Method of manufacturing carpet product and product obtainable using method
By using high-weight and high-twist polyester yarns combined with melt bonding technology, the problems of insufficient wear resistance and recyclability of polyester carpet products are solved, and the durability and environmental friendliness of carpet products for high-end commercial purposes are achieved. .
Patent Information
- Application Number
- CN202380024143.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-28
- Filing Date
- 2023-02-24
- Publication Date
- 2024-10-15
AI Technical Summary
It is difficult to manufacture polyester carpet products suitable for commercial use with existing technology. Polyester yarns have insufficient abrasion resistance and are not environmentally friendly, making it difficult to meet the durability and recycling requirements of high-end commercial uses.
Using high weight (at least 2500Dtex) and high twist (at least 100tpm) polyester yarns, the yarns are locked to the primary backing through melt bonding technology to form carpet products, and hot melt adhesives are used during processing to enhance Durability and dimensional stability.
It has realized carpet products that meet the European standard EN 1307:2014+A3:2019 for mid-to-high-end commercial use, improves durability and recyclability, reduces production costs, and is suitable for commercial applications.
Smart Images

Figure BDA0005014970670000131 
Figure BDA0005014970670000141 
Figure BDA0005014970670000142
Abstract
Description
[0001] General Field of the Invention
[0002] The present invention relates to a method for manufacturing a carpet product, the method generally comprising providing a sheet having a front surface and a back surface as a primary backing, and sewing one or more yarns through the first sheet so as to form a pile on the front surface of the primary backing. At the back surface, the one or more yarns are locked to the primary backing, typically by applying latex or other adhesive. In particular, the present invention relates to a method for producing a carpet product suitable for commercial use, i.e. a product of class 31 (medium commercial use), class 32 (normal commercial use) or class 33 (heavy commercial use) according to European standard EN 1307:2014+A3:2019 (including the Vetterman test according to ISO 10361:2015). The present invention also relates to a carpet product obtainable with the manufacturing method according to the present invention. Background of the Invention
[0004] In today's world, carpets are used for a variety of purposes. An important reason for using carpet products is aesthetics. Other purposes are (walking) comfort, noise attenuation and hygiene. However, factors that need to be considered when manufacturing carpet products for specific purposes also include the weight of the carpet product, the cost of the product, the feel (or "hand") of the product, and, importantly, durability. High-end carpet products are usually tufted structures. Tufted carpet products usually include a composite structure in which tufts or carpet fiber bundles are introduced (such as by sewing) into a primary backing, such as a woven or non-woven fabric. These carpet fibers are usually yarns composed of nylon, polyester, wool or polypropylene, of which nylon is the most common. A secondary backing or coating of a thermoplastic material is then usually applied to the underside of the carpet construction in order to firmly hold the tufted material in the primary backing. This secondary backing not only stabilizes the carpet product dimensionally, but also provides greater resistance to abrasion and wear, and can serve as a basis for adhering additional material layers. Tufted nylon carpets have excellent wear resistance and are therefore generally preferred in commercial applications (e.g., in stores, hotels, conference centers, restaurants, offices, cars, terminals, trains, airplanes, elevators, and entrance areas), where polyester carpet products are less wear resistant. However, nylon has some disadvantages. In addition to being relatively expensive, it is not easily recyclable (it requires chemical recycling) and is more sensitive to dyeing. Moreover, the dimensional stability is not optimal. In this regard, polyester, particularly polyethylene terephthalate (PET), appears to be a better alternative, being relatively cheap, easily recyclable, having natural stain resistance, and potentially better dimensional stability. However, the wear resistance of carpets made from polyester yarns is so low that a product suitable for commercial use cannot be obtained. Polyester carpets are thus mainly used in household applications.
[0005] In the art, several attempts have been made to obtain carpet products using polyester yarns with improved durability. For example, US2020 / 0190718 (assigned to Invista North America SARL, Wilmington, USA) discloses a carpet with self-twisting loop pile, which has an appearance and aesthetics similar to cut pile carpet products, but with improved durability. To this end, the carpet product includes a single yarn (so-called single-strand yarn) twisted with a higher twist than commonly used, which is sewn through a pre-built woven or non-woven fabric backing to form a loop pile or tuft. Due to the high twist, the loop pile is automatically twisted. It is described that the single-strand yarn is twisted in the range of 1 to 15 twists / inch (tpi), which is equal to 40-600tpm (twists / meter), especially 200-400tpm. The single yarn is directly tufted into the carpet without the need for a yarn heat setting step. Although PET carpets pass the Vetterman test in this respect for a high-quality carpet product, the disadvantage of the high twist level is that the tuft bond strength is relatively low, so that the overall durability is still lower than that required for (high-end) commercial use. In addition, the self-twisted single-ply yarns provide an appearance that is not popular in all markets.
