Polarizing film laminate and image display device

By directly joining the polarizing film and the resin film in the polarizing film laminate, and using ultraviolet light or electron beams to enhance the adhesive force, the problem of deformation and cracking caused by stress accumulation in the adhesive layer is solved, and high crack resistance is achieved and tightness.

CN118786367APending Publication Date: 2024-10-15NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380023913.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-20
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

When the existing polarizing film laminate is laminated in an adhesive layer, it is easy to cause deformation, cracks and peeling due to stress accumulation, and it is difficult to meet the crack resistance and adhesion requirements of repeated bending.

Method used

The polarizing film is directly bonded to the first resin film and the second resin film, with a thickness of 20 μm or less, and is bonded through energy rays such as ultraviolet light or electron beams to reduce interface stress and strain and improve adhesion.

Benefits of technology

The crack resistance and adhesion of the polarizing film laminate are significantly improved, and it can remain intact without cracks and peeling during repeated bending of 200,000 times.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118786367A_ABST
    Figure CN118786367A_ABST
Patent Text Reader

Abstract

The present invention relates to a polarizing film laminate in which a polarizing film, a first resin film, and a second resin film are provided in this order, the thickness of the polarizing film being 20 [mu] m or less, and the first resin film and the second resin film being directly bonded together. The polarizing film laminate has excellent crack resistance and adhesion to repeated bending.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polarizing film laminate and an image display device. Background Art

[0002] In the past, as polarizing films used in various image display devices such as liquid crystal display devices and organic EL display devices, polyvinyl alcohol films that have been dyed (containing dichroic substances such as iodine and dichroic dyes) have been used because they have both high transmittance and high polarization degree. The polarizing film can be manufactured by subjecting the polyvinyl alcohol film to various treatments such as swelling, dyeing, cross-linking, and stretching in a bath, followed by washing and drying. In addition, the polarizing film is usually used in the form of a polarizing film (polarizer) having a transparent protective film such as triacetyl cellulose bonded to one or both sides with an adhesive.

[0003] The polarizing film can be used as a polarizing film laminate (optical film) by laminating other resin films such as an optical layer as needed. In addition, as the polarizing film (polarizer), a polarizing film in which a polarizing film and a transparent protective film are directly bonded together without an adhesive layer or a pressure-sensitive adhesive layer is also known (Patent Documents 1-4).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: International Publication No. 2005 / 085918

[0007] Patent Document 2: Japanese Patent Application Publication No. 2002-303725

[0008] Patent Document 3: Japanese Patent Application Publication No. 2002-303726

[0009] Patent Document 4: Japanese Patent Application Publication No. 2002-303727 Summary of the invention

[0010] Problems to be solved by the invention

[0011] There is a strong demand for thinner polarizing films and polarizing films, but when the resin films of the polarizing film laminate are bonded together via an adhesive layer as described above, the adhesive layer is highly elastic, and stress is easily accumulated when the adhesive is cured. Therefore, when stress is accumulated at the interface, when the polarizing film laminate is deformed due to bending, etc., cracks and peeling may occur due to increased stress and strain at the interface.

[0012] In view of the above circumstances, an object of the present invention is to provide a polarizing film laminate having excellent crack resistance and adhesion to repeated bending.

[0013] Another object of the present invention is to provide an image display device including the above-mentioned polarizing film laminate.

[0014] Solutions to the problem

[0015] That is, the present invention relates to a polarizing film laminate, which includes a polarizing film, a first resin film, and a second resin film in this order, wherein the thickness of the polarizing film is 20 μm or less, and the first resin film and the second resin film are directly bonded together.

[0016] Furthermore, the present invention relates to an image display device including the polarizing film laminate.

[0017] Effects of the Invention

[0018] The details of the mechanism of action of the effect of the polarizing film laminate of the present invention can be estimated as follows. It should be noted that the interpretation of the present invention is not limited to this mechanism of action.

[0019] The polarizing film stack of the present invention is provided with a polarizing film, a first resin film, and a second resin film in sequence, the thickness of the polarizing film is less than 20 μm, and the first resin film and the second resin film are directly bonded together. Therefore, the stress and strain at the interface between the resin films are small, and therefore, the crack resistance and tightness to repeated bending are excellent. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 Schematic diagram showing a 180° folding endurance tester. DETAILED DESCRIPTION

[0021] <Polarizing film laminate>

[0022] The polarizing film laminate of the present invention comprises a polarizing film, a first resin film, and a second resin film in this order, the polarizing film has a thickness of 20 μm or less, and the first resin film and the second resin film are directly bonded together.

