Method for preparing non-stoichiometric iron phosphate compound by using acidic iron-air battery and sodium ion battery positive electrode material
Preparing non-stoichiometric iron phosphate composites through acidic iron-air batteries solves the problems of high energy consumption, environmental pollution and resource waste in the preparation of iron phosphate in the existing technology, achieves efficient and low-cost preparation of iron phosphate, and improves sodium Performance and industrial feasibility of cathode materials for ion batteries.
Patent Information
- Application Number
- CN202411016392.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-27
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-27
AI Technical Summary
Existing ferric phosphate preparation methods have problems such as high energy consumption, environmental pollution, resource waste, poor product purity and consistency, high production costs, and neglect of low iron-phosphorus ratio synthesis, which limits the performance and industrial development of sodium-ion battery cathode materials.
An acidic iron-air battery is used to generate a non-stoichiometric iron phosphate complex through a redox reaction. Porous carbon electrodes and iron electrodes are used to control the pH and gas flow rate of the electrolyte and regulate the reaction conditions to prepare efficient and low-cost iron phosphate precipitation. As a precursor of cathode materials for sodium-ion batteries.
The controllability, environmental protection and cost reduction of the process are achieved, the purity and consistency of iron phosphate are improved, the electrochemical performance of the cathode material of the sodium ion battery is enhanced, and the production cost is reduced.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and specifically refers to a method for preparing a non-stoichiometric iron phosphate composite by using an acidic iron-air battery and a sodium ion battery positive electrode material. Background Art
[0002] With the transformation of the global energy structure and the advancement of sustainable development, the rapid development of new energy fields, especially electric vehicles and energy storage systems, has led to an increasing demand for high-performance battery materials. Sodium-ion batteries are regarded as an important supplement and potential substitute for lithium-ion batteries due to their abundant raw materials, low cost, and environmental friendliness, showing great potential in large-scale energy storage and low-cost application scenarios.
[0003] As an important precursor in the synthesis of positive electrode materials for sodium-ion batteries, iron phosphate's chemical composition and cost are crucial to improving battery performance and reducing production costs. However, existing methods for preparing iron phosphate include electrolysis and chemical precipitation, which mainly have the following problems: For example, energy consumption: Traditional methods of preparing iron phosphate, such as electrolysis, require a large amount of electricity, which not only increases production costs but is also not conducive to sustainable development.
[0004] Such as environmental pollution: chemical precipitation method uses and generates a large amount of chemical reagents and by-products during the preparation process, and these substances may cause environmental pollution.
[0005] Such as waste of resources: the existing technology fails to effectively utilize raw materials, resulting in a large amount of waste during the preparation process, which reduces the efficiency of resource utilization.
[0006] Such as product purity and consistency: the iron phosphate product obtained by traditional methods has low purity and poor consistency, which directly affects the performance and life of sodium-ion batteries.
[0007] For example, production costs: high equipment investment, raw material costs and post-processing costs make the existing technology for synthesizing iron phosphate economically inefficient. In addition, only pursuing the synthesis of iron phosphate with a high iron-phosphorus ratio while ignoring the synthesis of iron phosphate with a low iron-phosphorus ratio or non-stoichiometric ratio is not conducive to promoting the development of the industry and the iteration of technology.
[0008] Such as battery performance limitations: Due to insufficient purity and morphology control of iron phosphate, the performance of sodium-ion battery positive electrode materials, such as capacity, cycle stability and safety, is limited. Summary of the invention
[0009] The purpose of the present invention is to provide a method for preparing a non-stoichiometric iron phosphate composite using an acidic iron-air battery and a positive electrode material for a sodium ion battery, which has the characteristics of controllable process, green environmental protection and low cost.
[0010] The present invention can be implemented by the following technical solutions: The invention discloses a method for preparing a non-stoichiometric iron phosphate composite by using an acidic iron-air battery. The iron-air battery comprises a positive electrode, a negative electrode and an electrolyte. A porous carbon electrode is used as the positive electrode, an iron electrode is used as the negative electrode, and an acidic phosphoric acid source solution containing phosphate and / or pyrophosphate is used as the electrolyte. A flowing oxygen atmosphere and an oxidant are added to the iron-air battery. Under temperature-controlled conditions, an oxidation-reduction reaction is achieved through the operation of the iron-air battery to generate a non-stoichiometric iron phosphate precipitate Fe. x H y (PO m ) (3x+y) / (2m-5) ·zH 2 O, the iron-hydrogen ratio x / y ranges from 0.5-8, x ranges from 0.6-0.96, y ranges from 0.12-1.2, z ranges from 1-4, and m ranges from 3.5-4.
[0011] In the present invention, due to the different concentrations of phosphate or pyrophosphate under acidic conditions, the Fe 3+ The concentration is also different. Considering the precipitation dissolution equilibrium, the iron-phosphorus ratio of the iron phosphate complex will be different if the proportion of each iron phosphate salt in the precipitate is different.
[0012] Specifically, the reactions that the present invention may involve are as follows: Negative electrode reaction: The iron electrode undergoes oxidation reaction at the negative electrode to generate divalent iron ions: Fe → Fe 2+ +2e − ; Positive electrode reaction: Oxygen is reduced at the air electrode and combines with hydrogen ions to generate water: O 2 +4H + +4e − →2H 2 O; Oxidation reaction: The divalent iron is oxidized by the flowing oxygen atmosphere and / or oxidant, 4Fe 2+ +O 2 +4H + →4Fe 3+ +2H 2 2Fe 2+ +H 2 O 2 +2H + →2Fe 3+ +2H 2 O; Precipitation reaction: Trivalent iron and different phosphate species undergo precipitation reaction, and the reaction equation is as follows: xH 2 O+Fe 3++PO 4 3− →FePO 4 ·xH 2 O↓; xH 2 O+Fe 3+ +3H 2 PO 4 − →Fe(H 2 PO 4 ) 3 ·xH 2 O↓; xH 2 O+2Fe 3+ +3HPO 4 2− →Fe 2 (HPO 4 ) 3 ·xH 2 O↓; 4Fe 3+ +3P 2 O 7 4− →2FeP 2 O 7 ↓.
