Weld metal for gas shielded arc welding

By adjusting the composition of the weld metal, the problem of insufficient strength and porosity resistance of the welded part in gas shielded arc welding technology is solved, the high strength and durability of the welded parts are achieved, the cost is reduced, and the light weight is suitable for the next generation of environmentally friendly cars. Quantify chassis component development.

CN118786000APending Publication Date: 2024-10-15POHANG IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380024541.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-02-01
Filing Date
2023-02-10
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing gas shielded arc welding technology has problems with insufficient welding strength and porosity resistance in automotive chassis components. Especially when coated steel is used, it is prone to early corrosion and fatigue degradation, and the welding productivity is low and the cost is high. .

Method used

By adjusting the components of the weld metal, ensure that C: 0.001 to 0.30%, Si: 0.25% or less, Mn: 0.50 to 3.00%, P: 0.030% or less, S: 0.030% or less, Cr: 0.50% or less, Mo: 0.60% or less, Al: less than 0.07%, Ni: 0.40% or less, Cu: 0.50% or less, and satisfy the specific relational expression 1 and relational expression 2 to reduce the zinc vapor pressure and the occurrence of pore defects, and improve the welding part strength and porosity resistance.

Benefits of technology

It effectively improves the strength and porosity resistance of the welded part, ensures the durability and economy of the welded parts, reduces the cost, and is suitable for the development of lightweight chassis parts for the next generation of environmentally friendly cars.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005019030260000131
    Figure BDA0005019030260000131
  • Figure BDA0005019030260000132
    Figure BDA0005019030260000132
  • Figure BDA0005019030260000141
    Figure BDA0005019030260000141
Patent Text Reader

Abstract

The invention provides a weld metal for gas-shielded arc welding. The present invention is a weld metal obtained by gas-shielded arc welding of a welding base material, the weld metal includes C: 0.001 to 0.30%, Si: 0.25% or less and 0% excluding, Mn: 0.50 to 3.00%, P: 0.030% or less and 0% excluding, S: 0.030% or less and 0% excluding, Cr: 0.50% or less and 0% excluding, Mo: 0.60% or less and 0% excluding, Al: less than 0.07% and 0% excluding, Ni: 0.40% or less and 0% excluding, Cu: 0.50% or less and 0% excluding, Ti: less than 0.07% and 0% excluding, and the balance being Fe and other unavoidable impurities, and satisfies relational expression 1 and relational expression 2.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a gas shielded arc welding weld metal. More specifically, the present invention relates to a gas shielded arc welding weld metal having excellent weld strength and porosity resistance and capable of ensuring the economic efficiency required for manufacturing parts. Background Art

[0002] In the automotive industry, due to fuel efficiency regulations for environmental protection such as global warming, the research on technologies to reduce the weight of vehicle bodies and parts is becoming a major issue. Chassis parts, which are crucial to the driving performance of automobiles, also need to follow this trend and use high-strength steel to reduce weight.

[0003] In order to achieve such lightweight components, the strength of the material must be improved, and ensuring the durability of components made of high-strength steel under repeated fatigue loads is an important factor.

[0004] However, when assembling automobile chassis parts, arc welding is mainly used to ensure strength, and arc welding is achieved by melting the welding wire to achieve lap welding between parts, so it is inevitable that the connection part has a geometric shape. Such a connection part becomes a repeated fatigue stress concentration part (notch effect) and becomes the starting point of fracture, which eventually leads to a decrease in the durability of the parts, so there is a limitation that the advantage of using high-strength steel is lost.

