mass percentage of the compound of formula II within the above range, it is beneficial for the compound of formula II to form a synergistic effect with the compound of formula I in the electrolyte, which can provide a stronger protective effect on the positive electrode interface and the negative electrode interface, further reduce the decomposition of the electrolyte, and make the viscosity of the electrolyte moderate, thereby further improving the cycle performance of the secondary battery.
[0045] In one embodiment of the present application, the compound of formula II includes at least one of the following compounds:
[0046]
[0047]
[0048] When the compound of formula II is selected from the compounds within the above range, the compound of formula II can form a synergistic effect with the compound of formula I in the electrolyte, can provide stronger protection for the positive electrode interface and the negative electrode interface, further inhibit the decomposition of the electrolyte, and thus further improve the cycle performance of the secondary battery.
[0049] In one embodiment of the present application, the ratio of the mass percentage of the compound of formula I to the mass percentage of the compound of formula II is W I / W II is 0.016 to 5, preferably 0.016 to 0.5. For example, the mass percentage content W of the compound of formula I I Mass percentage of fluorinated compounds W F The ratio x can be 0.016, 0.05, 0.1, 0.5, 1, 2, 3, 4, 5 or a range consisting of any two of these values. I / W IIWithin the above range, it is beneficial for the compound of formula II to form a synergistic effect with the compound of formula I in the electrolyte, which can provide a stronger protective effect on the positive electrode interface and the negative electrode interface, further inhibit the decomposition of the electrolyte, and at the same time make the viscosity of the electrolyte moderate, thereby further improving the cycle performance of the secondary battery.
[0050] In one embodiment of the present application, the non-aqueous electrolyte for a secondary battery includes a fluorinated compound, the fluorinated compound includes at least one of fluoroethylene carbonate (FEC), 2,2-difluoroethyl acetate (DFEA), 2,2,2-trifluoroethyl acetate, 2,2-difluoroethyl propionate, 2,2,2-trifluoroethyl propionate, ethyl sulfonyl fluoride, 2,2,2-trifluoroethyl methanesulfonate or 2,2,2-trifluoroethyl trifluoromethanesulfonate; based on the total mass of the non-aqueous electrolyte for a secondary battery, the mass percentage of the fluorinated compound W F For example, the mass percentage of the fluorinated compound W F It can be 5%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 71% or a range consisting of any two of these values. By regulating the content of the fluorinated compound within the above range, the stability of the positive electrode interface can be improved due to the strong antioxidant capacity of the fluorinated compound. On the other hand, the fluorinated compound can be reduced on the surface of the negative electrode to form a protective film, reduce the decomposition of the electrolyte, and further enhance the stability of the interface. Therefore, the fluorinated compound is used in combination with the compound of formula I to further improve the cycle performance and high temperature storage performance of the secondary battery.
[0051] In one embodiment of the present application, the mass percentage of the compound of formula I is W I Mass percentage of fluorinated compounds W F The ratio x is 0.001 to 0.2. For example, the mass percentage content W of the compound of formula I I Mass percentage of fluorinated compounds W F The ratio x can be 0.001, 0.005, 0.01, 0.05, 0.1, 0.15, 0.2 or a range composed of any two of the numerical values. The fluorinated compound has a strong antioxidant capacity and can improve the stability of the positive electrode interface. On the other hand, the fluorinated compound can be reduced on the negative electrode surface to form a protective film, reduce the decomposition of the electrolyte, and further enhance the stability of the positive electrode interface and the negative electrode interface. Therefore, the fluorinated compound is used in combination with the compound of formula I to further improve the cycle performance and high temperature storage performance of the secondary battery.
[0052] In one embodiment of the present application, the non-aqueous electrolyte for a secondary battery includes a compound of formula III:
[0053]
[0054] Among them, A 31 and A 32 Each independently selected Represents the binding site with the adjacent atom, m is selected from 0 or 1. When m = 0, the fragment is regarded as a covalent single bond, R 31 and R 32 Connected; R 31 , R 32 Each independently selected from a covalent single bond, a substituted or unsubstituted C1 to C5 alkylene, a substituted or unsubstituted C2 to C5 alkenylene, when substituted, the substituent is a F atom, and the substitution may be total or partial substitution. Based on the total mass of the non-aqueous electrolyte for secondary batteries, the mass percentage of the compound of formula III is 0.08% to 5%. For example, the mass percentage of the compound of formula III may be 0.08%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5% or a range consisting of any two of the values. When the mass percentage of the compound of formula III is within the above range, due to the strong antioxidant capacity of the compound of formula III, the stability of the positive electrode interface can be improved. On the other hand, the compound of formula III can be reduced on the surface of the negative electrode to form a protective film, reduce the decomposition of the electrolyte, and further enhance the stability of the interface. Thus, the combined use of the compound of formula III can further improve the cycle performance of the secondary battery.
[0055] In one embodiment of the present application, the compound of formula III includes at least one of the following compounds:
[0056]
[0057] Without being limited to any theory, the inventors of the present application have found that when the compound of formula III is selected from the compounds within the above range, the stability of the positive electrode interface can be improved due to the strong antioxidant ability of the compound of formula III. On the other hand, the compound of formula III can be reduced on the surface of the negative electrode to form a protective film, inhibiting the decomposition of the electrolyte and further enhancing the stability of the interface. Thus, the combined use of the compound of formula III can further improve the cycle performance of the secondary battery.
[0058] In one embodiment of the present application, the non-aqueous electrolyte for secondary batteries further comprises a compound of formula IV:
[0059]
[0060] Among them, R 41Selected from substituted C1 to C6 alkylene, substituted or unsubstituted C2 to C6 alkenylene, when substituted, the substituent is selected from C2 to C6 alkenyl; based on the total mass of the non-aqueous electrolyte for secondary batteries, the mass percentage of the compound of formula IV is 0.1% to 2%. For example, the mass percentage of the compound of formula IV can be 0.1%, 0.3%, 0.5%, 0.7%, 9%, 1.1%, 1.3%, 1.5%, 1.7%, 1.9%, 2% or a range consisting of any two of the values. When the mass percentage of the compound of formula IV is within the above range, the compound of formula IV can assist in enhancing the film formation stability of the solid electrolyte interface film (SEI film), reduce the decomposition of the SEI film during the charge and discharge process, further enhance the protective effect on the positive electrode interface and the negative electrode interface, reduce the interface contact probability between the active material and the electrolyte, reduce the side reaction between the electrolyte and the active material, thereby reducing the impedance generated by the accumulation of by-products during the cycle, and improving the cycle performance of the secondary battery.