[0023] <Polarizing film>

[0024] The polarizing film is formed by adsorbing and aligning a dichroic substance such as iodine or a dichroic dye in a polyvinyl alcohol film. From the viewpoint of initial polarization performance of the polarizing film, the polarizing film is preferably an iodine-based polarizing film containing iodine as the dichroic substance.

[0025] The polyvinyl alcohol (PVA) film can be used without particular limitation. The polyvinyl alcohol (PVA) film has light transmittance in the visible light region and disperses and adsorbs dichroic substances such as iodine and dichroic dyes. As the material of the polyvinyl alcohol film, polyvinyl alcohol or its derivatives can be cited. As the derivatives of the polyvinyl alcohol, for example, polyvinyl formal, polyvinyl acetal; olefins such as ethylene and propylene; derivatives modified with unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid and their alkyl esters, acrylamide, etc. The average polymerization degree of the polyvinyl alcohol is preferably about 100 to 10,000, more preferably about 1,000 to 10,000, and further preferably about 1,500 to 4,500. In addition, the saponification degree of the polyvinyl alcohol is preferably about 80 to 100 mol%, more preferably about 95 mol% to 99.95 mol. It should be noted that the average polymerization degree and the saponification degree can be obtained according to JIS K 6726.

[0026] The polarizing film can be obtained by a conventional method for producing a polarizing film, for example, by subjecting the polyvinyl alcohol film to any swelling step and washing step, and at least to a dyeing step, a crosslinking step, and a stretching step.

[0027] From the viewpoint of improving the initial polarization degree of the polarizing film, the thickness of the polarizing film is preferably 1 μm or more, more preferably 2 μm or more, and from the viewpoint of preventing the warping of the panel, it is preferably 15 μm or less, more preferably 10 μm or less, and further preferably 8 μm or less. In particular, in order to obtain a polarizing film having a thickness of about 8 μm or less, the following method for producing a thin polarizing film can be used, in which a laminate comprising a polyvinyl alcohol resin layer formed on a thermoplastic resin substrate is used as the polyvinyl alcohol film.

[0028] A polarizing film (thin polarizing film) can be obtained by an existing method for manufacturing a polarizing film, for example, by implementing a process of preparing a laminate by forming a polyvinyl alcohol resin layer (PVA resin layer) containing a polyvinyl alcohol resin (PVA resin) on one side of a long thermoplastic resin substrate; while transporting the obtained laminate in the length direction, performing an optional insolubilization treatment process, a cross-linking treatment process and a cleaning treatment process on the above-mentioned laminate; and at least performing an auxiliary stretching treatment process in a gas atmosphere, a dyeing treatment process and a stretching treatment process in an aqueous solution to obtain the laminate.

[0029] <First Resin Film and Second Resin Film>

[0030] The first resin film and the second resin film are not particularly limited as long as they are made of different materials. For example, organic substrates such as transparent protective films and retardation films that have been used in polarizing film laminates (optical films) can be used.

[0031] In addition, the thickness of the above-mentioned first resin film and the above-mentioned second resin film can be appropriately determined, but generally speaking, from the viewpoint of strength, handleability and other operability, it is preferably greater than 0.5 μm, more preferably greater than 1 μm, and further preferably greater than 2 μm. In addition, from the viewpoint of thin layer properties, it is preferably less than 500 μm, more preferably less than 300 μm, and further preferably less than 100 μm.

[0032] As materials constituting the above-mentioned transparent protective film, for example, cellulose ester resins, polycarbonate resins, (meth) acrylic resins, cyclic polyolefin resins, polyester resins, etc. can be cited. As the above-mentioned phase difference film, for example, birefringent films formed by unidirectional or bidirectional stretching of polymer raw materials, oriented films of liquid crystal polymers, phase difference plates formed by supporting the oriented layers of liquid crystal polymers with films, etc. can be cited. In addition, one or more layers of hard coatings, anti-reflection layers, anti-adhesion layers, diffusion layers, or anti-glare layers can be provided on the above-mentioned transparent protective film and the above-mentioned phase difference film; optical layers used in the formation of image display devices, such as reflective plates, semi-transmissive plates, phase difference plates (including 1 / 2, 1 / 4, etc. wave plates), viewing angle compensation films, etc. The above-mentioned other layers and optical layers can usually be bonded via adhesive layers or adhesive layers described later.

[0033] When the first resin film and / or the second resin film is bonded to both surfaces of the polarizing film, the resin films on both surfaces may be the same or different.