[0005] Therefore, in order to improve the fatigue characteristics of the weld, it is most important to reduce the angle (toe angle) of the end of the weld bead where the main stress is concentrated, and controlling the material and stress of the weld toe is an important factor. In addition, as mentioned above, due to the trend of high strength and lightweight of parts, the material is thinner, and the demand for rust resistance to prevent penetration corrosion has also increased. As a result, the use of coated steel tends to increase, but the weld metal of arc welding does not have a coating, so there is a limitation that the corrosion resistance after painting is poor compared with the base material. Therefore, there is a problem that the weld of the chassis parts made of coated steel plates will corrode early in the harsh corrosive environment when the vehicle is running and the fatigue characteristics will decrease. On the other hand, when gas shielded arc welding is performed on coated steel, due to the generation of zinc and other vapors, a large number of pits and pore-like pore defects will appear in the weld, and there is a concern that the strength of the weld will decrease, so the reduction in welding productivity has become a problem. In addition, for general uncoated steel, the slag generated in the weld during gas shielded arc welding can also cause poor painting, which becomes a factor in reducing corrosion resistance after painting. Therefore, when manufacturing parts, there is a problem of increased costs due to post-processing processes such as pickling or brushing to remove the slag after welding.

[0006] Recently, the development of lightweight chassis parts for next-generation environmentally friendly vehicles has been actively carried out, and in particular, the development of welding technology that can improve the characteristics of welded parts while ensuring economic efficiency has become an important issue.

[0007] [Prior art literature]

[0008] [Patent Document]

[0009] Patent document 1: Japanese Patent Publication No. 2019-118274 Summary of the invention

[0010] Technical issues to be solved

[0011] The present invention aims to provide a gas shielded arc welding weld metal having excellent weld strength and anti-porosity, which can ensure excellent weld strength and anti-porosity in the automotive industry. Weld metal refers to a metal obtained by melting a base material to be welded and a welding wire.

[0012] The problems of the present invention are not limited to the above-mentioned contents. Additional problems of the present invention are described throughout the specification, and it is not difficult for a person skilled in the art to which the present invention belongs to understand the additional problems of the present invention from the contents described in the specification of the present invention.

[0013] Technical Solution

[0014] Therefore, one aspect of the present invention relates to a weld metal for gas shielded arc welding, wherein:

[0015] The weld metal is a weld metal obtained by performing gas shielded arc welding on a welding base material, and contains, in weight%, C: 0.001-0.30%, Si: 0.25% or less and excluding 0%, Mn: 0.50-3.00%, P: 0.030% or less and excluding 0%, S: 0.030% or less and excluding 0%, Cr: 0.50% or less and excluding 0%, Mo: 0.60% or less and excluding 0%, Al: less than 0.07% and excluding 0%, Ni: 0.40% or less and excluding 0%, Cu: 0.50% or less and excluding 0%, Ti: less than 0.07% and excluding 0%, the balance Fe and other inevitable impurities, and satisfies the following Relationships 1 and 2.

[0016] [Equation 1]

[0017] 3.5≤[Si]×100 / [Mn]≤8.5

[0018] [Equation 2]

[0019] [Ti]+[Al]<0.07

[0020] In the above-mentioned Relational Formulas 1 and 2, [Si], [Mn], [Ti], and [Al] represent the contents (weight %) of the respective elements in parentheses with respect to the weld metal.

[0021] The weld metal may contain Si in the range of 0.05-0.15%.

[0022] The weld metal may further include one or more of Nb: 0.10% or less, V: 0.10% or less, and Zr: 0.10% or less.

[0023] The weld metal may further contain B: 0.01% or less.

[0024] The weld metal may satisfy a length fraction of porosity defects of 10% or less and including 0% relative to a total length of the weld metal.

[0025] The welding base material may be a hot-dip galvanized steel plate having a hot-dip galvanized layer formed on the surface.

[0026] In terms of weight %, the welding base material may include C: 0.04-0.18%, Si: 2.0% or less and including 0%, Mn: 0.5-3.0%, Cr: 2.0% or less and including 0%, Mo: 2.0% or less and including 0%, Al: 0.01-0.1%, P: 0.05% or less and excluding 0%, S: 0.05% or less and excluding 0%, and the balance of Fe and other inevitable impurities.

[0027] The welding base material may further contain one or more of Ti: 0.20% or less, Nb: 0.10% or less, and Cu: 0.10% or less.

[0028] The welding base material may have a thickness of 0.8 to 4.0 mm.

[0029] In another aspect, the present invention relates to an automobile component including the weld metal.

