Composition for forming resist underlayer film

By using specific resist underlayer film compositions and dry etching technology in semiconductor manufacturing, the problems of resist pattern shape and etching resistance are solved, and effective processing and precision improvement of highly integrated semiconductor devices are achieved.

CN118786391APending Publication Date: 2024-10-15NISSAN CHEM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380024074.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-06-09
Filing Date
2023-02-06
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In semiconductor device manufacturing, progress in high integration has led to shorter wavelengths of active light, making it difficult to form the resist pattern into a desired shape after development, and the resist underlayer film has insufficient etching resistance and planarization properties. , it is difficult to achieve sufficient substrate processing.

Method used

A composition for forming a resist underlayer film is used, which contains a polymer having a specific unit structure, and to which a surfactant, a cross-linking agent, an acid and its salt or an acid generator are added, and the composition is photonized Or electron beam irradiation and development form a resist pattern, which is then transferred to the substrate through dry etching technology.

Benefits of technology

It achieves excellent etching resistance, good planarization and embedding properties of the resist pattern, can maintain curing characteristics under nitrogen atmosphere, and effectively suppresses reflected light, improving the accuracy of photolithography processes in semiconductor manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118786391A_ABST
    Figure CN118786391A_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a composition for forming a resist underlayer film, which is used in a lithographic process for manufacturing a semiconductor device and has heat resistance. [Solution] A composition for forming a resist underlayer film, the composition containing a polymer having a unit structure represented by formula (I) or formula (I ') (in formula (I) or formula (I'), n1, n2, and n3 are 0, ring A and ring B are benzene rings or naphthalene rings, and D represents a divalent organic group including a structure represented by formula (II) and / or formula (III)). A method for manufacturing a semiconductor device, the method comprising: a step for forming an underlayer film on a semiconductor substrate by means of the resist underlayer film-forming composition; a step for forming a hard mask on the underlayer film; a step for further forming a resist film on the hard mask; a step for forming a resist pattern by irradiation and development with light or an electron beam; a step for etching the hard mask by means of the resist pattern; a step for etching the underlayer film by means of the patterned hard mask; and a step for processing the semiconductor substrate with the patterned underlayer film. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resist underlayer film-forming composition for lithography which is effective in processing a semiconductor substrate, a resist pattern forming method using the resist underlayer film-forming composition, and a method for producing a semiconductor device. Background Art

[0002] In the manufacture of semiconductor devices, micro-machining has been carried out by using photolithography of photoresist compositions. The above-mentioned micro-machining is to form a thin film of photoresist compositions on a processed substrate such as a silicon wafer, irradiate active light such as ultraviolet rays on it through a mask pattern depicting a pattern of a semiconductor device, and develop it, and use the obtained photoresist pattern as a protective film to etch the processed substrate such as a silicon wafer. However, in recent years, the high integration of semiconductor devices has progressed, and the active light used also has a tendency to be shortened from KrF excimer laser (248nm) to ArF excimer laser (193nm). Accompanied by this, it is known that the influence of diffuse reflection and standing waves of active light from the substrate has become a big problem, and a resist pattern with a desired shape cannot be formed. Therefore, a method for controlling optical constants by setting an anti-reflective film (Bottom Anti-Reflective Coating, BARC) between the photoresist and the processed substrate to suppress the influence of standing waves has been widely studied.

[0003] If the resist pattern is miniaturized, problems such as resolution and collapse of the resist pattern after development will arise, and the resist is expected to be thinned. Therefore, it is difficult to obtain a resist pattern film thickness sufficient for substrate processing, and a process is required to make not only the resist pattern but also the resist underlayer film made between the resist and the semiconductor substrate to be processed have the function of a mask during substrate processing. This process is a photolithography process that forms at least two layers of resist underlayer films and uses the resist underlayer films as mask materials. As materials for forming the above-mentioned at least two layers, organic resins (for example, acrylic resins, novolac resins, polyester resins, polyether resins, PEEK resins, maleimide resins, etc.), organic compounds (for example, amorphous carbon, etc.), silicone resins (for example, organopolysiloxanes, etc.), inorganic silicon compounds (for example, SiON, SiO 2, SiN, etc.). When dry etching is performed using a pattern formed by the above organic layer as a mask, it is considered necessary that the pattern has excellent etching resistance to etching gases (such as fluorocarbons, oxygen, etc.), although it depends on the processing conditions. In addition, due to the diversification of semiconductor manufacturing processes, materials that not only exhibit the above characteristics but also exhibit small film thickness differences and good coverage properties (flattening properties) with respect to various layouts in high-low substrates, embedding properties for fine patterns, and sufficient curing properties in a nitrogen atmosphere are also required.

[0004] Examples of the polymer for the resist underlayer film include the following.

[0005] There are exemplified resist underlayer film-forming compositions using polyvinylcarbazole (see Patent Documents 1, 2, and 3).

[0006] A resist underlayer film-forming composition using a fluorenephenol novolac resin is disclosed (for example, refer to Patent Document 4).

[0007] A resist underlayer film-forming composition using a fluorene naphthol novolac resin is disclosed (for example, refer to Patent Document 5).

[0008] A resist underlayer film-forming composition containing a resin having fluorenephenol and an aryl alkylene group as repeating units is disclosed (for example, see Patent Documents 6 and 7).

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: Japanese Patent Application Laid-Open No. 2-293850

[0012] Patent Document 2: Japanese Patent Application Laid-Open No. 1-154050

[0013] Patent Document 3: Japanese Patent Application Laid-Open No. 2-22657

[0014] Patent Document 4: Japanese Patent Application Laid-Open No. 2005-128509

[0015] Patent Document 5: Japanese Patent Application Laid-Open No. 2007-199653

[0016] Patent Document 6: Japanese Patent Application Laid-Open No. 2007-178974

[0017] Patent Document 7: U.S. Patent No. 7378217 Summary of the invention

[0018] Problems to be solved by the invention

[0019] The present invention provides a resist underlayer film forming composition for use in a photolithography process for manufacturing semiconductor devices. In addition, the present invention provides a resist underlayer film for photolithography that does not mix with a resist layer, obtains an excellent resist pattern, exhibits excellent etching resistance, has good planarization and embedding properties for a substrate that has been micro-processed, has resistance to solvents even in a nitrogen atmosphere, and exhibits sufficient curing characteristics. In addition, the present invention can also impart the ability to effectively absorb reflected light from a substrate when irradiation light of wavelengths such as 248nm, 193nm, and 157nm is used for micro-processing. Further, the present invention provides a method for forming a resist pattern using a resist underlayer film forming composition. Furthermore, a resist underlayer film forming composition for forming a resist underlayer film that also has heat resistance is provided.

[0020] Means for solving problems

[0021] According to a first aspect of the present invention, there is provided a resist underlayer film-forming composition comprising a polymer having a unit structure represented by the following formula (I) or formula (I'):

[0022]

[0023] (In formula (I) or formula (I'), ring A and ring B are aryl groups having 6 to 80 carbon atoms which may contain a heteroatom and may have a cyclic structure containing an alkyl chain. R 1 , R 2 and R 3 is a substituent of a hydrogen atom of a ring, and each is independently a halogen atom, a nitro group, a cyano group, an amino group, a hydroxyl group, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an alkynyl group having 2 to 10 carbon atoms, an aryl group having 6 to 80 carbon atoms, or a combination of these groups which may include an ether bond, a keto bond, a sulfide bond, a sulfonyl group, a carboxyl group or an ester bond. 4 is an alkynyl group having 2 to 10 carbon atoms. n1, n2, and n3 are each an integer greater than or equal to 0 and less than or equal to the maximum number of substitutions that can be made on the ring. D represents a divalent organic group having a structure represented by the following formula (II) and / or formula (III).

[0024]

[0025] (In formula (II), R and R' each independently represent a hydrogen atom, an aromatic hydrocarbon group having 6 to 30 carbon atoms which may have a substituent, a heterocyclic group having 3 to 30 carbon atoms which may have a substituent, or a linear, branched or cyclic alkyl group having 10 or less carbon atoms which may have a substituent.)