[0006] WO96 / 35836 (assigned to 3M, Saint Paul, USA) describes a carpet product that can withstand a large amount of pedestrian traffic and can be used to be placed at the entrance of a building, such as for wiping wet and / or dirty soles. It is described that polyester yarn can be used to make the carpet product. The product includes a pile layer of tufted bundles of textured synthetic resin filaments, each filament having a linear density of at least 800 deniers, and the filaments in each tufted bundle are arranged in loops of random shape and orientation and intermingled with the loops in the adjacent filament tufted bundles in the pile layer. When measured outward from the substrate surface, the pile layer has a thickness of at least 5mm and preferably 5mm to 15mm. In this way, a heavy carpet product is produced that has the ability to retain dirt and has sufficient resilience and durability to withstand pedestrian traffic without significant degradation. This makes the product very suitable for outdoor mats or carpets. However, the high pile prevents the product from maintaining its initial aesthetic appearance, which is not suitable for high-end indoor applications.
[0007] CN 10228619 discloses a high-end household colored glossy and resilient fine denier carpet and a manufacturing method. The carpet uses a yarn with a relatively high weight (DTex above 2400) and a twist of about 50-130 tpm. The combination of high weight yarn and high twist provides good appearance and resilience. However, the durability is too low to meet the requirements of commercial applications.
[0008] US2008 / 0220200 (assigned to Futuris Automotive Interiors Inc., Troy, USA) discloses a PET carpet product suitable as a carpet for the interior of an automobile. To this end, a tufted PET carpet product is described, comprising a pile of PET yarns composed of PET fibers and tufted to a first backing layer at a predetermined specification, the pile layer having a specific surface weight, an adhesive back coating adjacent to the first backing layer, and a cushioning layer adjacent to the second backing layer. The backing adhesive is applied using an extrusion process to lock the tufted PET to the backing, and steam is applied to the tufted PET to enhance the look and feel of the PET. This makes the product suitable for use in automobiles. However, the process is quite complex, making the product relatively expensive.
[0009] US2016 / 0136844 (assigned to Milliken & Company, Spartanburg, USA) discloses a 100% polyester fully recyclable carpet that uses a very high viscosity polyester adhesive to securely bond the tufted yarns. However, the fuzz resistance is still relatively low (Velcro roll fuzz resistance is 2 or less). At higher fuzz resistance (4), there is no adhesive left to bond the secondary backing. This makes the carpet less attractive for high-end uses.
[0010] Purpose of the Invention
[0011] The object of the present invention is to provide an improved method for manufacturing a carpet product which is easily recyclable but suitable for commercial use, in particular meeting at least class 31, preferably class 32 or 33 of European standard EN 1307:2014+A3:2019. Another object is to provide such a carpet product. SUMMARY OF THE INVENTION
[0013] In order to meet the purpose of the present invention, a method for manufacturing a carpet product is made, which includes providing a first sheet having a front surface and a back surface (the sheet is usually called a primary backing), providing one or more fibers having a Dtex of at least 2500 (e.g., at least 2500, 2550, 2600, 2650, 2700, 2750, 2800, 2850, 2900, 2950, 3000, 3050, 3100, 3150, 3200, 3250, 3300, 3350, 3400, 3450, 3460, 3470, 3480, 3490, 3500, 3600, 3690, 3700, 3710, 3720, 3730, 3740, 3750, 3760, 3770, 3780, 3790, 3800, 3810, 3820, 3830, 3840, 3850, 3860, 3870, 3880 00、3450、3500、3550、3600、3650、3700、3750、3800、3850、3900、3950、4000、4100、4200、4300、4400、4500、4600、47004800、4900、5000、5100、5200、5300、5400、5500、5600、5700、5800、5900、6000、6100、6200、6300、 6400, 6500, 6600, 6700, 6800, 6900, at least 7000 or even higher) and a twist of at least 100 tpm (e.g., at least 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 220, 230, 240, 250, 260, 270, 280, 290, at least 300 or even higher), and a polyester yarn having a weight of at least 100 tpm (e.g., at least 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 220, 230, 240, 250, 260, 270, 280, 290, at least 300 or even higher) and a polyester yarn having a twist ... A pile is formed on the front surface of a sheet of material, and the one or more yarns have free ends forming the pile and locking ends present at the back surface of the first sheet of material, thereby forming an intermediate product, and the intermediate product is processed by feeding the product along a body having a heated surface, the back surface being in contact with the heated surface to melt at least a portion of the polyester of the locking ends of the one or more yarns, and cooling the molten portion of the polyester to solidify the molten portion of the polyester, thereby connecting the locking ends of the one or more yarns to the first sheet of material and forming a carpet product.
[0014] As is well known in the art, polyester yarns are inherently easy to recycle. Mechanical recycling is an option and is one of many known chemical recycling processes, such as those used to recycle polyester bottles (for example, as disclosed in WO 2022 / 003084, assigned to CureTechnology BV). By combining the relatively high weight (also expressed as "count" or "fineness") of the polyester yarn (above 2500 dtex) with a relatively high twist level (above 100 tpm) and a method of connecting the yarn on the back of the primary backing by melting rather than using a coating such as latex, the durability requirements that meet commercial standards are surprisingly met. Such methods for connecting polymer yarns to primary backings are themselves known in the art, for example from WO 2012 / 076348 (assigned to Niaga BV), but have not been combined with other features to obtain a product that meets the requirements of high-end commercial use. It appears that when using polyester yarns, when these three technical features are combined (particularly Dtex level, twist and bonding of the yarn by fusion), the objectives of the present invention can be met, in particular being able to provide a carpet product that meets at least Class 31 of European Standard EN 1307:2014+A3:2019, and even Class 32 or 33, depending on (other) characteristics of the carpet product.