[0030] Beneficial Effects

[0031] According to the present invention described above, as a next-generation welding technology that ensures performance and cost competitiveness in sync with the era of widespread electric vehicles, it is possible to effectively provide gas shielded arc welding weld metal that is excellent in weld strength and porosity resistance. DETAILED DESCRIPTION

[0032] The present invention is described below.

[0033] Since zinc vapor is generated when welding galvanized steel sheets, there is a problem of pore defects in the weld. At this time, if the content of deoxidizer Si in the weld metal component is reduced to a certain level or more, the viscosity of the molten metal is reduced, the discharge of zinc vapor becomes smoother, and the O generated by the dissociation of CO2 in the shielding gas at high temperature during welding reacts more actively with the Zn in the coating to form Zn-based oxides, so the zinc vapor pressure can be effectively reduced, the arc is stable, and the generation of pore defects can be suppressed. However, the research results of the inventors show that when the content of strong deoxidizers Ti or Al in the weld metal component is above a certain level, it will interfere with the oxidation reaction of the Zn, and even if the Si content is low, it will lead to arc instability, increased pore defects and decreased weld strength. In particular, if the Ti+Al value is 0.07% or more, the pore defects increase significantly, and it is confirmed that the deposited metal with excellent weld strength and pore resistance cannot be ensured.

[0034] Therefore, the weld metal obtained by gas shielded arc welding of the welding base material of the present invention contains, in terms of weight%, C: 0.001-0.30%, Si: 0.25% or less and excluding 0%, Mn: 0.50-3.00%, P: 0.030% or less and excluding 0%, S: 0.030% or less and excluding 0%, Cr: 0.50% or less and excluding 0%, Mo: 0.60% or less and excluding 0%, Al: less than 0.07% and excluding 0%, Ni: 0.40% or less and excluding 0%, Cu: 0.50% or less and excluding 0%, Ti: less than 0.07% and excluding 0%, the balance of Fe and other inevitable impurities, and satisfies the following Relationships 1 and 2.

[0035] [Equation 1]

[0036] 3.5≤[Si]×100 / [Mn]≤8.5

[0037] [Equation 2]

[0038] [Ti]+[Al]<0.07

[0039] Hereinafter, a weld metal of a gas shielded arc welding according to an embodiment of the present invention will be described. First, the reasons for adding each component in the weld metal of the present invention and the reasons for limiting the content will be described in detail. It should be noted that, unless otherwise specified, the content of each component described below is based on weight %.

[0040] C:0.001~0.30%

[0041] The C is a main element, which can reduce the starting temperature of the acicular ferrite, bainite and martensite phase transformation based on non-diffusion phase transformation according to the continuous cooling in the high-temperature austenite phase during the solidification process of the weld metal. If the C content is less than 0.001%, the hardening performance is reduced, not only it is difficult to ensure the sufficient strength of the weld metal, but also due to the above-mentioned principle, the starting temperature of the low-temperature phase transformation will not be sufficiently reduced, so the tensile residual stress offset effect of the weld based on the low-temperature phase transformation expansion effect during the cooling process will be significantly reduced, and there may be a disadvantage of not being able to form a large-angle grain boundary structure with a large orientation angle difference between grains. On the other hand, if the C content is greater than 0.30%, the viscosity of the molten metal is reduced, not only the weld shape becomes poor, but also it will cause the weld metal to be over-hardened, and there may be a disadvantage of reduced toughness.

[0042] Si: 0.25% or less and excluding 0%

[0043] The Si is an element that promotes deoxidation of the molten metal during arc welding (deoxidation element), which is beneficial to suppress the generation of pores and increase the starting temperature of low-temperature phase transformation. However, when welding galvanized steel sheets, the oxidation of Zn and the reduction of zinc vapor pressure are promoted by reducing the Si content in the weld metal composition, thereby preventing the generation of pore defects in the weld. On the other hand, if the Si content is greater than 0.25%, a lot of non-conductive slag is generated, resulting in poor painting of the weld, and due to excessive deoxidation, the surface activation of the weld is insufficient, which may result in a disadvantage of reduced penetration of the molten metal. Therefore, in the present invention, it is preferred to control the Si content to less than 0.25%.