[0034] The first resin film and / or the second resin film may contain any appropriate additives such as ultraviolet absorbers, antioxidants, lubricants, plasticizers, mold release agents, anti-coloring agents, flame retardants, antistatic agents, pigments, colorants, etc.

[0035] <Method for bonding first resin film and second resin film>

[0036] The method of directly joining the first resin film and the second resin film without an adhesive layer or a pressure-sensitive adhesive layer can be cited as follows: a method of pressing, a method of laminating by irradiating energy rays such as ultraviolet rays, electron beams, etc., and in particular, from the viewpoint of improving adhesion, it is preferred to irradiate ultraviolet light to the laminating surface of either or both of the first resin film and the second resin film and perform surface treatment, and then laminating via a volatile medium and drying the volatile medium. By the presence of the volatile medium, it is possible to fit closely to the laminating surface without mixing with bubbles, etc., and further, by drying the volatile medium, the adhesion of the bonding surface (interface) is significantly improved. As ultraviolet light, for example, the wavelength is preferably 250-100nm, more preferably 200-100nm, wherein, from the viewpoint of mass production, a wavelength of 172nm using a xenon excimer lamp (excimer UV) is particularly preferred.

[0037] In addition, from the viewpoint of processing capacity, the illuminance of the ultraviolet light is preferably 1 mW / cm 2 More preferably, 50 mW / cm 2 In addition, from the viewpoint of adhesiveness, the accumulated light intensity is preferably 1 mJ / cm 2 More preferably, 50 mJ / cm 2 From the viewpoint of film damage, 5000 mJ / cm 2 Less than, more preferably 2000mJ / cm 2 In addition, the temperature during ultraviolet irradiation is not particularly limited. From the perspective of stabilization of surface modification, it is preferably about 0 to 50°C, more preferably about 10 to 40°C. In the production of polarizing films, room temperature is convenient. In addition, as for the atmosphere during ultraviolet irradiation, the oxygen concentration can be 21% or less. From the perspective of treatment efficiency, the oxygen concentration is preferably 7.0% or less.

[0038] The volatile medium is not particularly limited, but is preferably a solvent such as water, ethanol, toluene, cyclohexane, or acetone from the viewpoint of drying efficiency, and more preferably water from the viewpoint of environment.

[0039] The heating temperature may be any temperature that can properly dry the volatile medium. For example, when the volatile medium is water, the heating temperature is preferably about 40 to 80° C., and more preferably about 50 to 70° C. In addition, the drying time is affected by the temperature of the polarizing film, and therefore cannot be generalized. The drying time is preferably about 1 minute to 60 minutes, and more preferably about 3 to 15 minutes. The drying step may be performed only once, or may be performed multiple times as needed.

[0040] The above-mentioned bonding can be performed by a roll laminator or the like.

[0041] The bonding interface between the first resin film and the second resin film may include a modified layer or a high elastic layer resulting from a treatment during bonding.

[0042] In the polarizing film laminate, the adhesive force (peel strength) between the first resin film and the second resin film is preferably 0.5 N / 15 mm or more, more preferably 1.0 N / 15 mm or more, and even more preferably 1.5 N / 15 mm or more.

[0043] The polarizing film and the first resin film can usually be bonded together via a pressure-sensitive adhesive layer or an adhesive layer.

[0044] As the adhesive forming the adhesive layer, various adhesives that have been used for polarizing films can be used, for example, rubber adhesives, acrylic adhesives, silicone adhesives, urethane adhesives, vinyl alkyl ether adhesives, polyvinyl alcohol adhesives, polyvinyl pyrrolidone adhesives, polyacrylamide adhesives, cellulose adhesives, etc. Among these, acrylic adhesives are preferred.