[0061] In one embodiment of the present application, the compound of formula IV includes at least one of the following compounds:
[0062]
[0063] When the compound of formula IV is selected from the compounds within the above range, the compound of formula IV can assist in enhancing the film formation stability of the solid electrolyte interface film (SEI film), reduce the decomposition of the SEI film during the charge and discharge process, further enhance the protective effect on the positive electrode interface and the negative electrode interface, reduce the interface contact probability between the active material and the electrolyte, reduce the side reaction between the electrolyte and the active material, thereby reducing the impedance generated by the accumulation of by-products during the cycle process, and improving the cycle performance of the secondary battery.
[0064] In one embodiment of the present application, the non-aqueous electrolyte for secondary batteries also includes a boron lithium salt, and the boron lithium salt includes at least one of lithium tetrafluoroborate, lithium dioxalate borate (LiBOB) or lithium difluorooxalate borate; based on the total mass of the non-aqueous electrolyte for secondary batteries, the mass percentage of the boron lithium salt is 0.01% to 1%. For example, the mass percentage of the boron lithium salt can be 0.01%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1% or a range consisting of any two of the values. When the mass percentage of the boron lithium salt is within the above range, the boron lithium salt can form a film at the positive electrode interface, protect the positive electrode interface, and produce a synergistic effect with the compound of formula I, which can further improve the cycle performance of the secondary battery.
[0065] In one embodiment of the present application, the non-aqueous electrolyte for a secondary battery further includes a lithium salt and a non-aqueous solvent.
[0066] The present application has no special restrictions on lithium salts, as long as the purpose of the present application can be achieved. For example, lithium salts may include but are not limited to at least one of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, Li2SiF6, lithium bis(oxalateborate) (LiBOB) or lithium difluoroborate. The present application has no special restrictions on the content of lithium salts in the electrolyte, as long as the purpose of the present application can be achieved. For example, based on the mass of the non-aqueous electrolyte for secondary batteries, the mass percentage of lithium salts is 8% to 15%.
[0067] The present application has no particular limitation on the non-aqueous solvent as long as the purpose of the present application can be achieved. For example, the non-aqueous solvent may include but is not limited to at least one of carbonate compounds, carboxylate compounds, ether compounds or other organic solvents.
[0068] The carbonate compound may include but is not limited to at least one of a linear carbonate compound, a cyclic carbonate compound or a fluorinated carbonate compound. The linear carbonate compound may include but is not limited to at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC) or methyl ethyl carbonate (MEC). The cyclic carbonate may include but is not limited to at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC) or vinyl ethylene carbonate (VEC). The fluorinated carbonate compound may include, but is not limited to, at least one of fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, or trifluoromethylethylene carbonate. The above-mentioned carboxylate compound may include, but is not limited to, at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decalactone, valerolactone, or caprolactone. The above-mentioned ether compound may include but is not limited to at least one of dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran. The above-mentioned other organic solvents may include but are not limited to at least one of dimethyl sulfoxide, 1,2-dioxolane, cyclopentane, methyl cyclopentane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate or trioctyl phosphate. The present application does not particularly limit the content of the non-aqueous solvent in the non-aqueous electrolyte for secondary batteries, as long as the purpose of the present application can be achieved.
[0069] The present application has no particular limitation on the content of the non-aqueous solvent in the electrolyte, as long as the purpose of the present application can be achieved. For example, based on the mass of the non-aqueous electrolyte for secondary batteries, the mass percentage of the non-aqueous solvent is 0% to 91.92%.
[0070] In one embodiment of the present application, the electrolyte may include a compound of formula I, a lithium salt and a non-aqueous solvent, the mass percentage of the compound of formula I and the lithium salt is as described above, and the mass percentage of the non-aqueous solvent is 84% to 91.92%. The secondary battery including the above electrolyte has good cycle performance and high temperature storage performance.
[0071] In one embodiment of the present application, the electrolyte may include a compound of formula I, a compound of formula II, a fluorinated compound, a lithium salt and a non-aqueous solvent, the mass percentage of the compound of formula I, the compound of formula II, the fluorinated compound and the lithium salt is as described above, and the mass percentage of the non-aqueous solvent is 8% to 86.82%. The secondary battery including the above electrolyte has good cycle performance and high temperature storage performance.
[0072] In one embodiment of the present application, the electrolyte may include a compound of formula I, a compound of formula II, a fluorinated compound, a compound of formula III, a lithium salt and a non-aqueous solvent, the mass percentage of the compound of formula I, the compound of formula II, the fluorinated compound, the compound of formula III and the lithium salt is as described above, and the mass percentage of the non-aqueous solvent is 3% to 86.74%. The secondary battery including the above electrolyte has good cycle performance and high temperature storage performance.
[0073] In one embodiment of the present application, the electrolyte may include a compound of formula I, a compound of formula II, a fluorinated compound, a compound of formula III, a compound of formula IV, a lithium salt and a non-aqueous solvent, wherein the mass percentage of the compound of formula I, the compound of formula II, the fluorinated compound, the compound of formula III, the compound of formula IV and the lithium salt is as described above, and the mass percentage of the non-aqueous solvent is 1% to 86.64%. The secondary battery including the above electrolyte has good cycle performance and high temperature storage performance.
[0074] In one embodiment of the present application, the electrolyte may include a compound of formula I, a compound of formula II, a fluorinated compound, a compound of formula III, a compound of formula IV, a boron lithium salt, a lithium salt, and a non-aqueous solvent, wherein the mass percentage of the compound of formula I, the compound of formula II, the fluorinated compound, the compound of formula III, the compound of formula IV, the boron lithium salt, and the lithium salt is as described above, and the mass percentage of the non-aqueous solvent is 0% to 86.63%. The secondary battery including the above electrolyte has good cycle performance and high temperature storage performance.