[0044] More preferably, the Si content is controlled within a range of 0.05 to 0.15%. If the Si content is too low, the deoxidation effect is insufficient and pores may be easily generated.

[0045] Mn: 0.5~3.0%

[0046] The Mn is a deoxidizing element, which promotes the deoxidation of the molten metal during arc welding, helps to suppress the generation of pores, and reduces the low-temperature phase transformation start temperature like C. If the Mn content is less than 0.5%, the deoxidation effect is insufficient, and there may be a disadvantage of easily generating pores. However, if the Mn content in the weld metal component is too high when welding galvanized steel sheets, the oxidation of Zn is hindered, and the zinc vapor pressure is increased, which may cause arc instability and promote the generation of pore defects in the weld. On the other hand, if the Mn content is greater than 3.0%, the viscosity of the molten metal becomes too high, and when the welding speed is fast, the molten metal cannot flow into the welding part properly, and there may be a disadvantage of easily generating a poor weld shape due to the formation of a humping weld. More preferably, the Mn content is limited to 2.50% or less.

[0047] Cr: 0.50% or less and 0% or less

[0048] The Cr is a ferrite stabilizing element that lowers the low temperature transformation start temperature and is useful for improving the strength by ensuring the hardenability of the weld metal. If the Cr content is greater than 0.50%, the brittleness of the weld metal may increase unnecessarily in some cases, and there may be a disadvantage that it is difficult to ensure sufficient toughness. The Cr content is more preferably 0.30% or less, further preferably 0.20% or less, and most preferably 0.10% or less.

[0049] Mo: 0.60% or less and excluding 0%

[0050] Mo is a ferrite stabilizing element and is useful for ensuring hardening properties that improve the strength of the weld metal. If the content of Mo is greater than 0.60%, there may be a disadvantage that the toughness of the weld metal decreases in some cases.

[0051] P: 0.030% or less and excluding 0%

[0052] P is an element that is usually mixed as an inevitable impurity in steel and is also an element that is generally contained as an impurity in solid wire for arc welding. If the content of P is greater than 0.030%, there may be a disadvantage that high temperature cracking of the weld metal becomes apparent.

[0053] S: 0.030% or less and excluding 0%

[0054] The S is an element that is usually mixed as an inevitable impurity in steel, and is also an element contained as a regular impurity in solid wire for arc welding. If the S content is more than 0.030%, the toughness of the weld metal deteriorates in some cases, the surface tension of the molten metal is insufficient during welding, and the molten part flows out excessively due to gravity during rapid vertical welding (welding from top to bottom in vertical welding), which may cause the weld bead shape to become poor.

[0055] Al: less than 0.07% and excluding 0%

[0056] The Al is a deoxidizing element, and even in a trace amount, it can promote the deoxidation of the molten metal during arc welding, thereby improving the strength of the weld metal. In order to ensure the above-mentioned effect, 0% is excluded as the lower limit of the Al content. However, due to the deoxidizing effect of Al, when welding galvanized steel sheets, it will interfere with the oxidation reaction of Zn, which may promote the generation of porosity defects in the weld due to increased zinc vapor pressure and arc instability. If the Al content is 0.07% or more, the generation of Al-based oxides increases, and in some cases the strength and toughness of the weld metal decrease, and there may be a disadvantage that the weld becomes sensitive to poor electroplating caused by non-conductive oxides.

[0057] Ti: less than 0.07% and excluding 0%

[0058] The Ti is a deoxidizing element, and even in a trace amount, it can promote the deoxidation of the molten metal during arc welding, thereby improving the strength of the weld metal. In addition, it can promote the development of acicular ferrite that can improve the toughness of the weld. In order to ensure the above-mentioned effects, 0% is excluded as the lower limit of the Ti content. However, due to the deoxidizing effect of Ti, when welding galvanized steel sheets, it will interfere with the oxidation reaction of Zn, and may promote the generation of porosity defects in the weld caused by increased zinc vapor pressure and arc instability. If the Ti content is 0.07% or more, the generation of Ti-based oxides increases, and there may be a disadvantage that the strength and toughness of the weld metal decrease in some cases.