[0015] Although it is not entirely clear why the combination of these features provides the desired effect for carpet products using polyester yarns, it is believed that high twist at least partially compensates for the lack of inherent resilience of polyester yarns. The relatively high Dtex value in turn seems to be able to compensate for the loss of bulk due to high twist. Importantly, the applicant recognizes that high twist is usually disadvantageous for achieving appropriate filament bonding levels. This may be due to the fact that the adhesive may not penetrate into the yarn very effectively. However, the melting and cooling characteristics of the back-bonded yarn as used in this manufacturing method do not have this disadvantage. On the contrary, the higher the density of the yarn, the better the heat conduction, so that the melting process can occur better.
[0016] Although it has been found that meeting the Dtex and tpm values as described above can provide carpet products suitable for (high) end commercial use, it is particularly preferred that the tpm level (at a Dtex value of more than 2500) and the weight value of the yarn meet the following relationship:
[0017]
[0018] If the tpm level is indeed higher than the value according to the formula (60000 / (Dtex-2500)+100), the combination of relatively low tpm and low Dtex values (in the present invention) can be avoided, allowing greater freedom for other characteristics of the carpet product such as stitch gauge (the distance between needles per inch), weave gauge (the number of stitches per inch over the length of the carpet product), pile height, number of filaments in the yarn, number of strands in the yarn, dpf, etc.
[0019] According to the method as described herein, the present invention also relates to a carpet product comprising a first sheet having a front surface and a back surface and one or more polyester yarns sewn through the first sheet to form a pile on the front surface of the sheet, the yarn having a weight of at least 2500 Dtex and a twist of at least 100 tpm, wherein at least a portion of the polyester at the locked ends of the one or more yarns is melted, spread on the back surface of the sheet and solidified.
[0020] definition
[0021] Yarn is a single textile thread or thread that can be used in the sewing process. Typically, a yarn consists of a bundle of twisted fiber strands, which in turn consists of a bundle of entangled filaments.
[0022] A multi-ply yarn is a yarn consisting of multiple strands twisted together as one yarn. For example, a three-ply yarn consists of three single strands twisted together.
[0023] A polyester product is a product which consists of at least more than 50% by mass, preferably at least 55, 60, 65, 70, 75, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99 to 100% by mass of polyester polymer.
[0024] Polyesters are a class of polymers that contain ester functional groups in each repeating unit of their backbone chain ( H, Schmidt M, Brügging W, Rüter J, Kaminsky W (June 2000). "Polyesters". Ullmann's Encyclopedia of Industrial Chemistry. Weinheim, Germany: Wiley-VCH Verlag GmbH & Co. KGaA.). Examples of polyesters are polycaprolactone (PCL), polylactic acid (PLA), polyhydroxybutyrate (PHB), polyglycolic acid (PGA), polyethylene adipate (PEA), polyethylene terephthalate (PET; e.g. and ), polybutylene terephthalate (PBT; such as and ), polyethylene naphthalate (PEN), polytrimethylene terephthalate (PTT; such as ), polyester of 4-hydroxybenzoic acid and 6-hydroxynaphthalene-2-carboxylic acid (LCP), polyester of bisphenol A and phthalic acid (PAR).
[0025] Dtex (or dtex) is the mass (weight) of a (single) yarn in grams / 10,000 meters. In the art, this is also expressed as (total) yarn count or titer, and is the total mass of the final yarn after twisting.
[0026] Dpf is the denier per filament, where denier is the weight in grams of 9,000 meters of a single filament.
[0027] The twist of a yarn is the total number of twists present per meter of yarn, that is, the number of bumps per meter of yarn divided by the number of plies (Berka, Amanda (Winter 2007), "Technically Speaking: Twists Per Inch", Spin Off Magazine, Interweave, pp. 11-12).
[0028] A carpet product is a relatively thick textile product used to cover floors or other objects that are walked on, such as the interior of an automobile. Typical carpet products are broadloom carpets, carpet tiles, floor mats and floor mats.
[0029] A sheet is a substance or material that is substantially two-dimensional, ie wide and thin, and usually but not necessarily rectangular.
[0030] Fibrous means consisting essentially of fibers. "Essentially" means that the basic mechanical structure consists of an arrangement of fibers: however, the fibers may be impregnated or otherwise treated or combined with non-fibrous materials so that the final material also includes other components in addition to fibers. Typical fibrous sheets are woven and non-woven textile products, or combinations thereof.
[0031] Sewing is the process of mechanically making yarn parts of an object by stitches or as if with stitches (such as by tufting, knitting, sewing, weaving, etc.).
[0032] A felt layer is a layer in which the individual fibers of a nonwoven are entangled together using mechanical impact and optionally heat and moisture.
[0033] Hot melt adhesives are thermoplastic adhesives designed to melt, i.e., to be heated to undergo a first order phase change from a solid to a liquid state in order to adhere materials after solidification. Hot melt adhesives are generally non-reactive, (at least partially) crystalline, and contain little or no solvent (0-5m%, preferably 0-2m% or even 0-1m%), and therefore generally do not require curing and drying to provide adequate adhesion.