[0013] Furthermore, the electrolyte is an acid solution or a phosphate solution with an acid solution added thereto, the acid solution is one or more of phosphoric acid, pyrophosphoric acid, and sulfuric acid, the phosphate solution is one or more of phosphoric acid and pyrophosphate such as sodium dihydrogen phosphate solution, ammonium dihydrogen phosphate solution, and sodium pyrophosphate, the mass concentration range of phosphorus element in the electrolyte is 1.0-15wt%, and the pH of the electrolyte is 1-3. In the overall process, the pH of the reaction solution is not adjusted by alkaline solution, but mainly by regulating the working time of the battery and the concentration of the acid solution in the phosphorus source. The higher the concentration of the acid solution, the lower the pH of the solution. At the same time, increasing the phosphorus concentration is beneficial to increasing the ionic conductivity of the solution, which is beneficial to Fe 3+The combination of phosphorus sources, the higher the concentration of the phosphorus source, the faster the reaction rate of the two, and the greater the compaction density of the prepared product. However, if the concentration is too high, the viscosity of the solution will be too high, which is not conducive to the reaction. The pH of the solution is a key parameter for regulating the preparation of non-stoichiometric iron phosphate materials. The lower the pH of the solution, the more acidic species of phosphoric acid and pyrophosphoric acid in the solution, the lower the iron-hydrogen ratio of the prepared non-stoichiometric iron phosphate, which in turn leads to a lower iron-phosphorus ratio of the prepared non-stoichiometric iron phosphate. The higher the pH of the solution, the more conducive it is to the formation of iron phosphate, the higher the iron-hydrogen ratio of the prepared non-stoichiometric iron phosphate, which in turn leads to a higher iron-phosphorus ratio of the prepared non-stoichiometric iron phosphate. However, when the pH of the solution is too low, the solubility of the precipitate increases, which greatly reduces the production efficiency, and when the pH of the solution increases to more than 3, it tends to form iron hydroxide, which introduces impurities into the final product.
[0014] Further, the working conditions of the battery are: the working temperature is 30-90 ° C. In the present invention, the working temperature is the key to realize the efficient redox reaction and the precipitation reaction of the iron phosphate complex. The working temperature affects the rate of the internal chemical reaction of the battery and the activity of the electrode material, thereby affecting the charge and discharge efficiency and overall performance of the battery; at the same time, the temperature range of 30-90 ° C takes into account the safe operation requirements of the battery at the same time, avoiding potential safety risks caused by overheating; the working time is 1-10h. The working time of the battery has a direct impact on the concentration of iron ions in the solution and the pH of the solution. The longer the working time, the higher the pH in the solution, and the higher the concentration of iron ions in the solution, and then by regulating the working time of the battery, the iron-phosphorus ratio in the solution is regulated. The longer the working time, the higher the iron-phosphorus ratio in the solution. Therefore, as the working time of the battery is increased, it is beneficial to increase the iron-hydrogen ratio of the non-stoichiometric iron phosphate, thereby increasing the iron-phosphorus ratio of the prepared non-stoichiometric iron phosphate.
[0015] Further, the flowing oxygen atmosphere is oxygen and / or air, and according to the power demand and reaction efficiency of the battery, a flow meter or a mass flow controller is used to accurately control the gas flow entering the battery to optimize the electrode reaction. The gas flow rate needs to be determined according to the power demand and electrode reaction kinetics of the battery to ensure sufficient oxygen supply while avoiding unnecessary energy loss caused by excessive flow rate. Specifically, the flow rate of the flowing oxygen atmosphere is 0.1L / min-1.0L / min.
[0016] Furthermore, the iron electrode is an iron sheet, an iron plate, foamed iron or an iron alloy to optimize electrochemical performance and structural stability; the porous carbon electrode is a porous graphite sheet, carbon paper, carbon cloth or carbon nanotube.
[0017] Furthermore, the positive electrode and the negative electrode are electrically connected through a wire made of the above materials, and the wire material is copper, silver or tinned copper. The wire is made of materials with good conductivity and chemical stability to ensure efficient electron transmission and corrosion resistance. The wire is designed as a multi-strand twisted structure to improve flexibility and mechanical strength and reduce the risk of damage during battery assembly and operation. The connection between the wire and the electrode is achieved by welding, crimping or bolting to ensure the reliability and long-term stability of the electrical connection. There should be an appropriate insulation layer on the outside of the wire to prevent electrical safety problems caused by short circuits or accidental contact.
[0018] Furthermore, the iron electrode of the iron-air battery is provided with an air inlet for conveying a flowing oxygen atmosphere, and the porous electrode is provided with a liquid inlet for adding an oxidant. The oxidation of the divalent iron is achieved by flowing the oxygen atmosphere and / or the oxidant, and the oxygen at the air electrode can be reduced to hydrogen peroxide, thereby acting as an oxidant for the divalent iron.