[0059] Ni: 0.40% or less and excluding 0%

[0060] The Ni is an element that can improve the strength and toughness of the weld metal. In order to ensure the above-mentioned effects, the lower limit of the Ni content is 0%. However, if the Ni content is greater than 0.40%, there may be a disadvantage of being sensitive to cracking, so the Ni content is set to 0.40% or less. The Ni content is more preferably 0.30% or less, further preferably 0.20% or less, and most preferably 0.10% or less.

[0061] Cu: 0.50% or less and excluding 0%

[0062] The Cu is an element that effectively improves the strength of the weld metal. However, if the Cu content is greater than 0.50%, there may be a disadvantage that the crack sensitivity of the weld metal becomes high. The Cu content is more preferably 0.45% or less, further preferably 0.40% or less, and most preferably 0.30% or less. On the other hand, in order to fully obtain the effect of improving the strength, the weld metal may contain 0.01% or more of the Cu.

[0063] In addition, the weld metal of the present invention may further optionally contain one or more of Nb: 0.10% or less, V: 0.10% or less, and Zr: 0.10% or less.

[0064] Nb: 0.10% or less

[0065] The Nb is an element that can improve the strength and toughness of the weld metal by improving the hardenability and making the microstructure dense. In addition, it has the effect of improving the flow of molten metal and stabilizing the arc during arc welding. In order to ensure the above effects, the lower limit of the Nb content is 0%. However, if the Nb content is greater than 0.10%, a low melting point compound is formed at the grain boundary, which may cause high temperature cracking.

[0066] V: 0.10% or less

[0067] The V is an element that can improve the strength and toughness of the weld metal by improving the hardenability and making the microstructure dense. In addition, the V is a precipitation strengthening element that can improve the strength of the weld metal by generating carbonitrides. However, if the V content is greater than 0.10%, there may be a disadvantage that the toughness of the weld metal decreases in some cases due to excessive strength caused by excessive precipitates. Therefore, the V content is set to 0.10% or less.

[0068] Zr: 0.10% or less

[0069] The Zr is an element that promotes deoxidation of molten metal during arc welding (deoxidizing element), and is helpful in suppressing the generation of pores. However, if the content of the Zr is greater than 0.10%, there may be a disadvantage that the electroplating property of the welded part is reduced. Therefore, the Zr content is set to 0.10% or less.

[0070] Furthermore, optionally, the weld metal of the present invention may further contain B: 0.01% or less.

[0071] B: 0.01% or less

[0072] B is an element that improves the strength of the weld metal by improving the hardenability. However, if the content of B is greater than 0.01%, the toughness of the weld metal may decrease in some cases due to excessive hardenability. Therefore, the B content is set to 0.01% or less.

[0073] In addition, the remaining component of the present invention is iron (Fe). However, unexpected impurities are inevitably mixed into the raw materials or the surrounding environment during the conventional manufacturing process, so the mixing of impurities is not excluded. The impurities are impurities known to any ordinary technician, so all relevant contents are not specifically mentioned in the present invention.

[0074] On the other hand, the weld metal of the present invention contains Mn and Si so as to satisfy the following relational expression 1. By satisfying the following relational expression 1, the strength and porosity resistance of the above-mentioned weld metal can be improved. If the value defined by the relational expression 1 is less than 3.5, the deoxidation effect of the weld metal is insufficient, and thus the porosity resistance is reduced, resulting in insufficient strength. If the value defined by the relational expression 1 is greater than 8.5, not only the viscosity of the weld metal increases, but also the zinc vapor pressure increases during welding due to the above-mentioned principle, thereby causing arc instability and porosity resistance to decrease, resulting in insufficient strength. At the same time, due to the increase of Si-based non-conductive oxides, the problem of poor electrocoatability may occur. More preferably, the upper limit of the value defined by the relational expression 1 is controlled to 6.0.

[0075] [Equation 1]

[0076] 3.5≤[Si]×100 / [Mn]≤8.5

[0077] In the above relational expression 1, [Si] and [Mn] represent the contents (weight %) of the respective elements in parentheses with respect to the weld metal.