[0034] The intrinsic viscosity is a measure of the contribution of the solute to the viscosity η of the solution, see "Progress in Biophysics and Molecular Biology" (Harding 1997). IV can be measured according to DIN / ISO 1628. Typically, a polymer concentration of 1% is used and meta-cresol is used as solvent, where IV can be expressed in dl / g (usually without the latter dimension). A practical method for determining the intrinsic viscosity is to use an Ubbelohde viscometer.
[0035] Embodiments of the present invention
[0036] In a first embodiment of the method according to the invention, the one or more polyester yarns have a weight of at least 2800 Dtex and a twist of at least 120 tpm. At such Dtex and tpm levels, in combination with a melting step of the yarn at the back, even improved durability properties can be obtained, enabling the manufacture of carpet products meeting classes 32 and 33 (according to European Standard EN 1307:2014+A3:2019). Although it has been found that meeting these Dtex and tpm values enables the provision of carpet products suitable for high-end commercial use, it has been found that it is particularly preferred that the tpm level (at Dtex values above 2800) meets the following relationship to the weight value of the yarn:
[0037]
[0038] If the tpm level is indeed higher than the value according to this formula, the combination of relatively low tpm and low Dtex values (in the above embodiment) can be avoided, allowing greater freedom for other characteristics of the carpet product such as stitch gauge, weave gauge, pile height, number of filaments in the yarn, number of strands in the yarn, dpf, etc.
[0039] In a second embodiment of the method according to the invention, the polyester yarn or yarns have a weight of at least 3000 Dtex and a twist of at least 150 tpm. At such Dtex and tpm levels, combined with a melting step of the yarn at the back, even further improved durability properties can be obtained, enabling the manufacture of carpet products that even meet Class 33 (according to European Standard EN 1307:2014+A3:2019).
[0040] In a further embodiment of the method according to the invention, the first sheet is a polyester sheet. This has the advantage that the product is even easier to recycle, since the yarn and sheet do not need to be separated for recycling and can be processed as a whole, for example by shredding and subsequently melting the shredded product, optionally with subsequent chemical treatment.
[0041] In yet another embodiment, the polyester comprises PET (polyethylene terephthalate) and / or PTT (polytrimethylene terephthalate). It has been found that these types of polyesters (alone or in combination) are particularly suitable for the manufacture of carpet products. PET has the advantage that it is easily available as a recycled material at a low price and still meets high quality standards, enabling it to be used to produce high quality yarns for textile applications, even high-end carpet applications. For this reason, it is preferred that the polyester has an intrinsic viscosity above 0.8 dl / g (which is typical for bottle-grade products of PET). The higher the iv, the better the polymer is for producing high quality yarns and thus high-end carpet products. Furthermore, advantageously, in a carpet product, only one type of polyester is used for both yarn and sheet, and optionally other polymer-containing parts of the product.
[0042] In yet another embodiment of the method according to the invention, one or more yarns are multi-ply yarns, in particular 2, 3 or 4 ply. It has been found that with multi-ply yarns, it is easier to apply higher twists, thereby achieving higher levels of durability in the present invention. Single-ply yarns at high twists (usually above 120) can become self-twisting, which is disadvantageous for many applications.
[0043] In another embodiment of the method according to the invention, one or more yarns are each composed of multiple filaments having a weight of 2 to 40 dpf. This low dpf value can lead to a more comfortable feel while still being able to meet the desired durability requirements. This may be related to the higher flexibility of the filaments. Preferably, the filament weight is 5 to 20 dpf, even more preferably 8 to 12 dpf, such as 8, 9, 10, 11 or 12 dpf.
[0044] In a further embodiment of the method according to the invention, the one or more polyester yarns have a weight of at least 3500 Dtex, preferably at least 4000 Dtex. It has been found that at this weight, the durability can be further improved. For nylon carpet products, such weights are hardly applicable due to commodity costs.
[0045] In yet another embodiment of the method according to the invention, in the step of processing the intermediate product by feeding it along a body having a heated surface, the intermediate product has a relative speed (not zero) relative to the heated surface of the body. In this embodiment, the molten portion of the yarn is spread in a direction parallel to the surface of the first sheet by applying a mechanical force to the molten portion in said direction. The mechanical force can lead to a calendering process, in effect merging the (molten) yarn ends at the back of the intermediate product into one continuous and smooth material layer. This improves the tuft binding and, therefore, the durability properties of the resulting carpet product.
[0046] In another embodiment of the method according to the invention, the method comprises attaching the second sheet to the carpet product using an adhesive applied between the processed back surface of the first sheet and the second sheet. By applying a second sheet, usually referred to as a secondary backing, the dimensional stability of the product can be improved, as well as the (walking) comfort and / or the ease of laying the product.
[0047] Preferably, the adhesive is a hot melt adhesive. Due to its crystalline nature, hot melt adhesives are relatively brittle when cold. Therefore, it is expected that local deformation of the intermediate product will lead to cracking of the adhesive and thus delamination. However, this does not seem to be the case. In a further embodiment, the hot melt adhesive is a polyester adhesive. This is advantageous for recycling carpet products that already contain polyester yarns.
[0048] In another embodiment of the method according to the invention, the second sheet material is a fiber sheet material, preferably a felt sheet material.Most preferably, the second sheet material is a polyester sheet material.
[0049] It should be noted that any of the above-described features of embodiments of the method according to the present invention correspond to embodiments of the resulting carpet product.