[0045] In addition, as the adhesive forming the above-mentioned adhesive layer, various adhesives that have been used for polarizing films can be used, for example, isocyanate adhesives, polyvinyl alcohol adhesives, gelatin adhesives, vinyl latexes, water-based polyesters, etc. These adhesives are usually used in the form of adhesives made of aqueous solutions (water-based adhesives) and contain 0.5 to 60% by weight of solid components. As the above-mentioned adhesives, in addition to the above, active energy ray-curing adhesives such as ultraviolet curing adhesives and electron beam curing adhesives can be mentioned. As the above-mentioned active energy ray-curing adhesive, for example, (meth)acrylate adhesives can be mentioned. As the curable component in the above-mentioned (meth)acrylate adhesive, for example, compounds having a (meth)acryloyl group and compounds having a vinyl group can be mentioned. Examples of compounds having a (meth)acryloyl group include: (meth)acrylic acid alkyl esters such as (meth)acrylic acid chain alkyl esters having 1 to 20 alkyl carbon atoms, (meth)acrylic acid alicyclic alkyl esters, and (meth)acrylic acid polycyclic alkyl esters; hydroxyl group-containing (meth)acrylic acid esters; epoxy group-containing (meth)acrylic acid esters such as glycidyl (meth)acrylate, and the like. (Meth)acrylate adhesives may also contain nitrogen-containing monomers such as hydroxyethyl (meth)acrylamide, N-methylol (meth)acrylamide, N-methoxymethyl (meth)acrylamide, N-ethoxymethyl (meth)acrylamide, (meth)acrylamide, and (meth)acryloyl morpholine. (Meth)acrylate adhesives may contain tripropylene glycol diacrylate, 1,9-nonanediol diacrylate, tricyclodecane dimethanol diacrylate, cyclic trimethylolpropane methylal acrylate, dimethoxypropane methylal acrylate, and the like. Multifunctional monomers such as alkanediol diacrylate and EO modified diglycerol tetraacrylate are used as crosslinking components. In addition, as a cationic polymerization curing adhesive, a compound having an epoxy group or an oxetane group can also be used. The compound having an epoxy group is not particularly limited as long as it has at least two epoxy groups in the molecule, and various commonly known curable epoxy compounds can be used. In addition, as a cationic polymerization curing adhesive, a compound having an epoxy group or an oxetane group can also be used. Among these, from the viewpoint of curability and productivity, an active energy ray curing adhesive of a (meth)acrylate adhesive is preferably used.

[0046] The coating of the above-mentioned adhesive can be carried out on either the resin film side or the polarizing film side, or on both sides. After lamination, a drying process is carried out as needed to form an adhesive layer made of the coated dried layer. After the above-mentioned drying process, ultraviolet rays or electron beams can be irradiated as needed. The thickness of the above-mentioned adhesive layer is not particularly limited. When using a water-based adhesive, etc., it is preferably about 30 to 5000 nm, more preferably about 100 to 1000 nm. When using an ultraviolet curing adhesive, an electron beam curing adhesive, etc., it is preferably about 0.1 to 100 μm, more preferably about 0.5 to 10 μm.

[0047] The polarizing film laminate can be applied to an image display device. Representative examples of image display devices include liquid crystal display devices and organic electroluminescent (EL) display devices. The image display device can adopt a configuration known in the industry, and therefore, a detailed description thereof will be omitted.

[0048] Example

[0049] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.

[0050] <Example 1>

[0051] <Production of polarizing film>

[0052] A laminated body having a 9 μm thick PVA layer formed on an amorphous PET substrate was subjected to auxiliary stretching in a gas atmosphere at a stretching temperature of 130°C to produce a stretched laminated body, and then the stretched laminated body was dyed to produce a colored laminated body, and further, the colored laminated body was stretched in boric acid water at a stretching temperature of 65 degrees to produce an optical film laminated body including a 5 μm thick polarizing film stretched integrally with the amorphous PET substrate in a manner that the total stretching ratio reached 5.94 times. By such two-step stretching, an optical film laminated body including a polarizing film with a thickness of 5 μm was obtained, in which the PVA molecules of the PVA layer formed on the amorphous PET substrate were highly oriented, and the iodine adsorbed by dyeing was highly oriented in one direction in the form of a polyiodide ion complex.

[0053] <Production of polarizing film laminate>

[0054] In a nitrogen-substituted atmosphere having an oxygen concentration of about 2.5%, an excimer UV treatment apparatus (SVC342S-1N2-MN3-KWO1 manufactured by Ushio Electric Co., Ltd., xenon excimer lamp) was used to treat a cellulose triacetate resin film 1 having a thickness of 25 μm (manufactured by Konica Minolta, Inc., Konica Minolta TacKC2UA) and a cycloolefin resin film 2 having a thickness of 3 μm (a cycloolefin resin film with a release liner obtained as follows: a cycloolefin polymer (COP) film (trade name "ZEONOR FILM ZF14”) to prepare a COP solution, the prepared COP solution was applied on a PET film (release liner) using a wire bar coater #13, and then dried in an oven at 60°C for 3 minutes, thereby laminating a COP film with a thickness of 3 μm on the release liner. ) were irradiated with excimer UV light (wavelength 172 nm, peak illuminance 75 mW / cm 2 、Accumulated light quantity 450mJ / cm 2 ), surface modification was performed. Next, water was applied to the surface modified surface of each film, and before the water dried, the modified surfaces of each resin film were bonded to each other using a laminator, and then dried in an oven at 60°C for 5 minutes and 30 seconds, and the release liner was peeled off to obtain an optical laminate in which resin film 1 and resin film 2 were directly bonded. Next, the following active energy ray-curable adhesive was applied to the cycloolefin resin film surface of the optical laminate in which the triacetyl cellulose resin film 1 and the cycloolefin resin film 2 were directly bonded using a wire bar coater, and bonded to the polarizing film surface of the optical film laminate including a polarizing film with a thickness of 5 μm obtained in Example 1 using a laminator. In this state, active energy rays were irradiated from the resin film side to cure the adhesive, and a polarizing film laminate in which the above-mentioned optical laminate was bonded to the polarizing film via the active energy ray adhesive was obtained.