[0075] In one embodiment of the present application, the electrolyte may include a compound of formula I, a fluorinated compound, a lithium salt and a non-aqueous solvent, the mass percentage of the compound of formula I, the fluorinated compound and the lithium salt is as described above, and the mass percentage of the non-aqueous solvent is 26% to 86.92%. The secondary battery including the above electrolyte has good cycle performance and high temperature storage performance.
[0076] In one embodiment of the present application, the electrolyte may include a compound of formula I, a lithium salt, a non-aqueous solvent, and one of the compounds of formula II or formula III, wherein the mass percentage of the compound of formula I, the lithium salt, and one of the compounds of formula II or formula III is as described above, and the mass percentage of the non-aqueous solvent is 79% to 91.84%. The secondary battery including the above electrolyte has good cycle performance and high temperature storage performance.
[0077] In one embodiment of the present application, the electrolyte may include a compound of formula I, a compound of formula II, a compound of formula III, a lithium salt and a non-aqueous solvent, the mass percentage of the compound of formula I, the compound of formula II, the compound of formula III and the lithium salt is as described above, and the mass percentage of the non-aqueous solvent is 74% to 91.74%. The secondary battery including the above electrolyte has good cycle performance and high temperature storage performance.
[0078] In one embodiment of the present application, the electrolyte may include a compound of formula I, a lithium salt, a non-aqueous solvent, and one of a compound of formula IV or a boron lithium salt, the mass percentage of the compound of formula I, the lithium salt, and one of the compound of formula II or the compound of formula III is as described above, and the mass percentage of the non-aqueous solvent is 82% to 91.91%. The secondary battery including the above electrolyte has good cycle performance and high temperature storage performance.
[0079] In one embodiment of the present application, the electrolyte may include a compound of formula I, a boron lithium salt, a compound of formula IV, a lithium salt and a non-aqueous solvent, the mass percentage of the compound of formula I, the boron lithium salt, the compound of formula IV and the lithium salt is as described above, and the mass percentage of the non-aqueous solvent is 81% to 91.81%. The secondary battery including the above electrolyte has good cycle performance and high temperature storage performance.
[0080] In one embodiment of the present application, the electrolyte may include a compound of formula I, a lithium salt, a non-aqueous solvent, one of the compounds of formula II or formula III, and one of the compounds of formula IV or boron lithium salt, the mass percentage of the compound of formula I, the lithium salt, one of the compounds of formula II or formula III, and one of the compounds of formula IV or boron lithium salt is as described above, and the mass percentage of the non-aqueous solvent is 77% to 91.83%. The secondary battery including the above electrolyte has good cycle performance and high temperature storage performance.
[0081] In one embodiment of the present application, the electrolyte may include a compound of formula I, a lithium salt, a fluorinated compound, a non-aqueous solvent, and one of the compounds of formula II or formula III, the mass percentage of the compound of formula I, the lithium salt, and one of the compounds of formula II or formula III is as described above, and the mass percentage of the non-aqueous solvent is 8% to 86.84%. The secondary battery including the above electrolyte has good cycle performance and high temperature storage performance.
[0082] In one embodiment of the present application, the electrolyte may include a compound of formula I, a lithium salt, a fluorinated compound, a non-aqueous solvent, and one of a compound of formula IV or a boron lithium salt, the mass percentage of the compound of formula I, the lithium salt, the fluorinated compound, the fluorinated compound, and one of the compound of formula II or the compound of formula III is as described above, and the mass percentage of the non-aqueous solvent is 11% to 86.91%. The secondary battery including the above electrolyte has good cycle performance and high temperature storage performance.
[0083] In one embodiment of the present application, the electrolyte may include a compound of formula I, a compound of formula II, a compound of formula III, a lithium salt, a non-aqueous solvent, and one of a compound of formula IV or a boron lithium salt, wherein the mass percentage of the compound of formula I, the compound of formula II, the compound of formula III, the lithium salt, and one of the compound of formula IV or a boron lithium salt is as described above, and the mass percentage of the non-aqueous solvent is 72% to 91.81%. The secondary battery including the above electrolyte has good cycle performance and high temperature storage performance.
[0084] In one embodiment of the present application, the electrolyte may include a compound of formula I, a compound of formula II, a compound of formula III, a fluorinated compound, a lithium salt, and a non-aqueous solvent, wherein the mass percentage of the compound of formula I, the compound of formula II, the compound of formula III, the fluorinated compound, and the lithium salt is as described above, and the mass percentage of the non-aqueous solvent is 3% to 86.74%. The secondary battery including the above electrolyte has good cycle performance and high temperature storage performance.
[0085] In one embodiment of the present application, the electrolyte may include a compound of formula I, a compound of formula IV, a boron lithium salt, a fluorinated compound, a lithium salt, and a non-aqueous solvent, wherein the mass percentage of the compound of formula I, the compound of formula IV, the boron lithium salt, the fluorinated compound, and the lithium salt is as described above, and the mass percentage of the non-aqueous solvent is 59% to 91.64%. The secondary battery including the above electrolyte has good cycle performance and high temperature storage performance.
[0086] In one embodiment of the present application, the electrolyte may include one of the compounds of formula I, formula IV, boron lithium salt, formula II or formula III, lithium salt and non-aqueous solvent, the mass percentage of the compounds of formula I, formula IV, boron lithium salt, formula II or formula III and lithium salt is as described above, and the mass percentage of the non-aqueous solvent is 76% to 91.73%. The secondary battery including the above electrolyte has good cycle performance and high temperature storage performance.
[0087] In one embodiment of the present application, the electrolyte may include one of the compounds of formula I, fluorinated compounds, lithium salts, non-aqueous solvents, compounds of formula II or compounds of formula III, and one of the compounds of formula IV or boron lithium salts, the mass percentage of the compounds of formula I, fluorinated compounds, lithium salts, compounds of formula II or compounds of formula III, and one of the compounds of formula IV or boron lithium salts is as described above, and the mass percentage of the non-aqueous solvent is 6% to 86.83%. The secondary battery including the above electrolyte has good cycle performance and high temperature storage performance.