[0026]

[0027] (In formula (III), X and Y may be bonded to the same carbon on Z or to different carbons, and each independently represents an aromatic hydrocarbon group having 6 to 30 carbon atoms which may have a substituent, or a linear, branched or cyclic alkyl group having 10 or less carbon atoms which may have a heteroatom or a substituent; Z forms a 4 to 12-membered monocyclic, bicyclic or tricyclic aromatic ring which may be fused, may have a substituent, or may contain a heteroatom; i and j each independently represent 0 or 1; p, q and k represent the number of bonds; p and q each independently represent 0 or 1; p and q are not both 0; and k represents an integer from 0 to 2.))

[0028] As a second aspect, in the resist underlayer film forming composition according to the first aspect, ring A and ring B are benzene rings or naphthalene rings, n1+n2+n3 is 0 to 2, and R 4 is propargyl,

[0029] According to a third aspect, in the resist underlayer film forming composition according to the second aspect, D is a divalent organic group including a fluorene or fluorene derivative structure and / or an aromatic hydrocarbon group having 6 to 30 carbon atoms which may have a substituent,

[0030] According to a fourth aspect, the resist underlayer film forming composition according to the first aspect further comprises a surfactant.

[0031] According to a fifth aspect, the resist underlayer film forming composition according to the first aspect further comprises a crosslinking agent.

[0032] According to a sixth aspect, the resist underlayer film forming composition according to the first aspect further comprises a surfactant and a crosslinking agent.

[0033] According to a seventh aspect, the resist underlayer film forming composition according to the first aspect further comprises an acid and / or a salt thereof and / or an acid generator.

[0034] According to an eighth aspect, the resist underlayer film forming composition according to the first aspect further comprises a surfactant, and an acid and / or a salt thereof and / or an acid generator,

[0035] As a ninth aspect, the resist underlayer film forming composition according to the first aspect further comprises a crosslinking agent, and an acid and / or a salt thereof and / or an acid generator,

[0036] As a tenth aspect, the resist underlayer film forming composition according to the first aspect further comprises a surfactant and a crosslinking agent, and an acid and / or a salt thereof and / or an acid generator,

[0037] As an eleventh aspect, a resist underlayer film is obtained by applying the resist underlayer film-forming composition according to any one of the first aspect to the tenth aspect onto a semiconductor substrate and firing the coating.

[0038] As a twelfth aspect, a method for manufacturing a semiconductor device comprises: a step of forming an underlayer film on a semiconductor substrate using the resist underlayer film-forming composition according to any one of the first aspect to the tenth aspect; a step of forming a resist film on the underlayer film; a step of forming a resist pattern by irradiating and developing the resist pattern with light or electron beams; a step of etching the underlayer film using the resist pattern; and a step of processing the semiconductor substrate using the patterned underlayer film.

[0039] As a 13th aspect, in the method for manufacturing a semiconductor device according to the 12th aspect, the resist film is patterned by a nanoimprint method or a self-assembled film.

[0040] As a 14th aspect, a method for manufacturing a semiconductor device comprises: a step of forming an underlayer film on a semiconductor substrate using the resist underlayer film-forming composition according to any one of the first aspect to the tenth aspect; a step of forming a hard mask on the underlayer film; a step of further forming a resist film on the hard mask; a step of forming a resist pattern by irradiating and developing with light or electron beams; a step of etching the hard mask using the resist pattern; a step of etching the underlayer film using the patterned hard mask; a step of removing the hard mask; and a step of processing the semiconductor substrate using the patterned underlayer film.

[0041] As a fifteenth aspect, in the method for manufacturing a semiconductor device according to the fourteenth aspect, the resist film is patterned by nanoimprinting or self-assembled film.

[0042] As a 16th aspect, the method for manufacturing a semiconductor device according to the 15th aspect further comprises: a step of forming a vapor-deposited film (spacer) on the lower film from which the hard mask is removed; a step of processing the formed vapor-deposited film (spacer) by etching; a step of removing the lower film; and a step of processing the semiconductor substrate through the spacer.

[0043] As a 17th aspect, in the method for manufacturing a semiconductor device according to the 16th aspect, the step of removing the hard mask is performed by etching or an alkaline chemical solution.

[0044] Effects of the Invention

[0045] The resist underlayer film-forming composition of the present invention can form a good resist pattern shape without causing mixing of the upper layer portion of the resist underlayer film and the layer coated thereon.

[0046] The resist underlayer film-forming composition of the present invention can provide a performance of effectively suppressing reflection from a substrate and also have an effect of serving as an antireflection film for exposure light.

[0047] The resist underlayer film-forming composition of the present invention can provide an excellent resist underlayer film that exhibits excellent etching resistance, good planarization properties and embedding properties in a micro-processed substrate, has resistance to solvents even in a nitrogen atmosphere, and exhibits sufficient curing characteristics.

[0048] As the resist pattern becomes finer, the resist is thinned to prevent the resist pattern from collapsing after development. Such a thin film resist includes: a process of transferring the resist pattern to its underlying film by an etching process, and processing the substrate using the underlying film as a mask; a process of transferring the resist pattern to its underlying film by an etching process, and further transferring the pattern transferred to the underlying film to the underlying film using a different gas composition, and finally processing the substrate. The resist underlayer film of the present invention and the composition for forming the same are effective in these processes. When a substrate is processed using the resist underlayer film of the present invention, the processed substrate (for example, a silicon dioxide film (SiO 2 Film), silicon nitride film (Si 3 N 4 film), polycrystalline silicon film, etc.) has sufficient etching resistance.

[0049] Furthermore, the resist underlayer film of the present invention can be used as a planarization film with good planarization and embedding properties, a resist underlayer film, a contamination prevention film of the resist layer, and a film of dry etching selectivity. Thus, resist pattern formation in the photolithography process of semiconductor manufacturing can be easily performed with good accuracy.

[0050] The present invention has a process of forming a resist underlayer film formed by a resist underlayer film-forming composition according to the present invention on a substrate, forming a hard mask thereon, forming a resist film thereon, forming a resist pattern by exposure and development, transferring the resist pattern to the hard mask, transferring the resist pattern transferred to the hard mask to the resist underlayer film, and processing a semiconductor substrate with the resist underlayer film. In this process, the hard mask is formed by a coating composition comprising an organic polymer, an inorganic polymer and a solvent, and by vacuum evaporation of an inorganic substance. For vacuum evaporation of an inorganic substance (e.g., silicon nitride oxide), the evaporation material is deposited on the surface of the resist underlayer film, and the temperature of the surface of the resist underlayer film rises to about 400°C. Since the polymer used in the present invention is a polymer having a unit structure of formula (I) or formula (I'), the heat resistance is extremely high, and thermal degradation does not occur by the deposition of the evaporation material. DETAILED DESCRIPTION

[0051] The present invention is a resist underlayer film-forming composition comprising a polymer having a unit structure of the following formula (I) or formula (I').

[0052] In the present invention, the above-mentioned resist underlayer film forming composition for lithography comprises the above-mentioned polymer and solvent. Furthermore, a crosslinking agent and an acid may be included, and additives such as an acid generator and a surfactant may be included as needed. The solid content of the composition is 0.1 to 70% by mass or 0.1 to 60% by mass. The solid content is the proportion of all components after removing the solvent from the resist underlayer film forming composition. The above-mentioned polymer may be contained in the solid content in a ratio of 1 to 100% by mass, or 1 to 99.9% by mass, or 50 to 99.9% by mass, or 50 to 95% by mass, or 50 to 90% by mass.

[0053] The weight average molecular weight of the polymer used in the present invention is 600 to 1,000,000, or 600 to 200,000.

[0054]

[0055] In formula (I) or formula (I'), ring A and ring B are aryl groups having 6 to 80 carbon atoms which may contain a heteroatom, and may have a cyclic structure containing an alkyl chain. 1 , R 2 , and R 3 is a substituent of a hydrogen atom of a ring, and each is independently a halogen atom, a nitro group, a cyano group, an amino group, a hydroxyl group, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an alkynyl group having 2 to 10 carbon atoms, an aryl group having 6 to 80 carbon atoms, or a combination of these groups which may include an ether bond, a keto bond, a sulfide bond, a sulfonyl group, a carboxyl group or an ester bond.4 is an alkynyl group having 2 to 10 carbon atoms. n1, n2, and n3 are each an integer greater than or equal to 0 and less than or equal to the maximum number of substitutions that can be made on the ring. D represents a divalent organic group having a structure represented by the following formula (II) and / or formula (III).