[0019] Furthermore, the carrier container of the iron-air battery is a plastic container or a metal container, the plastic container is made of polytetrafluoroethylene, polypropylene, polyvinyl chloride or polyetheretherketone, and the metal container is made of stainless steel or titanium alloy. The above materials are all resistant to acid and corrosion, have good sealing performance, and are temperature tolerant, so as to ensure that no chemical reaction or degradation occurs during long-term use in an acidic environment.
[0020] Furthermore, non-stoichiometric iron phosphate Fe x H y (PO m ) (3x+y) / (2m-5) ·zH 2 After separation, an aging treatment is performed. The aging treatment conditions are as follows: an aging temperature of 30-90°C promotes the stabilization of the precipitate in the solution and the growth of particles. Within the aging temperature range of 30-90°C, the precipitate can obtain better stability and sedimentation performance, which is convenient for subsequent separation and washing; the aging time is 2-5h. Specifically, the solid-liquid separation method includes but is not limited to one or more of sedimentation, filtration, suction filtration, centrifugation, and filter press. Finally, Fe x H y (PO m ) (3x+y) / (2m-5) ·zH 2 O, in order to facilitate the expression of the general formula, 3x+y=3 is specified. Based on the test of the iron-hydrogen ratio of the product, the iron-hydrogen ratio x / y ranges from 0.5-8, the range of x is 0.6-0.96, the range of y is 0.12-1.2, the range of z is 1-4, and the range of m is 3.5-4. The pyrophosphate in the heating process and the raw materials is easy to introduce pyrophosphate into the final product, so the range of m is 3.5-4. The iron-phosphorus ratio of the non-stoichiometric acid ferric phosphate and the non-stoichiometric ferric phosphate material is 0.6-0.9.
[0021] Another aspect of the present invention is to protect a sodium ion battery positive electrode material, which uses the non-stoichiometric iron phosphate composite prepared as a raw material for a phosphorus source and / or an iron source. For example, a polyanionic composite sodium iron phosphate is obtained by high-temperature sintering using the composite as a phosphorus source, an iron source, a sodium source, and a carbon source, wherein the sodium source can be one or more of sodium carbonate, sodium dihydrogen phosphate, and sodium nitrate, and the carbon source can be one or more of citric acid, sucrose, glucose, starch, and PEG, and calcined under a protective atmosphere to form a carbon-coated composite sodium iron phosphate positive electrode material.
[0022] The present invention discloses a method for preparing a non-stoichiometric iron phosphate composite using an acidic iron-air battery and a positive electrode material for a sodium ion battery, which has the following beneficial effects: First, the process is controllable. By finely controlling the reaction temperature, gas flow rate (0.1-1.0 L / min) and reaction time (1-10 hours), the pH of the final solution and the concentration of trivalent iron in the solution are affected to regulate the iron phosphate complex Fe. x H y (PO m ) (3x+y) / (2m-5) ·zH 2 O parameters such as iron-phosphorus ratio, particle size, compacted density, etc.; Second, it is green and environmentally friendly. The preparation of iron phosphate using acidic iron-air batteries is based on the principle of primary batteries. The reaction is directly carried out inside the battery through electrochemical methods to convert chemical energy into electrical energy. No additional energy needs to be injected, which reduces the need for external energy input, realizes the oxidation of iron solution, and finally realizes the precipitation of iron phosphate complexes, thereby improving the overall energy efficiency of preparing iron phosphate. Third, it is low-cost and uses a combination of air electrode and iron electrode, as well as a suitable electrolyte solution, to achieve efficient electrochemical reaction; the dried iron phosphate complex is used as a precursor of sodium iron phosphate pyrophosphate, the positive electrode material for sodium ion batteries, which greatly reduces the production cost, and the positive electrode material exhibits excellent electrochemical properties. DETAILED DESCRIPTION
[0023] In order to enable those skilled in the art to better understand the technical solution of the present invention, the product of the present invention is further described in detail below in conjunction with embodiments.
[0024] The invention discloses a method for preparing a non-stoichiometric iron phosphate composite by using an acidic iron-air battery. The iron-air battery comprises a positive electrode, a negative electrode and an electrolyte. A porous carbon electrode is used as the positive electrode, an iron electrode is used as the negative electrode, and an acidic phosphoric acid source solution containing phosphate and / or pyrophosphate is used as the electrolyte. A flowing oxygen atmosphere and an oxidant are added to the iron-air battery. Under temperature-controlled conditions, an oxidation-reduction reaction is achieved through the operation of the iron-air battery to generate a non-stoichiometric iron phosphate precipitate Fe. x H y (PO m ) (3x+y) / (2m-5) ·zH 2 O, wherein the iron-hydrogen ratio x / y is in the range of 0.5-8, x is in the range of 0.6-0.96, y is in the range of 0.12-1.2, z is in the range of 1-4, and m is in the range of 3.5-4. .
[0025] Furthermore, the electrolyte is an acid solution or a phosphate solution to which an acid solution is added, the acid solution is one or more of phosphoric acid, pyrophosphoric acid, and sulfuric acid, the phosphate solution is one or more of phosphoric acid and pyrophosphate such as sodium dihydrogen phosphate solution, ammonium dihydrogen phosphate solution, and sodium pyrophosphate, the mass concentration range of phosphorus element in the electrolyte is 1.0-15wt%, and the pH of the electrolyte is 1-3.
[0026] Furthermore, the working conditions of the battery are: working temperature is 30-90°C; working time is 1-10h.
[0027] Furthermore, the flowing oxygen atmosphere is oxygen and / or air, and the flow rate of the flowing oxygen atmosphere is 0.1 L / min-1.0 L / min.
[0028] Furthermore, the iron electrode is an iron sheet, an iron plate, foamed iron or an iron alloy, and the porous carbon electrode is a porous graphite sheet, carbon paper, carbon cloth or carbon nanotube.