[0088] In one embodiment of the present application, the electrolyte may include one of the compounds of formula I, II, III, fluorinated compounds, lithium salts, non-aqueous solvents, and compounds of formula IV or boron lithium salts, the mass percentage of one of the compounds of formula I, II, III, fluorinated compounds, lithium salts, and compounds of formula IV or boron lithium salts is as described above, and the mass percentage of the non-aqueous solvent is 1% to 86.73%. The secondary battery including the above electrolyte has good cycle performance and high temperature storage performance.
[0089] In one embodiment of the present application, the electrolyte may include one of the compounds of formula I, formula IV, boron lithium salt, fluorinated compound, one of the compounds of formula II or formula III, lithium salt and non-aqueous solvent, the mass percentage of the compounds of formula I, formula IV, boron lithium salt, fluorinated compound, one of the compounds of formula II or formula III and lithium salt is as described above, and the mass percentage of the non-aqueous solvent is 5% to 86.73%. The secondary battery including the above electrolyte has good cycle performance and high temperature storage performance.
[0090] The second aspect of the present application provides a secondary battery, which includes a positive electrode plate, a separator, a negative electrode plate and the non-aqueous electrolyte for the secondary battery provided in the first aspect of the present application.
[0091] In one embodiment of the present application, the positive electrode plate includes a positive current collector and a positive electrode material layer disposed on at least one surface of the positive current collector. The above-mentioned "positive electrode material layer disposed on at least one surface of the positive current collector" means that the positive electrode material layer can be disposed on one surface of the positive current collector along its own thickness direction, or it can be disposed on two surfaces of the positive current collector along its own thickness direction. It should be noted that the "surface" here can be the entire area of the surface of the positive current collector, or it can be a partial area of the surface of the positive current collector. This application has no special restrictions, as long as the purpose of this application can be achieved. This application has no special restrictions on the positive current collector, as long as the purpose of this application can be achieved. For example, it can include aluminum foil, aluminum alloy foil or a composite current collector (such as an aluminum-carbon composite current collector). The positive electrode material layer includes a positive electrode active material. The present application has no particular limitation on the positive electrode active material as long as the purpose of the present application can be achieved. For example, the positive electrode active material may include but is not limited to lithium nickel cobalt manganese oxide (such as NCM811, NCM622, NCM523, NCM111), lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich manganese-based materials, lithium cobalt oxide (LiCoO2), lithium manganese oxide, lithium iron manganese phosphate or at least one of lithium titanate.
[0092] The positive electrode material layer may also include a conductive agent and a binder. The present application does not particularly limit the types of the conductive agent and the binder, as long as the purpose of the present application can be achieved. For example, it may be at least one of the above conductive agent and the above binder. The present application does not particularly limit the mass ratio of the positive electrode active material, the conductive agent, and the binder in the positive electrode material layer. Those skilled in the art can select according to actual needs, as long as the purpose of the present application can be achieved.
[0093] The present application has no particular limitation on the thickness of the positive electrode current collector and the positive electrode material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the positive electrode current collector is 5 μm to 20 μm, and the thickness of the positive electrode material layer is 30 μm to 120 μm.
[0094] Optionally, the positive electrode sheet may further include a conductive layer, which is located between the positive electrode current collector and the positive electrode material layer. The composition of the conductive layer is not particularly limited, and it can be a conductive layer commonly used in the art. The conductive layer includes a conductive agent and a binder. The present application has no particular restrictions on the conductive agent and the binder in the conductive layer, for example, it can be at least one of the above conductive agent and the above binder.
[0095] In one embodiment of the present application, the secondary battery further includes a negative electrode plate, and the negative electrode plate includes a negative electrode current collector and a negative electrode material layer disposed on at least one surface of the negative electrode current collector. The above-mentioned "negative electrode material layer is disposed on at least one surface of the negative electrode current collector" means that the negative electrode material layer can be disposed on one surface of the negative electrode current collector along its own thickness direction, or it can be disposed on two surfaces of the negative electrode current collector along its own thickness direction. It should be noted that the "surface" here can be the entire area of the surface of the negative electrode current collector, or it can be a partial area of the surface of the negative electrode current collector. This application is not particularly limited, as long as the purpose of this application can be achieved.
[0096] The present application has no particular limitation on the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, it may include copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, foam nickel, foam copper or a composite current collector. For example, the composite current collector may be a lithium-copper composite current collector, a carbon-copper composite current collector, a nickel-copper composite current collector, a titanium-copper composite current collector, etc.
[0097] The negative electrode material layer includes a negative electrode active material. The present application has no particular limitation on the negative electrode active material as long as the purpose of the present application can be achieved. For example, the negative electrode active material may include but is not limited to natural graphite, artificial graphite, mesophase microcarbon beads, hard carbon, soft carbon, silicon, silicon-carbon composite, Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel structured lithiated TiO2-Li4Ti5O 12 Or at least one of Li-Al alloy.
[0098] In one embodiment of the present application, the negative electrode material layer may also include a conductive agent and a binder. The present application does not particularly limit the types of conductive agents and binders, as long as the purpose of the present application can be achieved. For example, the conductive agent may include but is not limited to at least one of conductive carbon black (Super-P), carbon nanotubes (CNTs), carbon fibers, flake graphite, graphene, metal materials or conductive polymers, and the conductive carbon black may include but is not limited to at least one of acetylene black or Ketjen black. The above-mentioned carbon nanotubes may include but are not limited to single-walled carbon nanotubes and / or multi-walled carbon nanotubes. The above-mentioned carbon fibers may include but are not limited to vapor-grown carbon fibers (VGCF) and / or nano-carbon fibers. The above-mentioned metal materials may include but are not limited to metal powders and / or metal fibers, and specifically, the metal may include but is not limited to at least one of copper, nickel, aluminum or silver. The above-mentioned conductive polymers may include but are not limited to at least one of polyphenylene derivatives, polyaniline, polythiophene, polyacetylene or polypyrrole. For example, the binder may include, but is not limited to, at least one of polyacrylic acid, sodium polyacrylate, potassium polyacrylate, lithium polyacrylate, polyimide, polyvinyl alcohol, carboxymethyl cellulose, sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, polyimide, polyamide-imide, styrene-butadiene rubber, or polyvinylidene fluoride. The present application does not particularly limit the mass ratio of the negative electrode active material, the conductive agent, and the binder in the negative electrode material layer, and those skilled in the art may select according to actual needs, as long as the purpose of the present application can be achieved.