[0056]

[0057] (In formula (II), R and R' each independently represent a hydrogen atom, an aromatic hydrocarbon group having 6 to 30 carbon atoms which may have a substituent, a heterocyclic group having 3 to 30 carbon atoms which may have a substituent, or a linear, branched or cyclic alkyl group having 10 or less carbon atoms which may have a substituent.)

[0058]

[0059] (In formula (III), X and Y may be bonded to the same carbon on Z or to different carbons, and each independently represents an aromatic hydrocarbon group having 6 to 30 carbon atoms which may have a substituent, or a linear, branched or cyclic alkyl group having 10 or less carbon atoms which may have a heteroatom or a substituent; Z forms an aromatic ring which may be fused, may have a substituent, or may contain a heteroatom and is a 4 to 12-membered monocyclic, bicyclic or tricyclic ring; i and j each independently represent 0 or 1; p, q and k represent the number of bonds; p and q each independently represent 0 or 1; p and q are not both 0; and k represents an integer from 0 to 2.)

[0060] In formula (I) or formula (I'), R 1 , R 2 and R 3In the definition of , examples of the alkyl group having 1 to 10 carbon atoms include methyl, ethyl, n-propyl, isopropyl, cyclopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, cyclobutyl, 1-methyl-cyclopropyl, 2-methyl-cyclopropyl, n-pentyl, 1-methyl-n-butyl, 2-methyl-n-butyl, 3-methyl-n-butyl, 1,1-dimethyl-n-propyl, 1,2-dimethyl-n-propyl, 2,2-dimethyl-n-propyl, 1-ethyl-n-propyl, cyclopentyl, 1-methyl-cyclobutyl, 2-methyl-n-butyl, 1,2-dimethyl-cyclobutyl, 3-methyl-cyclobutyl, 1,2-dimethyl-cyclopropyl, 2,3-dimethyl-cyclopropyl, 1-ethyl-cyclopropyl, 2-ethyl-cyclopropyl, n-hexyl, 1-methyl-n-pentyl, 2-methyl-n-pentyl, 3-methyl-n-pentyl, 4-methyl-n-pentyl, 1,1-dimethyl-n-butyl, 1,2-dimethyl-n-butyl, 1,3-dimethyl-n-butyl, 2,2-dimethyl-n-butyl, 2,3-dimethyl-n-butyl, 3,3-dimethyl-n-butyl, 1- Ethyl-n-butyl, 2-ethyl-n-butyl, 1,1,2-trimethyl-n-propyl, 1,2,2-trimethyl-n-propyl, 1-ethyl-1-methyl-n-propyl, 1-ethyl-2-methyl-n-propyl, cyclohexyl, 1-methyl-cyclopentyl, 2-methyl-cyclopentyl, 3-methyl-cyclopentyl, 1-ethyl-cyclobutyl, 2-ethyl-cyclobutyl, 3-ethyl-cyclobutyl, 1,2-dimethyl-cyclobutyl, 1,3-dimethyl-cyclobutyl, 2,2-dimethyl-cyclobutyl, 2,3- Dimethyl-cyclobutyl, 2,4-dimethyl-cyclobutyl, 3,3-dimethyl-cyclobutyl, 1-n-propyl-cyclopropyl, 2-n-propyl-cyclopropyl, 1-isopropyl-cyclopropyl, 2-isopropyl-cyclopropyl, 1,2,2-trimethyl-cyclopropyl, 1,2,3-trimethyl-cyclopropyl, 2,2,3-trimethyl-cyclopropyl, 1-ethyl-2-methyl-cyclopropyl, 2-ethyl-1-methyl-cyclopropyl, 2-ethyl-2-methyl-cyclopropyl and 2-ethyl-3-methyl-cyclopropyl, etc.

[0061] Examples of the alkenyl group having 2 to 10 carbon atoms include vinyl, 1-propenyl, 2-propenyl, 1-methyl-1-vinyl, 1-butenyl, 2-butenyl, 3-butenyl, 2-methyl-1-propenyl, 2-methyl-2-propenyl, 1-ethylvinyl, 1-methyl-1-propenyl, 1-methyl-2-propenyl, 1-pentenyl, 2-pentenyl, 3-pentenyl, 4-pentenyl, 1-n-propylvinyl, 1-methyl-1-butenyl, 1-methyl-2-butenyl, 1-methyl-3-butenyl, 2-ethyl-2-propenyl, 2-methyl-1-butenyl, 2-methyl-2-butenyl, 2-methyl-3-butenyl. 1-butylene, 1-methyl-1-pentenyl, 1-methyl-2-pentenyl, 1-methyl-3-pentenyl, 1-methyl-4-pentenyl, 1-butylene, 2-methyl-1-pentenyl, 2-methyl-2-pentenyl, 2-methyl-3-pentenyl, 1-methyl-2-pentenyl, 1-methyl-3-pentenyl, 1-methyl-4-pentenyl, 1-butylene, 2-methyl-1-pentenyl, 2-methyl-2-pentenyl, 2-methyl-3-pentenyl , 2-methyl-4-pentenyl, 2-n-propyl-2-propenyl, 3-methyl-1-pentenyl, 3-methyl-2-pentenyl, 3-methyl-3-pentenyl, 3-methyl-4-pentenyl, 3-ethyl-3-butenyl, 4-methyl-1-pentenyl, 4-methyl-2-pentenyl, 4-methyl-3-pentenyl, 4-methyl-4-pentenyl, 1,1-dimethyl-2-butenyl, 1,1-dimethyl-3-butenyl, 1,2-dimethyl-1-butenyl, 1,2-dimethyl-2-butenyl, 1,2-dimethyl-3-butenyl, 1-methyl-2-ethyl-2-propenyl, 1-sec-butylvinyl, 1,3- dimethyl-1-butenyl, 1,3-dimethyl-2-butenyl, 1,3-dimethyl-3-butenyl, 1-isobutylvinyl, 2,2-dimethyl-3-butenyl, 2,3-dimethyl-1-butenyl, 2,3-dimethyl-2-butenyl, 2,3-dimethyl-3-butenyl, 2-isopropyl-2-propenyl, 3,3-dimethyl-1-butenyl, 1-ethyl-1-butenyl, 1-ethyl-2-butenyl, 1-ethyl-3-butenyl, 1-n-propyl-1-propenyl, 1-n-propyl-2-propenyl, 2-ethyl-1-butenyl, 2-ethyl-2-butenyl, 2-ethyl-3-butenyl, 1,1,2-Trimethyl-2-propenyl, 1-tert-butylvinyl, 1-methyl-1-ethyl-2-propenyl, 1-ethyl-2-methyl-1-propenyl, 1-ethyl-2-methyl-2-propenyl, 1-isopropyl-1-propenyl, 1-isopropyl-2-propenyl, 1-methyl-2-cyclopentenyl, 1-methyl-3-cyclopentenyl, 2-methyl-1-cyclopentenyl, 2-methyl-2-cyclopentenyl cyclopentenyl, 2-methyl-3-cyclopentenyl, 2-methyl-4-cyclopentenyl, 2-methyl-5-cyclopentenyl, 2-methylene-cyclopentyl, 3-methyl-1-cyclopentenyl, 3-methyl-2-cyclopentenyl, 3-methyl-3-cyclopentenyl, 3-methyl-4-cyclopentenyl, 3-methyl-5-cyclopentenyl, 3-methylene-cyclopentyl, 1-cyclohexenyl, 2-cyclohexenyl and 3-cyclohexenyl, etc.

[0062] Examples of the alkynyl group having 2 to 10 carbon atoms include the following structures.