[0029] Furthermore, the positive electrode and the negative electrode are electrically connected via a wire, and the wire is made of copper, silver or tinned copper.
[0030] Furthermore, the iron electrode of the iron-air battery is provided with an air inlet for conveying a flowing oxygen atmosphere, and the porous electrode is provided with a liquid inlet for adding an oxidant.
[0031] Furthermore, the carrier container of the iron-air battery is a plastic container or a metal container, the material of the plastic container is polytetrafluoroethylene, polypropylene, polyvinyl chloride or polyetheretherketone, and the material of the metal container is stainless steel or titanium alloy.
[0032] Furthermore, non-stoichiometric iron phosphate precipitation of Fe x H y (PO m ) (3x+y) / (2m-5)·zH 2 After separation, the O is further aged. The conditions for the ageing treatment are: an ageing temperature of 30-90°C; an ageing time of 2-5h.
[0033] Another aspect of the present invention is to protect a sodium ion battery positive electrode material, which uses the non-stoichiometric non-stoichiometric iron phosphate prepared as a raw material for a phosphorus source and / or an iron source.
[0034] Example 1 This embodiment involves using an acidic iron-air battery to prepare a non-stoichiometric iron phosphate composite and using it as a phosphorus source and an iron source to prepare a positive electrode material for a sodium ion battery, and the preparation process includes the following steps: S1. Assemble the battery module: use a polytetrafluoroethylene container as the electrolyte solution container (size is 12cm x12cm x 5cm), a porous graphite sheet (size is 10cm x 10cm x 0.1cm) as the air electrode, and foam iron (size is 10cm x 10cm x 0.1cm) as the negative electrode. Prepare a phosphorus reaction solution with a mass percentage of 5wt% of phosphorus as the electrolyte, and use copper wires wrapped with insulated wires to connect the positive and negative electrodes through an ammeter.
[0035] S2. Conduct electrochemical reaction: start mechanical stirring, set the speed to 600 r / min, set the operating temperature of the battery module to 50 degrees Celsius, introduce air flow into both the negative and positive electrodes, and the gas flow rate is 0.5 L / min. The reaction time is 5 hours, and the pH of the solution is raised to 1.5.
[0036] S3, aging, solid-liquid separation and drying: disconnect the circuit, transfer the material in the electrolyte solution container into a beaker, age it at 70 degrees Celsius for 4 hours, then separate the solid and liquid by centrifugation, and repeatedly centrifuge and wash it 5 times with deionized water as a detergent. The washed material is dried at 100 degrees Celsius to obtain non-stoichiometric iron phosphate, and the test results of its iron-hydrogen ratio and iron-phosphorus ratio are shown in Table 1.
[0037] S4. Preparation of positive electrode for sodium ion battery: The iron phosphate complex prepared in step S3 above is used as the iron-phosphorus source, and other sodium salts and organic carbon sources are mixed as raw materials, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode, the electrochemical properties of which are shown in Table 1.
[0038] Example 2 This embodiment involves using an acidic iron-air battery to prepare a non-stoichiometric non-stoichiometric iron phosphate and using it as a phosphorus source and an iron source to prepare a positive electrode material for a sodium ion battery, and the preparation process includes the following steps: S1. Assemble the battery module: Use a polytetrafluoroethylene container as the electrolyte solution container (size is 12cm x12cm x 5cm), a porous graphite sheet (size is 10cm x 10cm x 0.1cm) as the air electrode, and foam iron (size is 10cm x 10cm x 0.1cm) as the negative electrode. Prepare a phosphoric acid solution with a mass percentage of 5wt% of phosphorus as the electrolyte, and use copper wires wrapped with insulated wires to connect the positive and negative electrodes through an ammeter.
[0039] S2. Conduct electrochemical reaction: start mechanical stirring, set the speed to 600 r / min, set the operating temperature of the battery module to 70 degrees Celsius, introduce air flow into both the negative and positive electrodes, and the gas flow rate is 0.5 L / min. The reaction time is 5 hours, and the pH of the solution is raised to 2.
[0040] S3, aging, solid-liquid separation and drying: disconnect the circuit, transfer the material in the electrolyte solution container into a beaker, age it at 80 degrees Celsius for 4 hours, then separate the solid and liquid by centrifugation, and repeatedly centrifuge and wash it 5 times with deionized water as a detergent. The washed material is dried at 100 degrees Celsius to obtain non-stoichiometric iron phosphate, and the test results of its iron-hydrogen ratio and iron-phosphorus ratio are shown in Table 1.
[0041] S4. Preparation of positive electrode for sodium ion battery: Using the non-stoichiometric iron phosphate prepared in step S3 as the iron-phosphorus source, other sodium salts and organic carbon sources are mixed as raw materials, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode, the electrochemical properties of which are shown in Table 1.
[0042] Example 3 This embodiment involves using an acidic iron-air battery to prepare a non-stoichiometric non-stoichiometric iron phosphate and using it as a phosphorus source and an iron source to prepare a positive electrode material for a sodium ion battery, and the preparation process includes the following steps: S1. Assemble the battery module: Use a polytetrafluoroethylene container as the electrolyte solution container (size is 12cm x12cm x 5cm), a porous graphite sheet (size is 10cm x 10cm x 0.1cm) as the air electrode, and foam iron (size is 10cm x 10cm x 0.1cm) as the negative electrode. Prepare a phosphoric acid solution with a mass percentage of 7wt% of phosphorus as the electrolyte, and use copper wires wrapped with insulated wires to connect the positive and negative electrodes through an ammeter.