[0078] Furthermore, the weld metal of the present invention is required to contain Ti and Al so as to satisfy the following Relationship 2.

[0079] Since zinc vapor is generated when welding galvanized steel sheets, porosity defects will occur in the weld. At this time, if the content of deoxidizer Si in the weld metal composition is reduced to a certain level or more, the viscosity of the molten metal will decrease, the discharge of zinc vapor will become smoother, and the O (oxygen) generated by the dissociation of CO2 in the shielding gas at high temperature during welding will react more actively with the Zn in the coating to form Zn-based oxides, so the zinc vapor pressure can be effectively reduced, the arc can be stabilized, and the generation of porosity defects can be suppressed. However, when the content of strong deoxidizers Ti or Al in the weld metal composition is above a certain level, it will interfere with the oxidation reaction of the Zn, and even if the Si content is low, it will lead to arc instability, increased porosity defects and decreased weld strength. In particular, if the Ti+Al value is 0.07% or more, the porosity defects will increase significantly, making it impossible to ensure excellent weld strength and porosity-resistant deposited metal.

[0080] In more detail, the affinity of metals for oxygen, i.e., the thermodynamic stability of each metal element when combined with oxygen at a certain temperature, can be easily determined by the well-known Ellingham diagram. In the order of Al>Ti>Si>Zn, the Gibbs free energy decreases, making it easier to combine with oxygen, and thus the stability of the oxide increases. On the other hand, the temperature at which each of the above metal elements begins to combine with oxygen, i.e., the boiling point, is Al2O3: 2977°C, TiO2: 2972°C, SiO2: 2230°C, and ZnO: 2360°C. Compared with Si and Zn, Al and Ti are more likely to thermodynamically combine with oxygen first at high temperatures. Therefore, in the process of slowly cooling and solidifying the weld metal melted at the center temperature of the arc (i.e., about 3000 to 5000°C) during welding, the Si content decreases and Zn is more likely to combine with O. As the content of Al and Ti increases, they are oxidized before Zn, and thus the weld part porosity defects caused by the increase in Zn vapor pressure may also be more sensitive.

[0081] [Equation 2]

[0082] [Ti]+[Al]<0.07

[0083] In the above relational expression 2, [Ti] and [Al] represent the contents (weight %) of the respective elements in parentheses with respect to the weld metal.

[0084] In addition, in the present invention, the weld metal may satisfy a length fraction of pore defects of 10% or less and including 0% relative to the total length of the weld metal. Therefore, the present invention can effectively provide parts such as automobile parts having a welded portion with excellent pore resistance.

[0085] In addition, in the present invention, as the welding base material for forming the weld metal, a hot-dip galvanized steel sheet having a hot-dip galvanized layer formed on the surface can be used, the thickness of the hot-dip galvanized layer is 1 to 20 μm, and the single-sided coating amount is preferably 1 to 120 g / m 2 .

[0086] In addition, in the present invention, the alloy composition of the welding base material is not limited. As an example, the welding base material may include, in terms of weight%, C: 0.04-0.18%, Si: 2.0% or less and 0%, Mn: 0.5-3.0%, Cr: 2.0% or less and 0%, Mo: 2.0% or less and 0%, Al: 0.01-0.1%, P: 0.05% or less and 0% excluded, S: 0.05% or less and 0% excluded, and the balance of Fe and other inevitable impurities.

[0087] Optionally, the welding base material may further include one or more of Ti: 0.2% or less, Nb: 0.1% or less, and Cu: 0.1% or less.

[0088] Meanwhile, the welding base material may have a thickness of 0.8 to 4.0 mm.

[0089] In addition, in the present invention, the specific composition of the welding wire used to form the weld metal is not limited. As an example, a solid welding wire can be used, which contains, by weight%, C: 0.001-0.30%, Si: 0.25% or less and excluding 0%, Mn: 0.50-3.00%, P: 0.030% or less and excluding 0%, S: 0.030% or less and excluding 0%, Cr: 1.50% or less and excluding 0%, Mo: 0.60% or less and excluding 0%, Al: less than 0.10% and excluding 0%, Ni: 0.40% or less and excluding 0%, Cu: 0.50% or less and excluding 0%, Ti: less than 0.10% and excluding 0%, and the balance of Fe and other inevitable impurities. In addition, optionally, the welding wire composition may further include one or more of Nb: 0.10% or less, V: 0.10% or less, and Zr: 0.10% or less, or further include B: 0.01% or less.