[0063]

[0064] Examples of the alkoxy group having 1 to 10 carbon atoms include methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, sec-butoxy, tert-butoxy, n-pentyloxy, 1-methyl-n-butoxy, 2-methyl-n-butoxy, 3-methyl-n-butoxy, 1,1-dimethyl-n-propoxy, 1,2-dimethyl-n-propoxy, 2,2-dimethyl-n-propoxy, 1-ethyl-n-propoxy, n-hexyloxy, 1-methyl-n-pentyloxy, 2-methyl-n-pentyloxy, 3-methyl-n-butoxy, Pentyloxy, 4-methyl-n-pentyloxy, 1,1-dimethyl-n-butoxy, 1,2-dimethyl-n-butoxy, 1,3-dimethyl-n-butoxy, 2,2-dimethyl-n-butoxy, 2,3-dimethyl-n-butoxy, 3,3-dimethyl-n-butoxy, 1-ethyl-n-butoxy, 2-ethyl-n-butoxy, 1,1,2-trimethyl-n-propoxy, 1,2,2-trimethyl-n-propoxy, 1-ethyl-1-methyl-n-propoxy, and 1-ethyl-2-methyl-n-propoxy, etc.

[0065] Examples of the aryl group having 6 to 80 carbon atoms include phenyl, o-methylphenyl, m-methylphenyl, p-methylphenyl, o-chlorophenyl, m-chlorophenyl, p-chlorophenyl, o-fluorophenyl, p-fluorophenyl, o-methoxyphenyl, p-methoxyphenyl, p-nitrophenyl, p-cyanophenyl, α-naphthyl, β-naphthyl, o-biphenyl, m-biphenyl, p-biphenyl, 1-anthryl, 2-anthryl, 9-anthryl, 1-phenanthryl, 2-phenanthryl, 3-phenanthryl, 4-phenanthryl, 9-phenanthryl, and 1-pyrene.

[0066] The heterocyclic group is preferably an organic group consisting of a 5- to 6-membered heterocyclic ring containing nitrogen, sulfur and oxygen, and examples thereof include pyrrolyl, furyl, thienyl, imidazolyl, Azolyl, thiazolyl, pyrazolyl, iso Azolyl, isothiazolyl, pyridyl, etc.

[0067] Examples of the substituent include a halogen atom, a saturated or unsaturated straight-chain, branched or cyclic hydrocarbon group which may contain a heteroatom, a hydroxyl group, an amino group, a carboxyl group, a cyano group, a nitro group, an alkoxy group, an ester group, an amide group, a sulfonyl group, a thioether group, an ether group, an aryl group, and the like, but the substituent is not limited to these as long as the effects of the present invention are not impaired.

[0068] In formula (I) or formula (I'), R 4 , the following structures can be mentioned.

[0069]

[0070] The unit structure of formula (I) or formula (I') can be, for example, a benzene ring or a naphthalene ring is used as ring A and ring B, n1+n2+n3 is 0 to 2, and preferably R 4 The unit structure in the case of a propargyl group.

[0071] In the definitions of R and R' in formula (II), the "substituent" and "heterocyclic group" are as described above.

[0072] The aromatic hydrocarbon group having 6 to 30 carbon atoms is a group derived from an aromatic hydrocarbon compound by removing one or two hydrogen atoms. Such an aromatic hydrocarbon compound may be any of benzene, a ring-condensed aromatic hydrocarbon compound, and a ring-linked aromatic hydrocarbon compound.

[0073] Specific examples of the group derived from benzene include benzene-1,2-diyl, benzene-1,3-diyl, benzene-1,4-diyl, benzene-1,2,3-triyl, benzene-1,2,4-triyl and benzene-1,3,5-triyl.

[0074] Specific examples of the group derived from a ring-condensed aromatic hydrocarbon compound include naphthalene-1,2-diyl, naphthalene-1,3-diyl, naphthalene-1,4-diyl, naphthalene-1,5-diyl, naphthalene-1,6-diyl, naphthalene-1,7-diyl, naphthalene-1,8-diyl, naphthalene-2,3-diyl, naphthalene-2,6-diyl, naphthalene-2,7-diyl, anthracene-1,2-diyl, anthracene-1,3-diyl, anthracene-1,4-diyl, anthracene-1,5-diyl, anthracene-1,6-diyl, anthracene-1,7-diyl, anthracene-1,8-diyl, anthracene-1,9-diyl, anthracene-1,10-diyl, anthracene-2,3-diyl, anthracene-2,6-diyl, anthracene-2,7-diyl, anthracene-2,9-diyl, anthracene-2,10-diyl, anthracene-9 The present invention also includes groups derived from ring-condensed aromatic hydrocarbon compounds such as naphthalene-1,2,3-triyl, naphthalene-1,2,4-triyl, naphthalene-1,2,5-triyl, naphthalene-1,2,6-triyl, naphthalene-1,2,7-triyl, naphthalene-1,2,8-triyl, naphthalene-1,3,5-triyl, naphthalene-1,3,6-triyl, naphthalene-1,3,7-triyl, naphthalene-1,3,8-triyl, naphthalene-1,4,5-triyl, naphthalene-1,4,6-triyl, naphthalene-1,4,7-triyl, naphthalene-1,4,8-triyl, naphthalene-2,3,5-triyl, naphthalene-2,3,6-triyl, naphthalene-2,3,7-triyl and naphthalene-2,3,8-triyl, but is not limited to these.

[0075] Specific examples of the group derived from the ring-linked aromatic hydrocarbon compound include biphenyl-2,2'-diyl, biphenyl-2,3'-diyl, biphenyl-2,4'-diyl, biphenyl-3,3'-diyl, biphenyl-3,4'-diyl, biphenyl-4,4'-diyl, p-terphenyl-2,2'-diyl, p-terphenyl-2,3'-diyl, p-terphenyl-2,2"-diyl, p-terphenyl -2,3"-diyl, p-terphenyl-2,4"-diyl, p-terphenyl-3,2'-diyl, p-terphenyl-3,3'-diyl, p-terphenyl-3,3"-diyl, p-terphenyl-3,4"-diyl, p-terphenyl-4,4"-diyl, p-terphenyl-2',3'-diyl, p-terphenyl-2',5'-diyl, p-terphenyl-2',6'-diyl, etc. are aromatic rings connected. A group derived from a hydrocarbon compound, biphenyl-2,3,2'-triyl, biphenyl-2,3,3'-triyl, biphenyl-2,3,4'-triyl, biphenyl-2,4,2'-triyl, biphenyl-2,4,3'-triyl, biphenyl-2,4,4'-triyl, biphenyl-2,5,2'-triyl, biphenyl-2,5,3'-triyl, biphenyl-2,5,4'-triyl, biphenyl-2,6, The invention also includes groups derived from ring-linked aromatic hydrocarbon compounds such as biphenyl-2'-triyl, biphenyl-2,6,3'-triyl, biphenyl-2,6,4'-triyl, biphenyl-3,4,2'-triyl, biphenyl-3,4,3'-triyl, biphenyl-3,4,4'-triyl, biphenyl-3,5,2'-triyl, biphenyl-3,5,3'-triyl, and biphenyl-3,5,4'-triyl, but is not limited to these.