[0043] S2. Conduct electrochemical reaction: start mechanical stirring, set the speed to 600 r / min, set the operating temperature of the battery module to 50 degrees Celsius, introduce air flow into both the negative and positive electrodes, and the gas flow rate is 0.5 L / min. The reaction time is 5 hours, and the pH of the solution is raised to 1.
[0044] S3, aging, solid-liquid separation and drying: disconnect the circuit, transfer the material in the electrolyte solution container into a beaker, age it at 70 degrees Celsius for 4 hours, then separate the solid and liquid by centrifugation, and repeatedly centrifuge and wash it 5 times with deionized water as a detergent. The washed material is dried at 100 degrees Celsius to obtain non-stoichiometric iron phosphate, and the test results of its iron-hydrogen ratio and iron-phosphorus ratio are shown in Table 1.
[0045] Example 4 This embodiment involves using an acidic iron-air battery to prepare a non-stoichiometric non-stoichiometric iron phosphate and using it as a phosphorus source and an iron source to prepare a positive electrode material for a sodium ion battery, and the preparation process includes the following steps: S1. Assemble the battery module: Use a polytetrafluoroethylene container as the electrolyte solution container (size is 12cm x12cm x 5cm), a porous graphite sheet (size is 10cm x 10cm x 0.1cm) as the air electrode, and foam iron (size is 10cm x 10cm x 0.1cm) as the negative electrode. Prepare a phosphoric acid solution with a mass percentage of 5wt% of phosphorus as the electrolyte, and use copper wires wrapped with insulated wires to connect the positive and negative electrodes through an ammeter.
[0046] S2. Conduct electrochemical reaction: start mechanical stirring, set the speed to 600 r / min, set the operating temperature of the battery module to 50 degrees Celsius, introduce air flow into both the negative and positive electrodes, and the gas flow rate is 1 L / min. The reaction time is 5 hours, and the pH of the solution rises to 2.3.
[0047] S3, aging, solid-liquid separation and drying: disconnect the circuit, transfer the material in the electrolyte solution container into a beaker, age it at 70 degrees Celsius for 4 hours, then separate the solid and liquid by centrifugation, and repeatedly centrifuge and wash it 5 times with deionized water as a detergent. The washed material is dried at 100 degrees to obtain non-stoichiometric iron phosphate, and the test results of its iron-hydrogen ratio and iron-phosphorus ratio are shown in Table 1.
[0048] Example 5 This embodiment involves using an acidic iron-air battery to prepare a non-stoichiometric non-stoichiometric iron phosphate and using it as a phosphorus source and an iron source to prepare a positive electrode material for a sodium ion battery, and the preparation process includes the following steps: S1. Assemble the battery module: use a polytetrafluoroethylene container as the electrolyte solution container (size: 12cm x 12cm x 5cm), carbon paper (size: 10cm x 10cm x 0.1cm) as the air electrode, foam iron (size: 10cm x 10cm x 0.1cm) as the negative electrode, prepare a phosphoric acid solution with a mass percentage of 5wt% of phosphorus as the electrolyte, and use copper wires wrapped with insulated wires to connect the positive and negative electrodes through an ammeter.
[0049] S2. Conduct electrochemical reaction: start mechanical stirring, set the speed to 600 r / min, set the operating temperature of the battery module to 50 degrees Celsius, introduce air flow into both the negative and positive electrodes, and the gas flow rate is 0.5 L / min. The reaction time is 8 hours, and the pH of the solution rises to 2.2.
[0050] S3, aging, solid-liquid separation and drying: disconnect the circuit, transfer the material in the electrolyte solution container into a beaker, age it at 70 degrees Celsius for 4 hours, then separate the solid and liquid by centrifugation, and repeatedly centrifuge and wash it 5 times with deionized water as a detergent. The washed material is dried at 100 degrees Celsius to obtain non-stoichiometric iron phosphate, and the test results of its iron-hydrogen ratio and iron-phosphorus ratio are shown in Table 1.
[0051] S4. Preparation of positive electrode for sodium ion battery: Using the non-stoichiometric iron phosphate prepared in step S3 as the iron-phosphorus source, other sodium salts and organic carbon sources are mixed as raw materials, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode, the electrochemical properties of which are shown in Table 1.
[0052] Example 6 The present embodiment relates to the preparation of non-stoichiometric iron phosphate using an acidic iron-air battery and the use of the non-stoichiometric iron phosphate as a phosphorus source and an iron source to prepare a positive electrode material for a sodium ion battery, and the preparation process includes the following steps: S1, assembling a battery module: using a polytetrafluoroethylene container as an electrolyte solution container (size is 12cm x 12cm x 5cm), a porous graphite sheet (size is 10cm x 10cm x 0.1cm) for the air electrode, and foam iron (size is 10cm x 10cm x 0.1cm) for the negative electrode, a mixed solution of sodium dihydrogen phosphate and sulfuric acid is prepared as an electrolyte according to a mass percentage of 5wt% of the phosphorus element, and a copper wire wrapped with an insulated wire is used to connect the positive and negative electrodes through an ammeter.
[0053] S2. Conduct electrochemical reaction: start mechanical stirring, set the speed to 600 r / min, set the operating temperature of the battery module to 50 degrees Celsius, introduce air flow into both the negative and positive electrodes, and the gas flow rate is 0.5 L / min. The reaction time is 5 hours, and the pH of the solution is raised to 1.5.