[0090] On the other hand, in the present invention, the type of shielding gas used in the welding of the welding base material is not particularly limited. As the shielding gas, 100% CO2 gas, Ar+20CO2 gas, Ar+10%CO2 gas, Ar+5%CO2 gas, Ar+2%O2 gas, etc. can be used. However, when Ar+5-20%CO2 is used as the shielding gas, the significant effect of the present invention can be exerted. That is, in the present invention, in order to ensure the tensile strength of the welded part without the occurrence of weld metal or fuse rupture, it is preferred that 5-20%CO2 is mixed in Ar as the shielding gas during the welding.

[0091] Modes for Carrying Out the Invention

[0092] Hereinafter, the present invention is further described in detail by examples. However, it should be noted that the following examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. Because the scope of the present invention depends on the contents recorded in the claims and the contents reasonably derived therefrom.

[0093] (Example)

[0094] Two sheets of three kinds of hot-dip galvanized steel sheet base materials with tensile strength of 540 MPa (steel material 1), 670 MPa (steel material 2) and 780 MPa (steel material 3) were prepared respectively. These base materials had the alloy composition shown in Table 1 below, thickness of 2.0 mm, length of 200 mm, width of 150 mm and single-sided coating amount of 85 g / m 2 In addition, a variety of solid wires for gas shielded arc welding having various alloy compositions are prepared.

[0095] Next, the hot-dip galvanized steel sheets were overlapped using the solid welding wires. At this time, pulse current (Pulse DC) (shielding gas: Ar+10-20% CO2) was used as the welding method, and the shielding gas flow rate was 20 l / min. The angle of the welding torch was 45° relative to the vertical direction of the base material, the protruding length of the welding wire was 15 mm, and the welding current / voltage / speed conditions were 200A-20V-80cm / min. In addition, the overlap gap (Gap) was 0 mm and the overlap length was 10 mm.

[0096] On the other hand, welding was started at a position 10 mm from the starting point in the longitudinal direction of the welding base material, the welding length was 180 mm, and then welding was ended at a position 10 mm from the end point on the opposite side of the welding starting position.

[0097] For each weld formed by the welding, the microstructure of the cross section perpendicular to the longitudinal direction at the center of the longitudinal direction of the weld was observed with an optical microscope to confirm the area of ​​the weld metal in advance, and the area was cut into a fine chip shape. Next, for each chip sample, the chemical composition of the weld metal was measured by emission spectrometry based on high-frequency inductively coupled plasma (ICP), and the results are shown in Table 2 below.

[0098] In addition, the porosity of each weld formed by the welding was measured, and the results are shown in Table 3 below. At this time, the specific method of measuring the porosity is as follows: the prepared welding sample is irradiated with X-rays to measure the length of each pore distributed in the weld, and the total sum of the lengths of each pore is divided by the total length of the weld to calculate the porosity of the weld. At this time, the 10 mm section at the start and end of the weld is excluded from the measurement, and the porosity is the average value of the measured values ​​for the three welding samples.

[0099] In addition, a tensile test is performed on the formed welded portion, and the position where the fracture occurs is visually observed. At this time, if the weld base material or the heat-affected zone is fractured, it is evaluated as qualified (O), and if the weld metal is fractured, it is evaluated as unqualified (X). In addition, the specific tensile test method at this time is as follows: Each welded sample is processed into a tensile sample with a width of 30 mm and a length of 250 mm, and a uniaxial tensile test is performed at a speed of 10 mm / min, and the fracture position is checked. At this time, the reproducibility of the tensile test results is verified by evaluating 3 welded samples.