[0076] In the definitions of R and R' in formula (II), examples of "alkyl" include methyl, ethyl, n-propyl, isopropyl, cyclopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, cyclobutyl, 1-methyl-cyclopropyl, 2-methyl-cyclopropyl, n-pentyl, 1-methyl-n-butyl, 2-methyl-n-butyl, 3-methyl-n-butyl, 1,1-dimethyl-n-propyl, 1,2-dimethyl-n-propyl, 2,2-dimethyl-n-propyl, 1-ethyl-n-propyl, cyclopentyl, 1-methyl-cyclobutyl, 2-methyl-cyclobutyl, 3-methyl-cyclobutyl, 1,2-dimethyl-cyclopropyl, 2,3-dimethyl-cyclopropyl, 1-ethyl-cyclopropyl, 2-ethyl-cyclopropyl, n-hexyl, 1-methyl-n-pentyl, 2-methyl-n-pentyl, 3-methyl-n-pentyl, 4-methyl-n-pentyl, 1,1-dimethyl-n-butyl, 1,2-dimethyl-n-butyl, 1,3-dimethyl-n-butyl, 2,2-dimethyl-n-butyl, 2,3-dimethyl-n-butyl, 3,3-dimethyl-n-butyl, 1-ethyl- n-Butyl, 2-ethyl-n-butyl, 1,1,2-trimethyl-n-propyl, 1,2,2-trimethyl-n-propyl, 1-ethyl-1-methyl-n-propyl, 1-ethyl-2-methyl-n-propyl, cyclohexyl, 1-methyl-cyclopentyl, 2-methyl-cyclopentyl, 3-methyl-cyclopentyl, 1-ethyl-cyclobutyl, 2-ethyl-cyclobutyl, 3-ethyl-cyclobutyl, 1,2-dimethyl-cyclobutyl, 1,3-dimethyl-cyclobutyl, 2,2-dimethyl-cyclobutyl, 2,3-dimethyl-cyclobutyl, 2, 4-dimethyl-cyclobutyl, 3,3-dimethyl-cyclobutyl, 1-n-propyl-cyclopropyl, 2-n-propyl-cyclopropyl, 1-isopropyl-cyclopropyl, 2-isopropyl-cyclopropyl, 1,2,2-trimethyl-cyclopropyl, 1,2,3-trimethyl-cyclopropyl, 2,2,3-trimethyl-cyclopropyl, 1-ethyl-2-methyl-cyclopropyl, 2-ethyl-1-methyl-cyclopropyl, 2-ethyl-2-methyl-cyclopropyl, and 2-ethyl-3-methyl-cyclopropyl, n-heptyl, n-octyl, n-nonyl, and n-decyl.

[0077] Preferably, R and R' are each independently phenyl, naphthyl, anthracenyl, phenanthryl, naphthacene or pyrene.

[0078] If some specific examples of the divalent organic group including the structure represented by formula (II) are given, they are as follows: One of the two * represents a bonding site with the pentazolyl group. It goes without saying that the structure illustrated may be included in part of the whole.

[0079]

[0080] In formula (III), X and Y may be bonded to the same carbon on Z or to different carbons, and each independently represents an aromatic hydrocarbon group having 6 to 30 carbon atoms which may have a substituent, or a linear, branched or cyclic alkyl group having 10 or less carbon atoms which may have a heteroatom or a substituent, Z forms an aromatic ring which may be fused, may have a substituent, or may contain a heteroatom and is a 4 to 12-membered monocyclic, bicyclic or tricyclic ring, i and j each independently represent 0 or 1, p, q and k represent the number of bonding bonds, p and q each independently represent 0 or 1, p and q are not 0 at the same time, and k represents an integer of 0 to 2. The aromatic hydrocarbon group is divalent. The "aromatic hydrocarbon" is as described above.

[0081] In formula (III), examples of Z as a 4- to 12-membered monocyclic ring include cyclopropane, cyclobutane, cyclopentane, cyclohexane, cyclohexene, etc., examples of bicyclic rings include dicyclopentane, dicyclooctane, dicycloheptene, etc., and examples of tricyclic rings include tricyclooctane, tricyclononane, tricyclodecane, etc.

[0082] Examples of the aromatic ring that may be fused with a monocyclic, bicyclic or tricyclic ring include a benzene ring, a naphthalene ring, an anthracene ring, a pyrene ring, etc. These may be fused with one or more rings.

[0083] If some specific examples of the divalent organic group including the structure represented by formula (III) are given, they are as follows. The bonding site with the group B is not particularly limited. It goes without saying that the structure shown in the example may be included in part of the whole.

[0084]

[0085]

[0086] D in formula (I) or (I') is preferably a divalent organic group including a fluorene or fluorene derivative structure and / or an aromatic hydrocarbon group having 6 to 30 carbon atoms which may have a substituent. Here, the fluorene derivative structure refers to a structure having a fluorene skeleton.

[0087] D in the formula (I) or (I′) has, for example, the following structure as a part of D.

[0088]

[0089] Examples of the indole derivatives in the formula (I) or (I') (parts other than D in the formula (I) or (I')) include the following, but are not limited to the following.

[0090]

[0091]

[0092]

[0093]

[0094]

[0095]

[0096]

[0097]

[0098] In the present invention, the unit structure of formula (I) or (I′) forms a novolac resin between a heterocyclic compound containing ring A and ring B (aromatic compound containing a heterocyclic group) and aldehydes or ketones.

[0099] Examples of the aldehydes used in the production of the polymer of the present invention include formaldehyde, paraformaldehyde, acetaldehyde, propionaldehyde, butyraldehyde, isobutyraldehyde, valeraldehyde, caproaldehyde, 2-methylbutyraldehyde, hexaaldehyde, undecanal, 7-methoxy-3,7-dimethyloctanal, cyclohexanal, 3-methyl-2-butyraldehyde, glyoxal, malondialdehyde, succinaldehyde, valeraldehyde, caproaldehyde, 2-methylbutyraldehyde, hexaaldehyde, undecanal, 7-methoxy-3,7-dimethyloctanal, cyclohexanal, 3-methyl-2-butyraldehyde, glyoxal, malondialdehyde, succinaldehyde, valeraldehyde, 2-methylbutyraldehyde, hexaaldehyde, 2-methylbutyr ... Saturated aliphatic aldehydes such as dialdehyde, adipaldehyde, unsaturated aliphatic aldehydes such as acrolein and methacrolein, heterocyclic aldehydes such as furfural and pyridinealdehyde, benzaldehyde, naphthaldehyde, anthracenealdehyde, phenanthraldehyde, salicylaldehyde, phenylacetaldehyde, 3-phenylpropanal, tolualdehyde, (N,N-dimethylamino)benzaldehyde, acetoxybenzaldehyde, 1-pyrenecarboxaldehyde, anisaldehyde, terephthalaldehyde and the like. Aromatic aldehydes can be particularly preferably used.

[0100] The ketones used in the production of the polymer of the present invention are diaryl ketones, and examples thereof include diphenyl ketone, phenyl naphthyl ketone, dinaphthyl ketone, phenyl tolyl ketone, xylyl ketone, and 9-fluorenone.

[0101] The phenolic varnish resin having a repeating unit structure can be prepared by a known method. For example, it can be prepared by condensing a ring-containing compound represented by HAH with an oxygen-containing compound represented by OHC-B, O=CB, HO-B-OH, RO-B-OR, etc. (wherein, A and B have the same meaning as the above-mentioned ring A and ring B. R represents a halogen atom, or an alkyl group having about 1 to 3 carbon atoms). One type of the ring-containing compound and the oxygen-containing compound can be used alone, or two or more types can be used in combination. In the condensation reaction, the oxygen-containing / nitrogen-containing compound can be used in a ratio of 0.1 to 10 moles, preferably 0.1 to 2 moles, relative to 1 mole of the ring-containing compound.

[0102] Examples of the catalyst used in the condensation reaction include inorganic acids such as sulfuric acid, phosphoric acid, and perchloric acid; organic sulfonic acids such as p-toluenesulfonic acid, p-toluenesulfonic acid monohydrate, methanesulfonic acid, and trifluoromethanesulfonic acid; and carboxylic acids such as formic acid and oxalic acid.

[0103] The amount of the catalyst used varies depending on the type of catalyst used, but is usually 0.001 to 10,000 parts by mass, preferably 0.01 to 1,000 parts by mass, and more preferably 0.05 to 100 parts by mass, based on 100 parts by mass of the ring-containing compound (or the total of the ring-containing compound when there are two or more).

[0104] The condensation reaction can be carried out without a solvent, but is usually carried out using a solvent. The solvent is not particularly limited as long as it can dissolve the reaction substrate and does not hinder the reaction. Examples thereof include 1,2-dimethoxyethane, diethylene glycol dimethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, tetrahydrofuran, diethylene glycol dimethyl ether, diethylene glycol monomethyl ether acetate, diethylene glycol dimethyl ether ... Alkane, 1,2-dichloromethane, 1,2-dichloroethane, toluene, N-methylpyrrolidone, dimethylformamide, etc.