[0054] S3, aging, solid-liquid separation and drying: disconnect the circuit, transfer the material in the electrolyte solution container into a beaker, age it at 70 degrees Celsius for 4 hours, then separate the solid and liquid by centrifugation, and repeatedly centrifuge and wash it 5 times with deionized water as a detergent. The washed material is dried at 100 degrees to obtain non-stoichiometric iron phosphate, and the test results of its iron-hydrogen ratio and iron-phosphorus ratio are shown in Table 1.
[0055] S4. Preparation of positive electrode for sodium ion battery: Using the non-stoichiometric iron phosphate prepared in step S3 as the iron-phosphorus source, other sodium salts and organic carbon sources are mixed as raw materials, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode, the electrochemical properties of which are shown in Table 1.
[0056] Example 7 The present embodiment relates to the preparation of non-stoichiometric iron phosphate using an acidic iron-air battery and the use of the non-stoichiometric iron phosphate as a phosphorus source and an iron source to prepare a positive electrode material for a sodium ion battery, and the preparation process includes the following steps: S1, assembling a battery module: using a polytetrafluoroethylene container as an electrolyte solution container (size is 12cm x 12cm x 5cm), a carbon cloth (size is 10cm x 10cm x 0.1cm) for the air electrode, an iron sheet (size is 10cm x 10cm x 0.1cm) for the negative electrode, a phosphoric acid solution is prepared as an electrolyte according to a mass percentage of 5wt% of the phosphorus element, and a copper wire wrapped with an insulated wire is used to connect the positive and negative electrodes through an ammeter.
[0057] S2. Conduct electrochemical reaction: start mechanical stirring, set the speed to 600 r / min, set the operating temperature of the battery module to 50 degrees Celsius, introduce air flow into both the negative and positive electrodes, and the gas flow rate is 0.5 L / min. The reaction time is 5 hours, and the pH of the solution is raised to 1.5.
[0058] S3, aging, solid-liquid separation and drying: disconnect the circuit, transfer the material in the electrolyte solution container into a beaker, age it at 70 degrees Celsius for 4 hours, then separate the solid and liquid by centrifugation, and repeatedly centrifuge and wash it 5 times with deionized water as a detergent. The washed material is dried at 100 degrees Celsius to obtain non-stoichiometric iron phosphate, and the test results of its iron-hydrogen ratio and iron-phosphorus ratio are shown in Table 1.
[0059] S4. Preparation of positive electrode for sodium ion battery: Using the non-stoichiometric iron phosphate prepared in step S3 as the iron-phosphorus source, other sodium salts and organic carbon sources are mixed as raw materials, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode, the electrochemical properties of which are shown in Table 1.
[0060] Example 8 The present embodiment relates to the preparation of non-stoichiometric iron phosphate using an acidic iron-air battery and the use of the non-stoichiometric iron phosphate as a phosphorus source and an iron source to prepare a positive electrode material for a sodium ion battery, and the preparation process includes the following steps: S1, assembling a battery module: using a polytetrafluoroethylene container as an electrolyte solution container (size is 12cm x 12cm x 5cm), a carbon cloth (size is 10cm x 10cm x 0.1cm) for the air electrode, an iron sheet (size is 10cm x 10cm x 0.1cm) for the negative electrode, a phosphoric acid solution is prepared as an electrolyte according to a mass percentage of 5wt% of the phosphorus element, and a copper wire wrapped with an insulated wire is used to connect the positive and negative electrodes through an ammeter.
[0061] S2. Conduct electrochemical reaction: start mechanical stirring, set the speed to 600 r / min, set the operating temperature of the battery module to 50 degrees Celsius, introduce air flow into the positive electrode with a gas flow rate of 0.5 L / min, add hydrogen peroxide solution to the negative electrode solution, the reaction time is 5 hours, and the pH of the solution is raised to 1.5.
[0062] S3, aging, solid-liquid separation and drying: disconnect the circuit, transfer the material in the electrolyte solution container into a beaker, age it at 70 degrees Celsius for 4 hours, then separate the solid and liquid by centrifugation, and repeatedly centrifuge and wash it 5 times with deionized water as a detergent. The washed material is dried at 100 degrees to obtain non-stoichiometric iron phosphate, and the test results of its iron-hydrogen ratio and iron-phosphorus ratio are shown in Table 1.
[0063] S4. Preparation of positive electrode for sodium ion battery: Using the non-stoichiometric iron phosphate prepared in step S3 as the iron-phosphorus source, other sodium salts and organic carbon sources are mixed as raw materials, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode, the electrochemical properties of which are shown in Table 1.
[0064] Example 9 The present embodiment relates to the preparation of non-stoichiometric iron phosphate using an acidic iron-air battery and the use of the non-stoichiometric iron phosphate as a phosphorus source and an iron source to prepare a positive electrode material for a sodium ion battery, and the preparation process includes the following steps: S1, assembling a battery module: using a polytetrafluoroethylene container as an electrolyte solution container (size 12cm x 12cm x 5cm), a porous graphite sheet (size 10cm x 10cm x 0.1cm) for the air electrode, an iron sheet (size 10cm x 10cm x 0.1cm) for the negative electrode, a mixed solution of phosphoric acid and sodium dihydrogen phosphate is prepared as an electrolyte according to a mass percentage of 5wt% of the phosphorus element, and a copper wire wrapped with an insulated wire is used to connect the positive and negative electrodes through an ammeter.
[0065] S2. Conduct electrochemical reaction: start mechanical stirring, set the speed to 600 r / min, set the operating temperature of the battery module to 50 degrees Celsius, introduce air flow into both the negative and positive electrodes, and the gas flow rate is 0.5 L / min. The reaction time is 12 hours, and the pH of the solution is raised to 3.