[0100]

Table 1

[0101]

[0102] *The balance in Table 1 is Fe and unavoidable impurities

[0103]

Table 2

[0104]

[0105]

[0106] *The balance in Table 2 is Fe and unavoidable impurities

[0107]

Table 3

[0108]

[0109]

[0110] As shown in Table 1-3 above, for Invention Example 1-15 in which both the weld metal alloy composition and Relationship 1-2 are satisfied, the length fraction of the porosity defects relative to the total length of the weld metal is less than 10% and includes 0%, and the fracture position of the weld is also the weld base material or the heat-affected zone, which shows that the performance is excellent.

[0111] In contrast, Comparative Examples 1, 11 and Comparative Examples 4-5, 14-15 and 21-30 are situations where Relationship 1-2 is beyond the scope of the present invention, and show higher weld porosity under any one of the shielding gases or higher weld porosity under all of the shielding gases. The results confirm that the fracture position of the weld also appears in the weld metal.

[0112] In addition, Comparative Examples 2-3, 9-10, 12-13 and 19-20 do not satisfy Relationship 2, and show higher weld porosity under any one of the shielding gases or all of the shielding gases, resulting in the weld fracture position also appearing in the weld metal.

[0113] In addition, Comparative Examples 6-8 and Comparative Examples 16-18 do not satisfy Relational Expression 1, and exhibit high weld porosity under all shielding gases. As a result, it can be confirmed that the weld fracture position also appears in the weld metal.

Claims

1. A weld metal for gas shielded arc welding, wherein: The weld metal is a weld metal obtained by gas shielded arc welding of a welding base material, and contains, in weight%, C: 0.001-0.30%, Si: 0.25% or less and excluding 0%, Mn: 0.50-3.00%, P: 0.030% or less and excluding 0%, S: 0.030% or less and excluding 0%, Cr: 0.50% or less and excluding 0%, Mo: 0.60% or less and excluding 0%, Al: less than 0.07% and excluding 0%, Ni: 0.40% or less and excluding 0%, Cu: 0.50% or less and excluding 0%, Ti: less than 0.07% and excluding 0%, and the balance of Fe and other inevitable impurities, and satisfies the following Relationships 1 and 2, [Equation 1] 3.5≤[Si]×100 / [Mn]≤8.5 [Equation 2] [Ti]+[Al]<0.07 In the above-mentioned Relational Formulas 1 and 2, [Si], [Mn], [Ti], and [Al] represent the contents of the respective elements in parentheses in the weld metal in terms of weight %.

2. The weld metal of gas shielded arc welding according to claim 1, wherein: The weld metal contains Si in the range of 0.05-0.15%.

3. The weld metal of gas shielded arc welding according to claim 1, wherein: The weld metal further contains one or more of Nb: 0.10% or less, V: 0.10% or less, and Zr: 0.10% or less.

4. The weld metal of gas shielded arc welding according to claim 1, wherein: The weld metal further contains B: 0.01% or less.

5. The weld metal of gas shielded arc welding according to claim 1, wherein: The weld metal satisfies that a length fraction of porosity defects relative to a total length of the weld metal is 10% or less and includes 0%.

6. The weld metal of gas shielded arc welding according to claim 1, wherein: The welding base material is a hot-dip galvanized steel plate with a hot-dip galvanized layer formed on the surface.

7. The weld metal of gas shielded arc welding according to claim 1, wherein: In terms of weight %, the welding base material includes C: 0.04-0.18%, Si: 2.0% or less and including 0%, Mn: 0.5-3.0%, Cr: 2.0% or less and including 0%, Mo: 2.0% or less and including 0%, Al: 0.01-0.1%, P: 0.05% or less and excluding 0%, S: 0.05% or less and excluding 0%, and the balance Fe and other inevitable impurities.

8. The weld metal of gas shielded arc welding according to claim 7, wherein: The welding base material further contains one or more of Ti: 0.20% or less, Nb: 0.10% or less, and Cu: 0.10% or less.

9. The weld metal of gas shielded arc welding according to claim 1, wherein: The welding base material has a thickness of 0.8 to 4.0 mm. 10 . An automobile component comprising the weld metal according to claim 1 .