[0099] In one embodiment of the present application, the negative electrode material layer may further include a conductive agent and a binder. The present application does not particularly limit the types of the conductive agent and the binder, as long as the purpose of the present application can be achieved. For example, it may be at least one of the above conductive agent and the above binder. The present application does not particularly limit the mass ratio of the negative electrode active material, the conductive agent, and the binder in the negative electrode material layer. Those skilled in the art may select according to actual needs, as long as the purpose of the present application can be achieved.
[0100] In one embodiment of the present application, a conductive agent, a binder and a thickener may also be included. The present application has no particular restrictions on the types of conductive agents and thickeners, as long as the purpose of the present application can be achieved. For example, the conductive agent and the binder may be at least one of the above conductive agents and the above binders. The thickener may include but is not limited to at least one of sodium carboxymethyl cellulose or lithium carboxymethyl cellulose. The present application has no particular restrictions on the mass ratio of the negative electrode active material, the conductive agent, the binder and the thickener in the negative electrode material layer. Those skilled in the art can choose according to actual needs, as long as the purpose of the present application can be achieved.
[0101] The present application has no particular limitation on the thickness of the negative electrode material layer, as long as the purpose of the present application can be achieved, for example, the thickness of the negative electrode material layer is 30 μm to 120 μm. The present application has no particular limitation on the thickness of the negative electrode current collector, as long as the purpose of the present application can be achieved, for example, the thickness of the negative electrode current collector is 4 μm to 15 μm.
[0102] Optionally, the negative electrode plate may further include a conductive layer, which is located between the negative electrode current collector and the negative electrode material layer. The present application has no particular restrictions on the composition of the conductive layer, which may be a conductive layer commonly used in the art. For example, the conductive layer includes a conductive agent and a binder. The present application has no particular restrictions on the conductive agent and the binder in the conductive layer, which may be, for example, at least one of the above conductive agent and the above binder.
[0103] In one embodiment of the present application, the secondary battery further includes a separator. The present application has no particular restrictions on the separator, as long as the purpose of the present application can be achieved. For example, the material of the separator may include, but is not limited to, polyethylene (PE), polypropylene (PP)-based polyolefins (PO), polyesters (e.g., polyethylene terephthalate (PET) films), cellulose, polyimide (PI), polyamide (PA), spandex or aramid. The type of separator may include at least one of a woven membrane, a non-woven membrane, a microporous membrane, a composite membrane, a rolled membrane or a spun membrane.
[0104] In some embodiments of the present application, the isolation film may include a substrate layer and a surface treatment layer. The substrate layer may be a nonwoven fabric, a film or a composite film having a porous structure, and the material of the substrate layer may include at least one of polyethylene, polypropylene, polyethylene terephthalate or polyimide. Optionally, a polypropylene porous film, a polyethylene porous film, a polypropylene nonwoven fabric, a polyethylene nonwoven fabric or a polypropylene-polyethylene-polypropylene porous composite film may be used.
[0105] Optionally, a surface treatment layer is disposed on at least one surface of the substrate layer. The surface treatment layer may be a polymer layer or an inorganic layer, or a layer formed by mixing a polymer and an inorganic layer.
[0106] In one embodiment of the present application, the inorganic layer includes inorganic particles and a binder. The present application is not particularly limited to inorganic particles, such as inorganic particles can include at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide or barium sulfate. The present application is not particularly limited to binders, such as binders can be at least one of the above-mentioned binders. In some embodiments of the present application, the polymer layer includes polymers, and the material of the polymer includes at least one of polyamide, polyacrylonitrile, acrylate polymers, polyacrylic acid, polyacrylates, polyvinyl pyrrolidone, polyvinyl ether or polyvinylidene fluoride or poly (vinylidene fluoride-hexafluoropropylene).
[0107] In one embodiment of the present application, the thickness of the isolation film is not particularly limited as long as the purpose of the present application can be achieved. For example, the thickness of the isolation film may be 3 μm to 30 μm.
[0108] The secondary battery also includes a shell for accommodating a positive electrode plate, a separator, a negative electrode plate and an electrolyte, as well as other components known in the field of secondary batteries, and this application does not limit the above-mentioned other components. This application does not particularly limit the shell, and it can be a shell known in the art, as long as the purpose of this application can be achieved. For example, the shell can be a hard shell or a flexible shell. The material of the hard shell can be metal, and this application does not limit the type of metal. A metal hard shell known in the art can be used, as long as the purpose of this application can be achieved. The flexible shell can be a metal plastic film, such as an aluminum plastic film, a steel plastic film, etc.
[0109] The preparation process of the secondary battery of the present application is well known to those skilled in the art, and there is no particular limitation in the present application. For example, the preparation process of the secondary battery may include but is not limited to the following steps: stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and winding, folding and other operations as needed to obtain an electrode assembly of a winding structure, placing the electrode assembly in a shell, injecting the electrolyte into the shell and sealing it to obtain a secondary battery. Alternatively, stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and then fixing the four corners of the entire laminated structure with tape to obtain an electrode assembly of a laminated structure, placing the electrode assembly in a shell, injecting the electrolyte into the shell and sealing it to obtain a secondary battery. In addition, overcurrent protection elements, guide plates, etc. may also be placed in the shell as needed to prevent the pressure inside the secondary battery from rising and overcharging and discharging.
[0110] A third aspect of the present application provides an electronic device, wherein the electronic device includes the secondary battery provided in the second aspect of the present application.
[0111] The electronic device of the present application is not particularly limited, and it can be any electronic device known in the prior art. In some embodiments, the electronic device can include but is not limited to a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD TV, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery and a lithium-ion capacitor, etc.
[0112] Example
[0113] The following examples and comparative examples are given to more specifically describe the embodiments of the present application. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.