[0066] S3, aging, solid-liquid separation and drying: disconnect the circuit, transfer the material in the electrolyte solution container into a beaker, age it at 70 degrees Celsius for 4 hours, then separate the solid and liquid by centrifugation, and repeatedly centrifuge and wash it 5 times with deionized water as a detergent. The washed material is dried at 100 degrees to obtain non-stoichiometric iron phosphate, and the test results of its iron-hydrogen ratio and iron-phosphorus ratio are shown in Table 1.
[0067] S4. Preparation of positive electrode for sodium ion battery: Using the non-stoichiometric iron phosphate prepared in step S3 as the iron-phosphorus source, other sodium salts and organic carbon sources are mixed as raw materials, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode, the electrochemical properties of which are shown in Table 1.
[0068] Embodiment 11 This embodiment involves using an acidic iron-air battery to prepare a non-stoichiometric non-stoichiometric iron phosphate and using it as a phosphorus source and an iron source to prepare a positive electrode material for a sodium ion battery, and the preparation process includes the following steps: S1. Assemble the battery module: use a polytetrafluoroethylene container as the electrolyte solution container (size is 12cm x12cm x 5cm), a porous graphite sheet (size is 10cm x 10cm x 0.1cm) as the air electrode, and foam iron (size is 10cm x 10cm x 0.1cm) as the negative electrode. Prepare a mixed solution of phosphoric acid, pyrophosphoric acid, and sodium iron pyrophosphate according to a mass percentage of 5wt% of phosphorus as the electrolyte, and use copper wires wrapped with insulated wires to connect the positive and negative electrodes through an ammeter.
[0069] S2. Conduct electrochemical reaction: start mechanical stirring, set the speed to 600 r / min, set the operating temperature of the battery module to 50 degrees Celsius, introduce air flow into both the negative and positive electrodes, and the gas flow rate is 0.5 L / min. The reaction time is 5 hours, and the pH of the solution is raised to 1.5.
[0070] S3, aging, solid-liquid separation and drying: disconnect the circuit, transfer the material in the electrolyte solution container into a beaker, age it at 70 degrees Celsius for 4 hours, then separate the solid and liquid by centrifugation, and repeatedly centrifuge and wash it 5 times with deionized water as a detergent. The washed material is dried at 100 degrees Celsius to obtain non-stoichiometric iron phosphate, and the test results of its iron-hydrogen ratio and iron-phosphorus ratio are shown in Table 1.
[0071] S4. Preparation of positive electrode for sodium ion battery: Using the non-stoichiometric iron phosphate prepared in step S3 as the iron-phosphorus source, other sodium salts and organic carbon sources are mixed as raw materials, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode, the electrochemical properties of which are shown in Table 1.
[0072] Example 12 This embodiment involves using an acidic iron-air battery to prepare a non-stoichiometric non-stoichiometric iron phosphate and using it as a phosphorus source and an iron source to prepare a positive electrode material for a sodium ion battery, and the preparation process includes the following steps: S1. Assemble the battery module: Use a polytetrafluoroethylene container as the electrolyte solution container (size is 12cm x12cm x 5cm), a porous graphite sheet (size is 10cm x 10cm x 0.1cm) as the air electrode, and foam iron (size is 10cm x 10cm x 0.1cm) as the negative electrode. Prepare a mixed solution of phosphoric acid, sulfuric acid, and diammonium dihydrogen phosphate at a mass percentage of 5wt% of phosphorus as the electrolyte, and use copper wires wrapped with insulated wires to connect the positive and negative electrodes through an ammeter.
[0073] S2. Conduct electrochemical reaction: start mechanical stirring, set the speed to 600 r / min, set the operating temperature of the battery module to 50 degrees Celsius, introduce air flow into both the negative and positive electrodes, and the gas flow rate is 0.5 L / min. The reaction time is 5 hours, and the pH of the solution is raised to 1.5.
[0074] S3, aging, solid-liquid separation and drying: disconnect the circuit, transfer the material in the electrolyte solution container into a beaker, age it at 70 degrees Celsius for 4 hours, then separate the solid and liquid by centrifugation, and repeatedly centrifuge and wash it 5 times with deionized water as a detergent. The washed material is dried at 100 degrees Celsius to obtain non-stoichiometric iron phosphate, and the test results of its iron-hydrogen ratio and iron-phosphorus ratio are shown in Table 1.
[0075] S4. Preparation of positive electrode for sodium ion battery: Using the non-stoichiometric iron phosphate prepared in step S3 as the iron-phosphorus source, other sodium salts and organic carbon sources are mixed as raw materials, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode, the electrochemical properties of which are shown in Table 1.
[0076] Table 1 Performance test results The present invention firstly utilizes an acidic iron-air battery to prepare iron phosphate. Based on the principle of a primary battery, chemical energy is converted into electrical energy. Except for introducing an air flow, no additional energy needs to be injected to achieve oxidation of the iron solution and finally achieve precipitation of non-stoichiometric iron phosphate, thereby providing a new technical approach for the preparation of iron phosphate.
[0077] According to the test results in Table 1, it can be seen that the reaction progress can be adjusted by controlling the reaction temperature, reaction time, air flow rate, and concentration of reactants, which ultimately affects the pH during precipitation. By flexibly regulating various parameters, iron phosphates with different iron-phosphorus ratios can be prepared. Using the prepared low iron-phosphorus ratio non-stoichiometric iron phosphate as an iron-phosphorus source, a sodium iron pyrophosphate positive electrode material with high electrochemical performance can be prepared.