[0105] The reaction temperature during condensation is usually 40° C. to 200° C. The reaction time is variously selected depending on the reaction temperature, but is usually about 30 minutes to 50 hours.

[0106] The weight average molecular weight Mw of the polymer obtained as described above is usually 500 to 1,000,000, or 600 to 200,000.

[0107] Examples of the polymer having a unit structure of formula (I) or formula (I') include the following.

[0108]

[0109]

[0110]

[0111]

[0112]

[0113]

[0114]

[0115]

[0116]

[0117]

[0118]

[0119]

[0120]

[0121]

[0122]

[0123] The above-mentioned polymers may be used by mixing other polymers in an amount of up to 50% by mass of the total polymers.

[0124] Examples of these polymers include polyacrylate compounds, polymethacrylate compounds, polyacrylamide compounds, polymethacrylamide compounds, polyvinyl compounds, polystyrene compounds, polymaleimide compounds, polymaleic anhydride, and polyacrylonitrile compounds.

[0125] Examples of the raw material monomers of the polyacrylate compound include methyl acrylate, ethyl acrylate, isopropyl acrylate, benzyl acrylate, naphthyl acrylate, anthracene acrylate, anthracene methyl acrylate, phenyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2,2,2-trifluoroethyl acrylate, 4-hydroxybutyl acrylate, isobutyl acrylate, tert-butyl acrylate, cyclohexyl acrylate, isobornyl acrylate, 2-methoxyethyl acrylate, methoxytriethylene glycol acrylate, 2-ethoxyethyl acrylate, tetrahydrofurfuryl acrylate, 3-methoxybutyl acrylate, 2-methyl-2-adamantyl acrylate, 2-ethyl-2-adamantyl acrylate, 2-propyl-2-adamantyl acrylate, 2-methoxybutyl-2-adamantyl acrylate, 8-methyl-8-tricyclodecanyl acrylate, 8-ethyl-8-tricyclodecanyl acrylate, and 5-acryloyloxy-6-hydroxynorbornene-2-carboxy-6-lactone.

[0126] Examples of the raw material monomer of the polymethacrylate compound include ethyl methacrylate, n-propyl methacrylate, n-pentyl methacrylate, cyclohexyl methacrylate, benzyl methacrylate, naphthyl methacrylate, anthracene methacrylate, anthracene methyl methacrylate, phenyl methacrylate, 2-phenylethyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 2,2,2-trifluoroethyl methacrylate, 2,2,2-trichloroethyl methacrylate, methyl acrylate, isobutyl methacrylate, 2-ethylhexyl methacrylate, isodecyl methacrylate, n-lauryl methacrylate, n-stearyl methacrylate, methoxydiglycol methacrylate, and methoxypolyethylene glycol. Methacrylate, tetrahydrofurfuryl methacrylate, isobornyl methacrylate, tert-butyl methacrylate, isostearyl methacrylate, n-butoxyethyl methacrylate, 3-chloro-2-hydroxypropyl methacrylate, 2-methyl-2-adamantyl methacrylate, 2-ethyl-2-adamantyl methacrylate, 2-propyl-2-adamantyl methacrylate, 2-methoxybutyl-2-adamantyl methacrylate, 8-methyl-8-tricyclodecanyl methacrylate, 8-ethyl-8-tricyclodecanyl methacrylate, 5-methacryloyloxy-6-hydroxynorbornene-2-carboxy-6-lactone, and 2,2,3,3,4,4,4-heptafluorobutyl methacrylate, etc.

[0127] Examples of the raw material monomer of the acrylamide compound include acrylamide, N-methylacrylamide, N-ethylacrylamide, N-benzylacrylamide, N-phenylacrylamide, and N,N-dimethylacrylamide.

[0128] Examples of the raw material monomer of the polymethacrylic acid amide compound include methacrylamide, N-methylmethacrylamide, N-ethylmethacrylamide, N-benzylmethacrylamide, N-phenylmethacrylamide, and N,N-dimethylmethacrylamide.

[0129] Examples of the raw material monomer of the polyvinyl compound include vinyl ether, methyl vinyl ether, benzyl vinyl ether, 2-hydroxyethyl vinyl ether, phenyl vinyl ether, and propyl vinyl ether.

[0130] Examples of the raw material monomer of the polystyrene compound include styrene, methylstyrene, chlorostyrene, bromostyrene, and hydroxystyrene.

[0131] Examples of the raw material monomer of the polymaleimide compound include maleimide, N-methylmaleimide, N-phenylmaleimide, and N-cyclohexylmaleimide.

[0132] These polymers can be prepared by dissolving an addition polymerizable monomer and a chain transfer agent (10% or less relative to the mass of the monomer) in an organic solvent, adding a polymerization initiator to carry out a polymerization reaction, and then adding a polymerization inhibitor. The amount of the polymerization initiator added is 1 to 10% relative to the mass of the monomer, and the amount of the polymerization inhibitor added is 0.01 to 0.2% by mass. As the organic solvent used, propylene glycol monomethyl ether, propylene glycol monopropyl ether, ethyl lactate, cyclohexanone, methyl ethyl ketone, and dimethylformamide can be mentioned, as the chain transfer agent, dodecanethiol and dodecyl mercaptan can be mentioned, as the polymerization initiator, azobisisobutyronitrile and azobiscyclohexanecarbonitrile can be mentioned, and further, as the polymerization inhibitor, 4-methoxyphenol can be mentioned. As the reaction temperature, it is appropriately selected from 30 to 100° C., and as the reaction time, it is appropriately selected from 1 to 48 hours.

[0133] [Solvent]

[0134] The resist underlayer film forming composition according to the present invention contains a solvent. The solvent is not particularly limited as long as it can dissolve the compound containing an aromatic ring and any components added as needed. In particular, since the resist underlayer film forming composition according to the present invention is used in a uniform solution state, it is recommended to use a solvent generally used in a photolithography process in combination if its coating performance is taken into consideration.

[0135] Examples of such solvents include methyl cellosolve acetate, ethyl cellosolve acetate, propylene glycol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, methyl isobutyl carbinol, propylene glycol monobutyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, propylene glycol monobutyl ether acetate, toluene, xylene, methyl ethyl ketone, cyclopentanone, cyclohexanone, ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, ethyl ethoxylate, ethyl hydroxylate, methyl 2-hydroxy-3-methylbutyrate, methyl 3-methoxypropionate, methyl 3-methoxypropionate, Ethyl propionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monopropyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, diethylene glycol dibutyl ether, propylene glycol monomethyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, propylene glycol dipropyl ether, propylene glycol dibutyl ether, ethyl lactate, propyl lactate, isopropyl lactate, butyl lactate, isobutyl lactate Esters, methyl formate, ethyl formate, propyl formate, isopropyl formate, butyl formate, isobutyl formate, pentyl formate, isoamyl formate, methyl acetate, ethyl acetate, pentyl acetate, isoamyl acetate, hexyl acetate, methyl propionate, ethyl propionate, propyl propionate, isopropyl propionate, butyl propionate, isobutyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, isopropyl butyrate, butyl butyrate, isobutyl butyrate, ethyl hydroxyacetate, ethyl 2-hydroxy-2-methylpropionate, methyl 3-methoxy-2-methylpropionate, methyl 2-hydroxy-3-methylbutyrate, methyl 2-hydroxyisobutyrate, ethyl methoxyacetate, ethyl ethoxyacetate Ester, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate, 3-methoxybutyl acetate, 3-methoxypropyl acetate, 3-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxybutyl propionate, 3-methyl-3-methoxybutyl butyrate, methyl acetoacetate, toluene, xylene, methyl ethyl ketone, methyl propyl ketone, methyl butyl ketone, 2-heptanone, 3-heptanone, 4-heptanone, cyclohexanone, N,N-dimethylformamide, N-methylacetamide, N,N-dimethylacetamide, N-methylpyrrolidone, 4-methyl-2-pentanol, and γ-butyrolactone. These solvents can be used alone or in combination of two or more.

[0136] Among them, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, ethyl lactate, cyclohexanone, and methyl 2-hydroxyisobutyrate are more preferred, and propylene glycol monomethyl ether and propylene glycol monomethyl ether acetate are even more preferred.