[0114] Test methods and equipment
[0115] 45℃ Cyclic Performance Test
[0116] At 45°C, the lithium-ion battery was charged to 4.55V at 1C constant current and to 0.05C at 4.55V. It was then discharged to 3.0V at 0.5C current, and cycled for 100 and 150 cycles at 1C charge and 0.5C discharge. The discharge capacity at the third cycle was used as the benchmark, and the capacity retention rate was used as an indicator of the lithium-ion battery cycle performance.
[0117] 150-cycle capacity retention rate = discharge capacity at the 150th cycle / discharge capacity at the 3rd cycle × 100%.
[0118] High temperature storage performance test
[0119] The lithium-ion battery was charged at 25°C at a constant current of 0.5C to 4.55V, then charged at a constant voltage of 4.55V to a current of 0.05C, placed in an oven at 85°C for 4 hours, and the impedance was monitored. The impedance was tested at 1kHz before storage and after 6 hours of storage.
[0120] Storage impedance growth rate (%) = impedance after 4 h storage / impedance before storage × 100%.
[0121] Example 1-1
[0122] <Preparation of positive electrode sheet>
[0123] The positive electrode active material LiCoO2, the conductive agent conductive carbon black, and the binder polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 97.9:0.9:1.2, and N-methylpyrrolidone (NMP) was added as a solvent to prepare a slurry with a solid content of 75wt%, and the positive electrode slurry was obtained after vacuum stirring. The positive electrode slurry was evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 13μm, and dried at 120℃ to obtain a positive electrode sheet with a single-sided positive electrode material layer, and the coating weight of the positive electrode material layer was 225mg / 1540mm 2 Then repeat the above steps on the other surface of the aluminum foil to obtain a positive electrode sheet with a double-sided positive electrode material layer. After drying at 120°C, cold pressing, cutting and welding the tabs, a positive electrode sheet with a specification of 74mm×867mm is obtained for standby use. Among them, the compaction density of the positive electrode sheet is 4.15g / cm 3 .
[0124] <Preparation of negative electrode sheet>
[0125] The negative electrode active material artificial graphite, the binder styrene butadiene rubber SBR, and the thickener sodium carboxymethyl cellulose CMC were mixed in a mass ratio of 97.4:1.4:1.2, and deionized water was added as a solvent to prepare a slurry with a solid content of 45wt%. The negative electrode slurry was obtained after being stirred evenly by a vacuum mixer. The negative electrode slurry was evenly coated on one surface of a negative electrode current collector copper foil with a thickness of 10μm, and dried at 120°C to obtain a negative electrode sheet with a single-sided coating of a negative electrode material layer. The coating weight of the negative electrode material layer was 130mg / 1540mm 2 Then repeat the above steps on the other surface of the copper foil to obtain a negative electrode sheet with a negative electrode material layer coated on both sides. After drying at 120°C, cold pressing, cutting and welding the tabs, a negative electrode sheet with a specification of 78mm×875mm is obtained for standby use. Among them, the compaction density of the negative electrode sheet is 1.8g / cm 3 .
[0126] <Preparation of non-aqueous electrolyte for secondary battery>
[0127] In an environment with a water content of less than 10ppm, ethylene carbonate (EC), propylene carbonate PC, and diethyl carbonate DEC are mixed uniformly in a mass ratio of 2:1:7 to obtain a non-aqueous solvent, and then lithium salt LiPF6 is added to the non-aqueous solvent, and then a compound of formula I-8 is added, and mixed uniformly to obtain a non-aqueous electrolyte for a secondary battery. Among them, based on the mass of the non-aqueous electrolyte for a secondary battery, the mass percentage of the compound of formula I-8 is 0.08%, the mass percentage of LiPF6 is 12.5%, and the rest is a non-aqueous solvent.
[0128] <Isolation film>
[0129] The base material of the isolation film is 5 μm thick polyethylene (PE), and a 2 μm thick alumina ceramic layer is coated on one side of the isolation film base material. Finally, 2.5 mg / 1540.25 mm2 of alumina is coated on both sides of the isolation film coated with a single ceramic layer. 2 The binder polyvinylidene fluoride (PVDF) was dried. The porosity of the isolation membrane was 39%.
[0130] <Preparation of lithium-ion batteries>
[0131] The positive electrode sheet, separator, and negative electrode sheet prepared above are stacked in order, so that the separator is located between the positive electrode sheet and the negative electrode sheet to play an isolating role, and the ceramic layer of the separator is facing the positive electrode sheet, and the electrode assembly is wound. The electrode assembly is placed in an aluminum-plastic film packaging bag, and the water is removed at 80°C, and the electrolyte prepared above is injected. After vacuum packaging, standing, formation, degassing, trimming and other processes, a lithium-ion battery is obtained. Among them, the formation upper limit voltage is 4.15V, the formation temperature is 70°C, and the formation standing time is 2h.
[0132] Example 1-2 to Example 1-8
[0133] Except that the type and mass percentage of the compound of formula I are adjusted in <Preparation of non-aqueous electrolyte for secondary battery>, the mass percentage of the non-aqueous solvent is changed accordingly, and the mass percentage of the lithium salt remains unchanged, the rest is the same as Example 1-1.
[0134] Example 2-1 to Example 2-12
[0135] Except for adding the compound of formula II in <Preparation of non-aqueous electrolyte for secondary battery> and adjusting the type and mass percentage of the compound of formula II, the mass percentage of the non-aqueous solvent is changed accordingly, and the mass percentage of the lithium salt remains unchanged, the rest is the same as Example 1-2.
[0136] Example 3-1 to Example 3-16
[0137] In addition to adding the compound of formula III, the compound of formula IV and the boron lithium salt in the <Preparation of non-aqueous electrolyte for secondary batteries>, and adjusting the type and mass percentage of the compound of formula III, the type and mass percentage of the compound of formula IV, the type and mass percentage of the boron lithium salt, the mass percentage of the non-aqueous solvent is changed accordingly, and the mass percentage of the lithium salt remains unchanged, the rest is the same as Example 1-2.