[0078] In summary, the present invention has good technical contributions in the following aspects: Adjustability: By adjusting the reaction conditions such as pH value, temperature, reaction time, etc., non-stoichiometric iron phosphate with different iron-hydrogen ratios and iron-phosphorus ratios can be prepared. x H y (PO m ) (3x+y) / (2m-5) ·zH 2 O, increased product diversity.
[0079] Improved environmental friendliness: The present invention does not adopt the traditional chemical precipitation method or electrolysis method, thus avoiding the use of harmful chemical reagents and energy-intensive processes commonly found in these methods, and reducing the negative impact on the environment.
[0080] Energy efficiency: The reaction is directly carried out inside the battery through electrochemical methods, which reduces the need for external energy input and improves the overall energy efficiency of iron phosphate preparation. At the same time, battery packs can be connected in series to achieve efficient preparation and scalability.
[0081] Cost-effectiveness: It uses low-cost raw materials such as iron and phosphoric acid, while simplifying the preparation process and reducing production costs.
[0082] Product purity and consistency: By precisely controlling the electrochemical conditions and reaction time, high purity and consistency of iron phosphate products can be obtained, which is beneficial to improving the performance of the final product.
[0083] Improved performance of sodium-ion batteries: High-purity non-stoichiometric iron phosphate obtained through solid-liquid separation can be used as a high-quality precursor for sodium-ion battery positive electrode materials, which helps to improve battery performance and reduce production costs.
[0084] The above embodiments are only specific embodiments of the present invention, and their descriptions are relatively specific and detailed, but they cannot be understood as limiting the scope of the present invention. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, and these obvious replacement forms all belong to the protection scope of the present invention.
Claims
1. A method for preparing a non-stoichiometric iron phosphate composite using an acidic iron-air battery, wherein the iron-air battery comprises a positive electrode, a negative electrode and an electrolyte, Features: A porous carbon electrode is used as the positive electrode, an iron electrode is used as the negative electrode, and an acidic phosphate source solution containing phosphate and / or pyrophosphate is used as the electrolyte. A flowing oxygen atmosphere and an oxidant are added to the iron-air battery. Under temperature-controlled conditions, the iron-air battery is operated to realize a redox reaction to generate non-stoichiometric iron phosphate precipitate Fe. x H y (PO m ) (3x+y) / (2m-5) ·zH 2 O, wherein: the iron-hydrogen ratio x / y is in the range of 0.5-8, the range of x is 0.6-0.96, the range of y is 0.12-1.2, the range of z is 1-4, and the range of m is 3.5-4.
2. The method for preparing a non-stoichiometric iron phosphate composite using an acidic iron-air battery according to claim 1, Features: The electrolyte is an acid solution or a phosphate solution to which an acid solution is added, the acid solution is one or more of phosphoric acid, pyrophosphoric acid, and sulfuric acid, the phosphate solution is one or more of phosphoric acid and pyrophosphate such as sodium dihydrogen phosphate solution, ammonium dihydrogen phosphate solution, and sodium pyrophosphate, the mass concentration range of phosphorus element in the electrolyte is 1.0-15wt%, and the pH of the electrolyte is 1-3.
3. The method for preparing a non-stoichiometric iron phosphate composite using an acidic iron-air battery according to claim 1, Features: The working conditions of the battery are: working temperature of 30-90°C; working time of 1-10h.
4. The method for preparing a non-stoichiometric iron phosphate composite using an acidic iron-air battery according to claim 1, Features: The flowing oxygen atmosphere is oxygen and / or air, and the flow rate of the flowing oxygen atmosphere is 0.1 L / min-1.0 L / min.
5. The method for preparing a non-stoichiometric iron phosphate composite using an acidic iron-air battery according to claim 4, Features: The iron electrode is an iron sheet, an iron plate, foamed iron or an iron alloy, and the porous carbon electrode is a porous graphite sheet, carbon paper, carbon cloth or carbon nanotube.
6. The method for preparing a non-stoichiometric iron phosphate composite using an acidic iron-air battery according to claim 1, Features: The positive electrode and the negative electrode are electrically connected via a wire, and the wire is made of copper, silver or tinned copper.
7. The method for preparing a non-stoichiometric iron phosphate composite using an acidic iron-air battery according to claim 1, Features: The iron electrode of the iron-air battery is provided with an air inlet for conveying a flowing oxygen atmosphere, and the porous electrode is provided with a liquid inlet for adding an oxidant.
8. The method for preparing a non-stoichiometric iron phosphate composite using an acidic iron-air battery according to claim 1, Features: The carrier container of the iron-air battery is a plastic container or a metal container. The material of the plastic container is polytetrafluoroethylene, polypropylene, polyvinyl chloride or polyetheretherketone, and the material of the metal container is stainless steel or titanium alloy.
9. The method for preparing a non-stoichiometric iron phosphate composite using an acidic iron-air battery according to claim 1, Features: The non-stoichiometric ferric phosphate precipitate Fe x H y (PO m ) (3x+y) / (2m-5) ·zH 2 After separation, the O is further aged. The conditions for the ageing treatment are: an ageing temperature of 30-90°C; an ageing time of 2-5h.
10. A sodium ion battery cathode material, Features: The non-stoichiometric iron phosphate complex prepared according to any one of claims 1 to 9 is used as a raw material for a phosphorus source and / or an iron source.
Citation Information
Patent Citations
Method for preparing superfine iron phosphate through electrolytic method
CN102051630A
Preparation method and application of battery-grade iron phosphate precursor
CN115259124A
Method for preparing lamellar spherical iron phosphate based on electrochemical anodic oxidation
CN116426935A
Method for recovering iron phosphate
JP2016172654A
Cited By
Preparation method of three-dimensional micron spherical iron phosphate and product
CN120698429A