[0137] In addition, a solvent having a boiling point of 160° C. or higher may be contained. For example, the following compounds described in WO2018 / 131562A1 can be used.

[0138]

[0139] (R in formula (i) 1 , R 2 and R 3 Each represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms which may be interrupted by an oxygen atom, a sulfur atom or an amide bond, and may be the same or different from each other and may be bonded to each other to form a ring structure.

[0140] The resist underlayer film forming composition according to the present invention may contain any components other than those described above. Each component will be described below.

[0141] [Crosslinking agent]

[0142] The resist underlayer film forming composition of the present invention may include a crosslinking agent. As the crosslinking agent, melamine-based, substituted urea-based, or polymers thereof may be cited. Preferably, the crosslinking agent has at least two crosslinking substituents, such as methoxymethylated glycoluril (e.g., tetramethoxymethyl glycoluril), butoxymethylated glycoluril, methoxymethylated melamine, butoxymethylated melamine, methoxymethylated benzoguanamine, butoxymethylated benzoguanamine, methoxymethylated urea, butoxymethylated urea, or methoxymethylated thiourea. In addition, condensates of these compounds may also be used.

[0143] As the crosslinking agent, a crosslinking agent with high heat resistance can be used. As the crosslinking agent with high heat resistance, a compound containing a crosslinking-forming substituent having an aromatic ring (for example, a benzene ring or a naphthalene ring) in the molecule can be preferably used.

[0144] Examples of the compound include a compound having a partial structure of the following formula (4) and a polymer or oligomer having a repeating unit of the following formula (5).

[0145]

[0146] The above R 11 , R 12 , R 13 , and R 14It is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and the alkyl groups exemplified above can be used. n1 is an integer of 1 to 4, n2 is an integer of 1 to (5-n1), and (n1+n2) represents an integer of 2 to 5. n3 is an integer of 1 to 4, n4 is 0 to (4-n3), and (n3+n4) represents an integer of 1 to 4. The oligomer and polymer can be used in the range of 2 to 100 or 2 to 50 repeating unit structures.

[0147] The compounds, polymers and oligomers of formula (4) and formula (5) are exemplified below.

[0148]

[0149]

[0150] R: -H or -CH(CH 3 )CH 2 OCH 3

[0151] The above compounds can be obtained as products of Asahi Organic Materials Industries, Ltd. and Honshu Chemical Industries, Ltd. For example, among the above crosslinking agents, the compound of formula (4-23) can be obtained as Honshu Chemical Industries, Ltd. under the trade name TMOM-BP, and the compound of formula (4-20) can be obtained as Asahi Organic Materials Industries, Ltd. under the trade name TM-BIP-A.

[0152] The amount of the crosslinking agent added varies depending on the coating solvent used, the substrate used, the required solution viscosity, the required film shape, etc., but is 0.001 mass % or more, 0.01 mass % or more, 0.05 mass % or more, 0.5 mass % or more, or 1.0 mass % or more, and 80 mass % or less, 50 mass % or less, 40 mass % or less, 20 mass % or less, or 10 mass % or less relative to the total solid content. Although these crosslinking agents sometimes undergo a crosslinking reaction caused by self-condensation, when there is a crosslinking substituent in the compound containing the aromatic ring of the present invention, a crosslinking reaction can occur with these crosslinking substituents.

[0153] [Acid and / or its salt and / or acid generator]

[0154] The resist underlayer film-forming composition according to the present invention may contain an acid and / or a salt thereof and / or an acid generator.

[0155] Examples of the acid include p-toluenesulfonic acid, trifluoromethanesulfonic acid, salicylic acid, 5-sulfosalicylic acid, 4-phenolsulfonic acid, camphorsulfonic acid, 4-chlorobenzenesulfonic acid, benzenedisulfonic acid, 1-naphthalenesulfonic acid, citric acid, benzoic acid, hydroxybenzoic acid, and naphthoic acid.

[0156] As the salt, the salt of the above acid can also be used. The salt is not limited, but ammonia derivative salts such as trimethylamine salt and triethylamine salt, pyridine derivative salt, morpholine derivative salt, etc. can be preferably used.

[0157] The acid and / or its salt may be used alone or in combination of two or more thereof. The amount thereof is usually 0.0001 to 20% by mass, preferably 0.0005 to 10% by mass, and more preferably 0.01 to 5% by mass, based on the total solid content.

[0158] Examples of the acid generator include a thermal acid generator and a photoacid generator.

[0159] Examples of the thermal acid generator include organic sulfonic acid alkyl esters such as 2,4,4,6-tetrabromocyclohexadienone, benzoin toluenesulfonate, 2-nitrobenzyl toluenesulfonate, K-PURE [registered trademark] CXC-1612, K-PURE CXC-1614, K-PURE TAG-2172, K-PURE TAG-2179, K-PURE TAG-2678, K-PURE TAG2689, and K-PURE TAG2700 (manufactured by King Industries), and SI-45, SI-60, SI-80, SI-100, SI-110, and SI-150 (manufactured by Sanshin Chemical Industry Co., Ltd.).

[0160] The photoacid generator generates acid when the resist is exposed. Therefore, the acidity of the lower film can be adjusted. This is a method for making the acidity of the lower film consistent with the acidity of the upper resist. In addition, by adjusting the acidity of the lower film, the pattern shape of the resist formed on the upper layer can be adjusted.

[0161] Examples of the photoacid generator contained in the resist underlayer film-forming composition of the present invention include: Salt compounds, sulfonimide compounds, and disulfonyldiazomethane compounds, etc.

[0162] As Salt compounds, such as diphenyl iodide Hexafluorophosphate, diphenyl iodide Trifluoromethanesulfonate, diphenyl iodide Nonafluorobutane sulfonate, diphenyl iodide Perfluorooctane sulfonate, diphenyl iodide Camphorsulfonate, bis(4-tert-butylphenyl)iodide Camphorsulfonate and bis(4-tert-butylphenyl)iodide Trifluoromethanesulfonate and other iodine Sulfonium salt compounds, and sulfonium salt compounds such as triphenylsulfonium hexafluoroantimonate, triphenylsulfonium nonafluoro-n-butanesulfonate, triphenylsulfonium camphorsulfonate and triphenylsulfonium trifluoromethanesulfonate.

[0163] Examples of the sulfonyl imide compound include N-(trifluoromethanesulfonyloxy)succinimide, N-(nonafluoro-n-butanesulfonyloxy)succinimide, N-(camphorsulfonyloxy)succinimide, and N-(trifluoromethanesulfonyloxy)naphthalimide.

[0164] Examples of the disulfonyldiazomethane compound include bis(trifluoromethylsulfonyl)diazomethane, bis(cyclohexylsulfonyl)diazomethane, bis(phenylsulfonyl)diazomethane, bis(p-toluenesulfonyl)diazomethane, bis(2,4-dimethylbenzenesulfonyl)diazomethane, and methylsulfonyl-p-toluenesulfonyldiazomethane.

[0165] The acid generator may be used alone or in combination of two or more.

[0166] When the acid generator is used, the ratio thereof is 0.01 to 10 parts by mass, or 0.1 to 8 parts by mass, or 0.5 to 5 parts by mass based on 100 parts by mass of the solid content of the resist underlayer film-forming composition.