[0138] Example 4-1 to Example 4-11
[0139] The method is the same as Example 1-2 except that the compound of formula II, the compound of formula III, the compound of formula IV, the fluorinated compound and the boron lithium salt are added in the <Preparation of non-aqueous electrolyte for secondary batteries>, and the type and mass percentage of the compound of formula II, the type and mass percentage of the compound of formula III, the type and mass percentage of the compound of formula IV, the type and mass percentage of the fluorinated compound, and the type and mass percentage of the boron lithium salt are adjusted, the mass percentage of the non-aqueous solvent is changed accordingly, and the mass percentage of the lithium salt remains unchanged.
[0140] Comparative Example 1
[0141] Except that the compound of formula I is not added in the preparation of non-aqueous electrolyte for secondary battery, the mass percentage of non-aqueous solvent is changed accordingly, and the mass percentage of lithium salt remains unchanged, the rest is the same as Example 1-1.
[0142] Comparative Example 2
[0143] Except that an excess amount of the compound of formula I-6 is added in <Preparation of non-aqueous electrolyte for secondary battery>, the mass percentage of the non-aqueous solvent changes accordingly, and the mass percentage of the lithium salt remains unchanged, the rest is the same as Example 1-1.
[0144] Table 1
[0145]
[0146] Note: (1) The “ / ” in Table 1 indicates that there is no corresponding preparation parameter or substance. (2) Taking Example 1-8 as an example, “Type of compound of formula I” is “I-3+I-8”, and “Mass percentage of compound of formula I” is “0.1+0.2”, which means that the compound of formula I includes compound of formula I-3 and compound of formula I-8. Based on the total mass of the electrolyte, the mass percentage of compound of formula I-3 is 0.1%, and the mass percentage of compound of formula I-8 is 0.2%. The same applies to other examples.
[0147] It can be seen from Examples 1-1 to 1-8 and Comparative Examples 1 to 2 that when the type and mass percentage of the compound of formula I are within the scope of the present application, the lithium-ion battery has a higher 150-cycle capacity retention rate and a lower storage impedance growth rate, indicating that the cycle performance and high-temperature storage performance of the lithium-ion battery are improved. The type and mass percentage of the compound of formula I in Comparative Examples 1 to 2 are not within the scope of the present application, and the obtained lithium-ion battery has a low 150-cycle capacity retention rate and a high storage impedance growth rate, indicating that the lithium-ion battery has poor cycle performance and high-temperature storage performance. It can be seen from Examples 1-1 to 1-8 that the lithium-ion battery of the present application has a high 150-cycle capacity retention rate and a low storage impedance growth rate, indicating that the lithium-ion battery of the present application has good cycle performance and high-temperature storage performance.
[0148] Table 2
[0149]
[0150]
[0151] Note: (1) The “ / ” in Table 2 indicates that there is no corresponding preparation parameter or substance. (2) Taking Example 2-5 as an example, “Type of compound of formula II” is “II-1+II-3” and “Mass percentage of compound of formula II” is “1+1”, which means that the compound of formula II includes compound of formula II-1 and compound of formula II-3. Based on the total mass of the electrolyte, the mass percentage of compound of formula II-1 is 1%, and the mass percentage of compound of formula II-3 is 1%. The same applies to other examples.
[0152] The type and mass percentage of the compound of formula II usually affect the cycle performance and high temperature storage performance of the secondary battery. It can be seen from Examples 1-2 and 2-1 to 2-12 that when the type and mass percentage of the compound of formula II are within the scope of the present application, the 150 cycle capacity retention rate of the lithium ion battery is further improved, and the storage impedance growth rate is further reduced, indicating that the cycle performance and high temperature storage performance of the lithium ion battery are improved.
[0153] W I / W II The value of usually affects the cycle performance and high temperature storage performance of the secondary battery. It can be seen from Examples 1-2, 2-1 to 2-12 that when W I / W II When the value of is within the range of the present application, the 150-cycle capacity retention rate of the lithium-ion battery is further improved, and the storage impedance growth rate is further reduced, indicating that the cycle performance and high-temperature storage performance of the lithium-ion battery are improved.
[0154] Table 3
[0155]
[0156]
[0157] Note: (1) The “ / ” in Table 3 indicates that there is no corresponding preparation parameter or substance. (2) Taking Example 3-5 as an example, “Type of compound of formula III” is “III-1+III-6” and “Mass percentage of compound of formula III” is “4+1”, which means that the compound of formula III includes compound of formula III-1 and compound of formula III-6. Based on the total mass of the electrolyte, the mass percentage of compound of formula III-1 is 4%, and the mass percentage of compound of formula III-6 is 1%. The same applies to other examples.
[0158] The type and mass percentage of the compound of formula III usually affect the cycle performance and high temperature storage performance of the secondary battery. It can be seen from Examples 1-2 and 3-1 to 3-5 that when the type and mass percentage of the compound of formula III are within the scope of the present application, the 150 cycle capacity retention rate of the lithium ion battery is further improved, and the storage impedance growth rate is further reduced, indicating that the cycle performance and high temperature storage performance of the lithium ion battery are improved.
[0159] The type and mass percentage of the compound of formula IV usually affect the cycle performance and high temperature storage performance of the secondary battery. It can be seen from Examples 1-2, 3-6 to 3-9 that when the type and mass percentage of the compound of formula IV are within the scope of the present application, the 150 cycle capacity retention rate of the lithium ion battery is further improved, and the storage impedance growth rate is further reduced, indicating that the cycle performance and high temperature storage performance of the lithium ion battery are improved.
[0160] The type and mass percentage of boron lithium salts usually affect the cycle performance and high temperature storage performance of secondary batteries. It can be seen from Examples 1-2, 3-10 to 3-13 that when the type and mass percentage of boron lithium salts are within the range of this application, the 150 cycle capacity retention rate of the lithium ion battery is further improved, and the storage impedance growth rate is further reduced, indicating that the cycle performance and high temperature storage performance of the lithium ion battery are improved.
[0161] Table 4
[0162]
[0163] Note: (1) The “ / ” in Table 4 indicates that there is no corresponding preparation parameter or substance. (2) Taking Example 4-2 as an example, “Fluorinated compound type” is “FEC+DFEA”, “W F” is “10+25”, indicating that the fluorinated compound includes FEC and DFEA. Based on the total mass of the electrolyte, the mass percentage of FEC is 10%, and the mass percentage of DFEA is 25%. The same applies to other embodiments.