[0050] The invention will now be explained in more detail using the following non-limiting examples, which disclose specific embodiments of the invention and comparative examples. Example
[0051] Figure 1 A cross section of a prior art textile product is schematically shown.
[0052] Figure 2 schematically shows Figure 1 Details of the product.
[0053] Figure 3 The configuration for applying the fiber bonding process is shown schematically.
[0054] Figure 4 The lamination configuration is shown schematically.
[0055] Fig. 5 schematically shows a cross section of a textile product according to the invention.
[0056] Example 1 describes various carpet products according to the present invention.
[0057] Example 2 describes various comparative examples.
[0058] Example 3 provides several methods for recycling carpet products according to the present invention.
[0059] Figure 1
[0060] Figure 1 A cross section of a carpet product according to the invention is schematically shown, in this case a carpet tile type 33. The tile comprises a first sheet 2 - the so-called primary backing, Propex Artis True TM , which is a woven PET sheet obtained from PropexFabric GmbH, Gronau, Germany, with a 30 g / m 2 A cap of PET yarn (see Figure 5). A three-lobed PET yarn 5 with a dpf of 30 obtained from Pataga, Peer, Belgium was tufted into the primary backing at a needle gauge of 1 / 10" and a weave gauge of 42. Prior to tufting, the yarn was plied to obtain a 2-ply yarn, twisted to a level of 200 tpm, and then the yarn was heat set to maintain the twist. By plying and twisting the base yarn in this way, the resulting yarn had a Dtex value of 3600. After tufting and cutting, the yarn 5 was extended with its end 7 through the backing and formed a loop on its back surface 4. In this way, the end 7 was locked into the primary backing 2. The free end 6 of the yarn 5 extended from the first surface 3 of the sheet to form a pile thereon. By using a method as described in reference Figure 3 The fiber bonding process described seals the locking end 7 to the second surface 4 of the sheet to mechanically and durably connect the yarn 5 to the primary backing. To provide mechanical stability, the carpet tile 1 includes a second sheet 8, in this case a backing of polyester needle felt backing fleece obtained from VEBE Floor Coverings Genemuiden. The weight of the second sheet is about 900 g / m 2 Optionally, between the first and second sheets is an additional backing layer 10, for example having a thickness of 330 g / m 2 The polyester expanded fleece fabric of 100 g / m2, which is available as an Abstandsvliesstof from TWE, is a non-needled nonwoven fabric. Both sides of the layer 10 consist of a web of 100% PET that has been mechanically coagulated. The thickness of the middle layer is about 4 mm. The layers 11 and 12 are made of a 100% PET web of about 300 g / m2. 2The backings were adhered together with a polyester hot melt adhesive from Covestro, Leverkusen, Germany, applied with a weight of 1000 g. The total weight of the resulting carpet tile (without the optional backing layer 10) was about 2.2 kg / m 2 .
[0061] Figure 2
[0062] Figure 2 schematically shows Figure 1 Details of a product at various stages of manufacture. Figure 2 depicts an intermediate product 100 consisting of a primary backing 2 and yarns 5 tufted therein. As depicted, the locked ends 7 of the yarns 5 form a loop at the back surface 4 of the primary backing. The free ends 6 extend from the front surface 3 of the primary backing. In theory, the yarns 5 can be easily removed from the intermediate product because the yarns are simply sewn into the backing. For example, each yarn can be easily removed from the primary backing by applying a slight pulling force by hand. In order to durably connect the yarns to the primary backing, a fiber bonding process as known from WO2012 / 076348 is applied, reference Figure 3 Further details. In the process, the back side of the intermediate product 100 is dragged along the heating body in contact therewith so as to at least partially melt the loop of the yarn and also to melt some of the material of the primary backing at its back surface and at the same time to smooth the back surface by forcing the molten material to spread slightly on the back surface 4 of the primary backing. This results in a flat and smooth layer in which at least a portion of the material of the locking end 7 - as long as it was initially present in the loop and melted - is spread more or less in a flat configuration on the back surface 4 of the primary backing. Figure 2B The processed intermediate product 100' is depicted in . It has been found that, despite the melting and spreading effects, the yarn can still be pulled out of the processed product (and thus out of the final textile product) when a pulling force is applied, which corresponds to the pulling force applied during (extremely) high load use of the textile product, depending on the type of yarn, the yarn material, the type of primary backing, its material, etc. Without being bound by theory, it is believed that this may be due to the accumulation of tension at the positions 51 and 52 where the yarn emerges from the primary backing. High tension accumulation can lead to breakage and therefore to the free end of the yarn no longer being tightly fixed to the back of the primary backing. If the tuft bond strength is indeed lower than 20-25N, it is usually necessary to apply a secondary backing, which inherently increases the tuft bond strength.