[0055] [Active energy ray-curable adhesive]

[0056] 2-Hydroxyethylacrylamide (manufactured by KJ Chemical Co., Ltd., trade name: HEAA) 16.5 parts by weight, 4-vinylphenylboric acid (manufactured by Tokyo Chemical Industry Co., Ltd.) 1 part by weight, 2-hydroxy-3-phenoxypropyl acrylate (manufactured by Toagosei Co., Ltd., trade name: Aronix M-5700) 30.5 parts by weight, 1,9-nonanediol diacrylate (manufactured by Kyoeisha Chemical Co., Ltd., trade name: LIGHT ACRYLATE 1,9ND-A) 25 parts by weight, hydroxypivalic acid diacrylate (manufactured by Kyoeisha Chemical Co., Ltd., trade name: LIGHT ACRYLATE HPP-A) 13 parts by weight, an oligomer obtained by polymerizing a (meth)acrylate (manufactured by Toagosei Co., Ltd., trade name: ARFON UP-1190) 15 parts by weight, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one (IGM 3 parts by weight of 2,4-diethylthioxanthone (manufactured by Nippon Kayaku Co., Ltd., trade name: KAYACURE-DETX-S)

[0057] [Active energy rays]

[0058] Visible light (gallium-encapsulated metal halide lamp) was used as active energy ray. Irradiation device: Light HAMMER 10 manufactured by Heraeus. Valve: V valve. Peak illuminance: 800 mW / cm 2 , cumulative exposure 800 / mJ / cm 2 (Wavelength: 380 to 440 nm) The illuminance of visible light was measured using a Sola-Check system manufactured by Solatell.

[0059] <Evaluation of repeated bending>

[0060] The adhesive layer (1) is moved from the diaphragm to the TAC side of the polarizing film laminate obtained above, and the adhesive layer (2) is moved from the diaphragm to the polarizing film side, thereby producing an optical laminate having adhesive layers on both sides. Next, a PET film (transparent substrate, manufactured by Mitsubishi Resins Co., Ltd., trade name: DIAFOIL) with a thickness of 25 μm that has been corona-treated is bonded to the adhesive layer (2) surface of the optical laminate. Furthermore, a polyimide film (PI film, manufactured by DuPont Toray Industries, Ltd., KAPTON 300V, substrate) with a thickness of 77 μm that has been corona-treated is bonded to the adhesive layer (1) surface, thereby producing a sample for evaluating a laminated optical film. Figure 1A schematic diagram of a 180° folding resistance tester (manufactured by Imoto Manufacturing Co., Ltd.) is shown in the figure. This device is a mechanism that clamps a mandrel in a constant temperature chamber to repeatedly bend a single-side chuck 180°, and the bending radius can be changed by the diameter of the mandrel. It is a mechanism that stops the test if the film breaks. The evaluation sample (5cm×15cm) of the optical laminate manufactured as described above was set in the device so that the polarizing film was located on the outside (TAC was on the mandrel side), and the test was carried out under the conditions of a bending angle of 180°, a bending radius of 3mm, a bending speed of 1 second / time, and a weight of 100g. The evaluation criteria are as follows.

[0061] [Adhesion]

[0062] ○: Even when the bending frequency reaches 200,000 times, there is no peeling between the first resin film and the second resin film.

[0063] △: Even when the number of folding times reached 200,000, there was a slight peeling between the first resin film and the second resin film only in the folding region (practical level).

[0064] ×: When the number of folding times reached 200,000 times, there was peeling between the first resin film and the second resin film (not a practical level).