[0164] The type and mass percentage of the fluorinated compound usually affect the cycle performance and high-temperature storage performance of the secondary battery. It can be seen from Examples 4-1 to 4-5 that when the type and mass percentage of the fluorinated compound are within the range of this application, the 150-cycle capacity retention rate of the lithium-ion battery is further improved, and the storage impedance growth rate is further reduced, indicating that the cycle performance and high-temperature storage performance of the lithium-ion battery are improved.
[0165] Different types of electrolytes usually affect the cycle performance and high-temperature storage performance of secondary batteries. It can be seen from Examples 3-14 to 3-17 and Examples 4-6 to 4-11 that when the electrolytes combined within the scope of this application are selected, the 150-cycle capacity retention rate of the lithium-ion battery is further improved, and the storage impedance growth rate is further reduced, indicating that the cycle performance and high-temperature storage performance of the lithium-ion battery are improved.
[0166] The terms "comprises," "comprising," or any other variations thereof are intended to cover a non-exclusive inclusion such that a process, method, or article that includes a list of elements includes not only those elements but also other elements not expressly listed or that are inherent to such process, method, or article.
[0167] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.
[0168] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included in the scope of protection of the present application.
Claims
1. A non-aqueous electrolyte for a secondary battery, comprising a compound of formula I: in, A 1 Independently selected from cyano or Represents the binding site with the adjacent atom, R 1 is selected from a hydrogen atom, a C1-C5 alkyl group, a C1-C5 alkyl group substituted by a cyano group, a C1-C5 alkyl group substituted by a fluorine group, a C1-C5 alkoxy group, or a C1-C5 alkoxy group substituted by a fluorine group; Based on the total mass of the non-aqueous electrolyte for secondary batteries, the mass percentage of the compound of formula I is W I It is between 0.08% and 1%.
2. The non-aqueous electrolyte for secondary batteries according to claim 1, wherein The compound of formula I comprises at least one of the following compounds:
3. The non-aqueous electrolyte for a secondary battery according to claim 1, wherein The non-aqueous electrolyte for secondary batteries includes a compound of formula II: wherein n is selected from an integer from 0 to 4; A 2 Selected from R 21 , R 22 , R 23 , R 24 independently selected from a covalent single bond, a C1 to C5 alkylene group, a C2 to C4 alkenylene group or R 25 R is selected from a hydrogen atom, a cyano group, a C1 to C3 alkyl group, or a C1 to C3 alkyl group substituted with a cyano group; 26 , R 27 independently selected from a covalent single bond or a C1 to C3 alkylene group; Based on the total mass of the non-aqueous electrolyte for secondary batteries, the mass percentage of the compound of formula II is W II 0.1% to 5%.
4. The non-aqueous electrolyte for secondary battery according to claim 3, wherein The compound of formula II comprises at least one of the following compounds:
5. The non-aqueous electrolyte for secondary battery according to claim 3, wherein The ratio of the mass percentage of the compound of formula I to the mass percentage of the compound of formula II is W I / W II 0.016 to 5.
6. The non-aqueous electrolyte for secondary battery according to claim 5, wherein The ratio of the mass percentage of the compound of formula I to the mass percentage of the compound of formula II is W I / W II It is 0.016 to 0.
5.
7. The non-aqueous electrolyte for a secondary battery according to claim 1, wherein The non-aqueous electrolyte for a secondary battery includes a fluorinated compound, wherein the fluorinated compound includes at least one of fluoroethylene carbonate, 2,2-difluoroethyl acetate, 2,2,2-trifluoroethyl acetate, 2,2-difluoroethyl propionate, 2,2,2-trifluoroethyl propionate, ethylsulfonyl fluoride, 2,2,2-trifluoroethyl methanesulfonate, or 2,2,2-trifluoroethyl trifluoromethanesulfonate; Based on the total mass of the non-aqueous electrolyte for secondary batteries, the mass percentage of the fluorinated compound is W F 5% to 71%.
8. The non-aqueous electrolyte for a secondary battery according to claim 7, wherein The mass percentage content of the compound of formula I is W I Mass percentage of fluorinated compounds W F The ratio x is between 0.001 and 0.
2.
9. The non-aqueous electrolyte for a secondary battery according to claim 1, wherein The non-aqueous electrolyte for secondary batteries includes a compound of formula III: Among them, A 31 and A 32 Each independently selected Represents the binding site with the adjacent atom, m is selected from 0 or 1; R 31 , R 32 Each is independently selected from a covalent single bond, a substituted or unsubstituted C1 to C5 alkylene group, a substituted or unsubstituted C2 to C5 alkenylene group, and when substituted, the substituent is a fluorine atom; Based on the total mass of the non-aqueous electrolyte for a secondary battery, the mass percentage of the compound of formula III is 0.08% to 5%.
10. The non-aqueous electrolyte for secondary battery according to claim 9, wherein The compound of formula III includes at least one of the following compounds:
11. The non-aqueous electrolyte for a secondary battery according to claim 1, wherein The non-aqueous electrolyte for secondary batteries includes a compound of formula IV: Among them, R 41 is selected from substituted C1 to C6 alkylene, substituted or unsubstituted C2 to C6 alkenylene, and when substituted, the substituent is selected from C2 to C6 alkenyl; Based on the total mass of the non-aqueous electrolyte for a secondary battery, the mass percentage of the compound of formula IV is 0.1% to 2%.
12. The non-aqueous electrolyte for a secondary battery according to claim 11, wherein The compound of formula IV comprises at least one of the following compounds:
13. The non-aqueous electrolyte for a secondary battery according to claim 1, wherein Also included is a boron lithium salt, wherein the boron lithium salt includes at least one of lithium tetrafluoroborate, lithium dioxalate borate or lithium difluorooxalate borate; Based on the total mass of the non-aqueous electrolyte for a secondary battery, the mass percentage of the boron lithium salt is 0.01% to 1%. 14 . A secondary battery comprising a positive electrode sheet, a separator, a negative electrode sheet, and the non-aqueous electrolyte for a secondary battery according to claim 1 .