[0063] Figure 3
[0064] Figure 3 Schematically shows a configuration for applying a fiber bonding process, in this case a method derived from the basic method as known from WO 2012 / 076348. Figure 3In the configuration shown in a, there are a first heating block 500 and a second heating block 501 to heat the heating elements also represented as heating blades or heating bodies 505 and 506, respectively. These heating elements have working surfaces 515 and 516, respectively, which are in contact with the intermediate product 100 to be processed, and the intermediate product 100 is usually a primary backing, and the yarn is applied to the primary backing via a stitching process such as tufting. The working surfaces all have a working width of 18 mm and a center distance of 26 mm. The back surface of the product is in contact with the working surface of the heating element. In order to be able to apply sufficient pressure to the product to be processed, there is a Teflon support 520, which is used to offset the thrust applied to the heating element. In operation, the heating element moves relative to the product in the direction X shown. Typically, the heating element is stationary and forces the intermediate product 100 product to travel between the working surface and the Teflon support in the direction opposite to the direction shown in X. The product 100 to be processed with the above configuration is tufted into a sheet, and the configuration consists of a first sheet (primary backing) with cut pile of polyester yarn. The yarn generally has a melting temperature of about 255-265°C. The product is processed using a temperature of the first heating element of 200-220°C in order to preheat the product. The second heating element is maintained at a temperature of about 15-20°C above the yarn melting temperature. In order to maintain the temperature at the desired level, the heating block and the heating element are provided with insulating material layers 510, 511, 512 and 513, respectively. The product is supplied at a speed of 12 mm / sec (0.72 m / min) or more, and the pressure applied by the heating element is about 1.35 N / cm2. Thereafter, the product is cooled to a temperature exceeding the solidification temperature of the molten polyester (which is equal to the crystallization temperature for pure crystalline polyester) to solidify the molten portion of the polyester, thereby forming an anchor of the yarn, and thereby connecting the locked end of the yarn to the primary backing. This obtains a product 100' with a calendered back surface, i.e., smooth and shiny at the position where the stitching yarn extends from the back surface.
[0065] Figure 4
[0066] Figure 4 Schematic diagram showing a method for applying a second sheet (in this case a dimensionally stable secondary backing sheet) to a substrate with a bonding agent. Figure 3 The back side of the first sheet of the laminated structure of the method described is manufactured. In this figure, a first roller 600 is depicted, according to the combination Figure 3A 2 meter wide web of the processed intermediate product 100' made by the described method is wound onto the roller. The product is unwound from roller 600 so that its back side 217 is in contact with a second roller 601. The roller is provided so that a layer of polyester hot melt adhesive (HMA) 219 is applied to the back side 217. To this end, a large amount of HMA 219 is present and heated between rollers 601 and 602. The thickness of the layer can be adjusted by adjusting the gap between the two rollers. Downstream of the HMA application position is the secondary backing 215, which is unwound from roller 603. The secondary backing is pressed against the hot and tacky adhesive and cooled in unit 700. The unit consists of two belts 701 and 702, which, on the one hand, press the secondary backing 215 against the primary product 100' and, on the other hand, cool the adhesive to below its solidification temperature. The resulting final product 201 is then wound onto roller 604. In an alternative embodiment, as in Figure 3 The fiber bonding process and the lamination process are performed online. Figure 3 The fiber bonding device shown can be placed between roller 600 and roller 601. In this case, the intermediate product 100 is wound on roller 600 and fed along the remaining process steps.
[0067] Figure 5
[0068] Figure 5 schematically shows a cross section of an intermediate carpet product for use according to the invention. Figure 1 , but shows the primary backing 2' cover 20 in detail. Figure 5A In FIG. 1 , a first sheet 2 having a front surface 3 and a back surface 4 is depicted. The back surface 4 of the Propex woven PET sheet 2 is covered with a porous layer 20, in this case a felt fiber layer of short PET yarns. This layer is made by covering the back surface of the sheet 2 with 5Dtex fibers having a length of about 50 mm. The fibers are at a density of about 30 g / m 2 This layer is needle-punched and felted onto the first sheet, thereby forming a new double-layer primary backing 2' (corresponding to Figure 1 Element 2 in ). When a final thickness of about 2 mm (for the porous layer) was reached, the needle felting process was stopped. The porosity obtained in this layer was about 98%.
[0069] like Figure 5A As depicted in FIG. 1 , the yarn 5 is tufted into the primary backing 2' so that the locking end 7 forms a loop extending on the back surface 4' of the porous layer 20 (which is actually the back surface of the complete primary backing 2'), thereby forming an intermediate product 110. The product is subjected to the same Figure 3 The fiber bonding process described above. The result is schematically depicted in Figure 5BThe porous layer partially melts together with a portion of the locked ends 7 of the yarns 5 and forms a thin layer 20' of partially molten and pressed fleece fabric, with the ends of the yarns securely locked therein. This layer can best be compared to a glass fiber reinforced resin: a more or less continuous layer, provided with entangled fibers, including the ends of the yarns in its body. In this way, the yarns 5 in the processed intermediate product 110' appear to be even better bonded to the primary backing when compared with the bond obtained in the absence of the porous layer.