[0065] [Crack resistance]

[0066] ○: Even after being bent 200,000 times, no cracks were generated in the first resin film, the second resin film, and the polarizing film.

[0067] ×: When the number of bending times reached 200,000 times, cracks occurred in at least one of the first resin film, the second resin film, and the polarizing film.

[0068] <Evaluation of Adhesion (Peel Strength)>

[0069] A double-sided tape (No. 500, manufactured by Nitto Denko Corporation) was attached to the resin film 2 surface of the optical laminate formed by the resin film 1 and the resin film 2. Further, a size of 200 mm × 15 mm was cut, and a cut was made between the resin film 1 and the resin film 2 with a cutter, and then the release film of the double-sided tape was peeled off, so that the adhesive surface was attached to the glass plate. The polarizing film and the transparent protective film were peeled off in a 90-degree direction at a peeling speed of 1000 mm / min using an angle-variable adhesive / film peeling analysis device (VPA-2, manufactured by Kyowa Interface Chemical Co., Ltd.), and the peeling strength (N / 15 mm) was measured.

[0070] <Comparative Example 1>

[0071] The above-mentioned active energy ray-curable adhesive was applied to a cellulose triacetate resin film 1 (manufactured by Konica Minolta Tac KC2UA, Ltd.) having a thickness of 25 μm as a resin film using a wire bar coater, and then laminated with a cycloolefin resin film 2 having a thickness of 3 μm using a laminator (a cycloolefin resin film with a release liner obtained as follows: a COP solution was prepared by adding 10 g of a cycloolefin polymer (COP) film (trade name: "ZEONOR FILMZF14") to 90 g of a 2:3 mixed solvent of 2,4-trichlorobenzene and toluene, and the prepared COP solution was applied to a PET film (release liner) using a wire bar coater #13, followed by drying in an oven at 60°C for 3 minutes, thereby laminating a COP film having a thickness of 3 μm on the release liner.) In this state, the resin film 2 side was irradiated with active energy rays to cure the adhesive, and an optical laminate in which the resin film 1 and the resin film 2 were bonded together via the adhesive was obtained. Next, the release liner of the resin film 2 of the optical laminate was peeled off, and the active energy ray-curable adhesive was applied to the surface of the resin film 2 side using a wire bar coater, and the polarizing film surface of the optical film laminate including the polarizing film with a thickness of 5 μm obtained in Example 1 was laminated using a laminator. In this state, the resin film side was irradiated with active energy rays to cure the adhesive, and a polarizing film laminate in which the resin film was bonded to the polarizing film via the adhesive was obtained.

[0072] <Comparative Example 2>

[0073] A roll laminator was used to press-bond a cycloolefin resin film having a thickness of 50 μm and a cycloolefin resin film having a thickness of 15 μm at a temperature of 145° C. to obtain an optical laminate in which the cycloolefin resin films were directly bonded. Next, the cycloolefin resin film side having a thickness of 15 μm of the obtained optical laminate was press-bonded to a polarizing film having a thickness of 30 μm under the same conditions as above to obtain a polarizing film in which the optical laminate and the polarizing film were directly bonded.

[0074] The same evaluation as in Example 1 was performed using the polarizing films obtained in the above-mentioned respective Examples and Comparative Examples. The results are shown in Table 1.

[0075] [Table 1]

[0076] Example 1 Comparative Example 1 Comparative Example 2 First resin film TAC(25um) TAC(25um) COP(50um) Adhesive Adhesive(1μm) -(Heating and pressing) Second resin film COP(3um) COP(3um) COP(15um) Adhesive Adhesive(1μm) Adhesive(1μm) -(Heating and pressing) Polarizing film Polarizing film (5μm) Polarizing film (5μm) Polarizing film (30μm) Adhesion ○ × Δ Crack resistance ○ ○ × Adhesion (peel strength) (N / 15mm) 1.6 1.0 Difficult to peel off

Claims

1. A polarizing film laminate, comprising a polarizing film, a first resin film, and a second resin film, The thickness of the polarizing film is less than 20 μm. The first resin film and the second resin film are directly bonded together.

2. The polarizing film laminate according to claim 1, wherein: The adhesive strength of the bonding surface between the first resin film and the second resin film is 0.5 N / 15 mm or more under the conditions of a peeling angle of 90° and a peeling speed of 1000 mm / min.

3. The polarizing film laminate according to claim 1 or 2, wherein: The polarizing film and the first resin film are bonded together via an adhesive layer. 4 . An image display device comprising the polarizing film laminate according to claim 1 .