[0070] Example 1
[0071] Example 1 describes various carpet products according to the invention. The yarns used were all PET yarns, plied, twisted and heat set after twisting (as is commonly done in the art to more or less ensure twisting). In each case, the primary backing was a woven PET backing obtained from the companies indicated in Table 1. The primary backings all had a cover as described with reference to Figure 5. Carpet products 1 to 4 used 50 g / m 2 For Nos. 5 to 10, the coating has a thickness of 30 g / m 2 The weight of the Figure 3 The method described was used to bond the yarns to fibers. For products 1 to 4, a melt temperature of 295°C was used. For products 5 to 9, a temperature of 270°C was used, and for product 10, the temperature was 275°C. The products all used a secondary felt PET backing as shown in the table. The backing was adhered with a polyester hot melt adhesive (see WO 2014 / 198731 and WO 2014 / 198732). The Dtex value shown is the total Dtex of the plied yarn used for stitching. The primary backings used were all woven PET products obtained from Mattex, Harelbeke, Belgium or Propex Fabric GmbH, Gronau, Germany. The secondary backings were all needle-punched felt PET products. The TWE backing was obtained from TWE Vliesstoffwerke GmbH & Co Emsdetten (500 g / m for products 1 and 3 2 , for products 2 and 4: 900g / m 2 ). VeBe backing was obtained from VEBE Floor Coverings Genemuiden (all 900 g / m 2 ). The yarns were all PET yarns. Pharr yarns were obtained from Pharr McAdenville, USA. Pataga yarns were obtained from Pataga, Peer, Belgium and Beekaylon yarns were obtained from Beekaylon, Mumbia, India.
[0072] The resulting carpet products are subjected to classification tests according to European Standard EN1307:2014+A3:2019, including the commonly known Vetterman test. This test may lead to the following determinations:
[0073] Home Use
[0074] Class 21: Medium household use
[0075] Category 22: General household use
[0076] Class 23: Heavy household use
[0077] Commercial Use
[0078] Class 31: Medium commercial use
[0079] Class 32: General commercial use
[0080] Class 33: Heavy commercial use
[0081] The products of the present invention all meet the classification for commercial use, and even reach 32 and 33 classes for some products, especially under the combination of 3000 or higher Dtex and 144 or higher twist. As is well known, the needle gauge and weave gauge have almost no influence on the obtained classification, especially when the typical needle gauge such as 5 / 32 "to 1 / 12", such as the common 1 / 8" and 1 / 10" are applied to the needle gauge, and the typical weave gauge such as 10 to 70, such as the common 30-60, especially 38-44, is applied to the weave gauge. The tested weave gauge is selected because this is the most compatible with the fiber bonding technology used. Higher weave gauge is also generally beneficial to the Vetterman test results.
[0082] Table 1 Carpet products of the present invention
[0083]
[0084]
[0085] Table 1 Carpet products of the present invention
[0086]
[0087] Example 2
[0088] In this example, various comparative examples are described and depicted in Table 2.
[0089] Table 2 Comparative Examples
[0090]
[0091]
[0092] The materials used for the comparative examples are the same as for the examples according to the invention and the fiber bonding methods are also applied accordingly. The difference is due to the difference in Dtex of the stitching yarns and the lower twist (reaching commercial categories 31, 32 and 33 at a level consistent with ordinary nylon carpet tiles). It can be seen that this results in a lower classification.
[0093] Example 3
[0094] In this example, several methods for completely recycling the carpet products according to the present invention are described, in addition to reusing the yarn itself (by cutting and making new carpet products with the yarn). None of these methods require separation of the carpet products into various polymer-containing materials, because all carpet products according to Table 1 (as well as those of Table 2) are pure PET products, which means that all polymer materials used in the products (yarn, primary backing, secondary backing, adhesive) are polyethylene terephthalate. This provides various relatively easy options for recycling the product for recycling (as opposed to processes such as pyrolysis, decarbonization and use of PET as an additive in, for example, stone chip mortar asphalt, cementitious materials, mortar or concrete composites, etc.).
[0095] These processes all involve the main step of first cutting the carpet product into smaller pieces that can be easily accessed in the recycling process.
[0096] A first example of a class of methods that allow recycling of polyester is a method based on (thermo)mechanical methods to recycle polyester waste materials. The simplest method of thermomechanical recycling is to remelt the polyester waste. This method is applied, for example, to bottle-to-bottle technologies, where sorted PET bottles are remelted in crushed shape and reprocessed into bottles as beverage packaging.
[0097] The second category of methods for recycling polyester waste is the so-called chemical recycling (chemical decomposition) methods, in which the recycling of polyester waste materials is achieved by depolymerization into monomers and / or oligomers. Depending on the type of reactants used for chemical decomposition, this category can be divided into a number of subcategories.
[0098] One example is the use of ionic liquids for depolymerization, which was first described around 2000. This process was developed to avoid the disadvantages of other processes such as alcoholysis (high pressure and temperature and heterogeneous reaction products) or acidic and basic hydrolysis (pollution issues) to provide environmentally friendly degraders for polymers and capable of degradation under moderate reaction conditions.
[0099] As an alternative, castor oil is used for depolymerization. This process was developed to provide a renewable alternative to petrochemical reagents (such as diols) for PET depolymerization. After depolymerization, the reaction products are intended to prepare polyurethane systems.
[0100] The use of enzymes to degrade polyester polymers was first described in the 1970s. Such biochemical methods were developed to provide an environmentally friendly polymer recycling procedure compared to conventional chemical recycling methods due to the use of ionic liquids and castor oil.
[0101] Alcoholysis for PET depolymerization was first described in the early 1990s. This method was developed to avoid the disadvantages of acidic and alkaline hydrolysis (pollution problems) to provide a renewable and more environmentally friendly degradation agent for polymers. Typically, polyesters are depolymerized with excess alcohol to obtain the corresponding esters of the corresponding acid and ethylene glycol. In the alcoholysis process, the reaction with methanol has become particularly important due to the low price and availability of methanol. Ethylene glycol (a diol, the use of which is sometimes classified separately as "glycolysis", although it belongs to the alcoholysis category) is also mainly used in reactive extrusion to make low molecular weight oligomers. However, these oligomers must be separated and purified for further processing because the crude reaction product consists of a heterogeneous mixture of monomers, oligomers and polymers. Various other alcohols that can be used are described, such as pentaerythritol, 1-butanol, 1-pentanol and 1-hexanol and 2-ethyl-1-hexanol. Other glycols besides ethylene glycol, such as BHET, neopentyl glycol (NPG), tetraethylene glycol (TEEG), polyethylene glycol, polyoxytetramethylene and trimer [poly(oxyethylene)-poly-(oxypropylene)-poly(oxyethylene)] have also been described in the art for depolymerizing polyesters by alcoholysis. In a recent patent application WO 2022 / 003084 (assigned to Cure Technology BV), an improved alcoholysis process is described in which, in the first of two consecutive stages, a stream of polyester waste material is continuously fed into an extruder operating at a temperature above the melting temperature of the polyester while alcohol is fed into the extruder, and in the second stage, the fluid mixture is continuously fed into a continuous stirred tank reactor (CSTR) operating at a temperature above the melting temperature of the polyester while a second amount of alcohol is co-fed into the CSTR to provide a continuous stream of polyester depolymerized into oligomeric esters at the outlet of the CSTR. The oligomers can be used to prepare new polyesters of any quality.
[0102] Aminolysis and aminolysis were developed for polyester recycling because the amine groups are more reactive than the hydroxyl groups or the alcohols used for polyester alcoholysis.
[0103] Finally, an alternative chemical recycling of polyesters is provided by controlled depolymerization of polyesters using a defined amount of depolymerizing agent to block chain scission (see Geyer et al. in eXPRESS Polymer Letters Vol. 10 No. 7 (2016) 559–586). This process produces polyester oligomers with well-defined molecular weights over a wider range than existing chemical processes such as alcoholysis.
Claims
1. A method of manufacturing a carpet product, comprising: - providing a first sheet having a front surface and a back surface, - providing one or more polyester yarns having a weight of at least 2500 Dtex and a twist of at least 100 tpm, - forming a pile on the front surface of the first sheet by stitching the one or more yarns through the first sheet, the one or more yarns having a free end forming the pile and a locked end present at the back surface of the first sheet, thereby forming an intermediate product, - processing the intermediate product by feeding it along a body having a heated surface, the back surface being in contact with the heated surface, so as to melt at least a portion of the polyester of the locked ends of the one or more yarns, - Cooling the molten portion of the polyester to solidify the molten portion of the polyester, thereby connecting the locked ends of the one or more yarns to the first sheet and forming a carpet product.
2. The method according to claim 1, characterized in that The one or more polyester yarns have a weight of at least 2800 Dtex and a twist of at least 120 tpm.
3. The method according to any one of the preceding claims, characterized in that The one or more polyester yarns have a weight of at least 3000 Dtex and a twist of at least 150 tpm.
4. The method according to any one of the preceding claims, characterized in that The first sheet is a polyester sheet.
5. The method according to any one of the preceding claims, characterized in that The polyester includes PET (polyethylene terephthalate) and / or PTT (polytrimethylene terephthalate).
6. The method according to any one of the preceding claims, characterized in that The polyester of the yarn has an intrinsic viscosity higher than 0.8 dl / g.
7. The method according to any one of the preceding claims, characterized in that The one or more yarns are multi-ply yarns, in particular 2, 3 or 4 ply yarns.
8. The method according to any one of the preceding claims, characterized in that The one or more yarns are each composed of a plurality of filaments having a weight of 2 to 40 dpf.
9. The method according to claim 8, characterized in that The filament weight is 5 to 20 dpf, preferably 8 to 12 dpf.
10. The method according to any one of the preceding claims, characterized in that The one or more polyester yarns have a weight of at least 3500 Dtex, preferably at least 4000 Dtex.
11. The method according to any one of the preceding claims, characterized in that In the step of processing the intermediate product by feeding the intermediate product along a body having a heated surface, the intermediate product has a relative speed with respect to the heated surface of the body.
12. The method according to any one of the preceding claims, characterized in that The method includes attaching the second sheet to the carpet product using an adhesive applied between the processed back surface of the first sheet and the second sheet.
13. The method according to claim 12, characterized in that The adhesive is a hot melt adhesive.
14. The method according to claim 13, characterized in that The adhesive is a polyester hot melt adhesive.
15. The method according to any one of claims 12 to 14, characterized in that The second sheet material is a fiber sheet material, preferably a felt sheet material.
16. The method according to any one of claims 12 to 15, characterized in that The second sheet is a polyester sheet.
17. A carpet product comprising a first sheet having a front surface and a back surface and one or more polyester yarns sewn through the first sheet to form a pile on the front surface of the sheet, the yarn having a weight of at least 2500 Dtex and a twist of at least 100 tpm, wherein at least a portion of the polyester at the locked ends of the one or more yarns is melted, spread on the back surface of the sheet and solidified.