[0167] [Other ingredients]

[0168] The resist underlayer film-forming composition of the present invention may contain a surfactant in order to prevent pinholes, streaks, and the like from being generated and to further improve coating properties on uneven surfaces. Examples of the surfactant include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene cetyl ether, and polyoxyethylene oleyl ether; polyoxyethylene alkyl aryl ethers such as polyoxyethylene octylphenol ether and polyoxyethylene nonylphenol ether; polyoxyethylene / polyoxypropylene block copolymers; sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan trioleate, and sorbitan tristearate; and sorbitan fatty acid esters such as polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan trioleate, and polyoxyethylene sorbitan tristearate. Polyoxyethylene sorbitan fatty acid esters and other non-ionic surfactants, such as acid esters, Efutur EF301, EF303, EF352 (manufactured by Tofu Co., Ltd. , trade name), メガファック F171, F173, R-40, R-40N, R-40LM (made by DIC Co., Ltd., trade name), フロラード FC430, F Fluorine-based surfactants such as C431 (made by Sumitomo Silamide Co., Ltd., trade name), Asahigard AG710, Surflon S-382, SC101, SC102, SC103, SC104, SC105, and SC106 (made by Asahi Glass Co., Ltd., trade name), and organosiloxane polymer KP341 (made by Shin-Etsu Chemical Co., Ltd.) are used. The amount of these surfactants mixed is usually 2.0% by mass or less, preferably 1.0% by mass or less, relative to the total solid content of the resist underlayer film-forming composition. These surfactants can be used alone or in combination of two or more. When using a surfactant, as its ratio, it is 0.0001 to 5 parts by mass, or 0.001 to 1 part by mass, or 0.01 to 0.5 parts by mass relative to 100 parts by mass of the solid content of the resist underlayer film-forming composition.

[0169] The resist underlayer film-forming composition of the present invention may contain a light absorber, a rheology modifier, an adhesion promoter, etc. The rheology modifier is effective in improving the fluidity of the underlayer film-forming composition. The adhesion promoter is effective in improving the adhesion between the semiconductor substrate or the resist and the underlayer film.

[0170] As the light absorber, for example, commercially available light absorbers described in "Industrial Colorant Technology and Market" (published by CMC) and "Dye Handbook" (edited by the Society of Synthetic Organic Chemistry) can be suitably used, for example, CI Disperse Yellow 1, 3, 4, 5, 7, 8, 13, 23, 31, 49, 50, 51, 54, 60, 64, 66, 68, 79, 82, 88, 90, 93, 102, 114 and 124; CI Disperse Orange 1, 5, 13, CI Disperse Red 1, 5, 7, 13, 17, 19, 43, 50, 54, 58, 65, 72, 73, 88, 117, 137, 143, 199, and 210; CI Disperse Violet 43; CI Disperse Blue 96; CI Fluorescent Brighteners 112, 135, and 163; CI Solvent Orange 2 and 45; CI Solvent Red 1, 3, 8, 23, 24, 25, 27, and 49; CI Pigment Green 10; CI Pigment Brown 2, etc. The light absorber is usually blended in a ratio of 10% by mass or less, preferably 5% by mass or less, based on the total solid content of the resist underlayer film-forming composition.

[0171] The rheology modifier is mainly added for the purpose of improving the fluidity of the resist underlayer film-forming composition, especially improving the film thickness uniformity of the resist underlayer film in the baking process, and improving the filling property of the resist underlayer film-forming composition into the inside of the hole. As specific examples, phthalic acid derivatives such as dimethyl phthalate, diethyl phthalate, diisobutyl phthalate, dihexyl phthalate, and butylisodecyl phthalate, adipic acid derivatives such as di-n-butyl adipate, diisobutyl adipate, diisooctyl adipate, and octyldecyl adipate, maleic acid derivatives such as di-n-butyl maleate, diethyl maleate, and dinonyl maleate, oleic acid derivatives such as methyl oleate, butyl oleate, and tetrahydrofurfuryl oleate, or stearic acid derivatives such as n-butyl stearate and glyceryl stearate can be cited. These rheology control agents are usually blended in a ratio of less than 30% by mass based on the total solid content of the resist underlayer film-forming composition.

[0172] The adhesion aid is mainly added for the purpose of improving the adhesion between the substrate or the resist and the resist underlayer film-forming composition, and in particular, for the purpose of preventing the resist from peeling off during development. Specific examples include chlorosilanes such as trimethylchlorosilane, dimethylhydroxymethylchlorosilane, methyldiphenylchlorosilane, and chloromethyldimethylchlorosilane; alkoxysilanes such as trimethylmethoxysilane, dimethyldiethoxysilane, methyldimethoxysilane, dimethylhydroxymethylethoxysilane, diphenyldimethoxysilane, and phenyltriethoxysilane; silazanes such as hexamethyldisilazane, N,N'-bis(trimethylsilyl)urea, dimethyltrimethylsilylamine, and trimethylsilylimidazole; silanes such as hydroxymethyltrichlorosilane, γ-chloropropyltrimethoxysilane, γ-aminopropyltriethoxysilane, and γ-glycidoxypropyltrimethoxysilane; benzotriazole, benzimidazole, indazole, imidazole, 2-mercaptobenzimidazole, 2-mercaptobenzothiazole, and 2-mercaptobenzothiazole. Heterocyclic compounds such as azole, urea, thiouracil, mercaptoimidazole, and mercaptopyrimidine, urea such as 1,1-dimethylurea and 1,3-dimethylurea, or thiourea compounds. These adhesion promoters are usually mixed in a ratio of less than 5% by mass, preferably less than 2% by mass, relative to the total solid content of the resist underlayer film forming composition.

[0173] The solid content of the resist underlayer film forming composition of the present invention is usually 0.1 to 70% by mass, preferably 0.1 to 60% by mass. The solid content is the content ratio of all components after removing the solvent from the resist underlayer film forming composition. The proportion of the above-mentioned aromatic ring-containing compound in the solid content is preferably 1 to 100% by mass, 1 to 99.9% by mass, 50 to 99.9% by mass, 50 to 95% by mass, and 50 to 90% by mass, respectively.

[0174] The resist used in the present invention is a photoresist or an electron beam resist.

[0175] As the photoresist to be coated on the upper part of the photolithography resist underlayer film in the present invention, both negative and positive types can be used, and there are positive photoresists composed of novolac resin and 1,2-naphthoquinonediazosulfonate, chemically amplified photoresists composed of a binder having a group whose alkali dissolution rate increases when decomposed by acid and a photoacid generator, chemically amplified photoresists composed of an alkali-soluble binder, a low molecular compound whose alkali dissolution rate increases when decomposed by acid, and a photoacid generator, chemically amplified photoresists composed of a binder having a group whose alkali dissolution rate increases when decomposed by acid, a low molecular compound whose alkali dissolution rate increases when decomposed by acid, and a photoacid generator, photoresists having Si atoms in the skeleton, and the like, for example, manufactured by Lombard Hards Co., Ltd., trade name APEX-E.

[0176] In addition, as the electron beam resist to be coated on the upper part of the photolithography resist underlayer film in the present invention, for example, a composition composed of a resin containing Si-Si bonds in the main chain and aromatic rings at the ends and an acid generator that generates an acid by electron beam irradiation, or a composition composed of poly(p-hydroxystyrene) in which a hydroxyl group is substituted with an organic group containing N-carboxyamine and an acid generator that generates an acid by electron beam irradiation, etc. In the latter electron beam resist composition, the acid generated from the acid generator by electron beam irradiation reacts with the N-carboxyaminooxy group of the polymer side chain, and the polymer side chain is decomposed into a hydroxyl group, showing alkali solubility and dissolving in an alkaline developer, forming a resist pattern. Examples of the acid generator that generates an acid by irradiation with electron beams include halogenated organic compounds such as 1,1-bis[p-chlorophenyl]-2,2,2-trichloroethane, 1,1-bis[p-methoxyphenyl]-2,2,2-trichloroethane, 1,1-bis[p-chlorophenyl]-2,2-dichloroethane, and 2-chloro-6-(trichloromethyl)pyridine, triphenylsulfonium salts, and diphenyliodonium. Salt, etc. salts, sulfonates such as nitrobenzyl tosylate and dinitrobenzyl tosylate.

[0177] As a developer for resists with resist lower films formed using resist lower film materials for photolithography of the present invention, aqueous solutions of alkalis such as inorganic alkalis such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate, ammonia water, primary amines such as ethylamine, n-propylamine, secondary amines such as diethylamine, di-n-butylamine, tertiary amines such as triethylamine, methyldiethylamine, alcohol amines such as dimethylethanolamine, triethanolamine, quaternary ammonium salts such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, choline, cyclic amines such as pyrroles and piperidine can be used. Further, it is also possible to add an appropriate amount of alcohols such as isopropanol, nonionic surfactants and the like in the aqueous solution of the above-mentioned alkalis and use them. Preferred developer among them is a quaternary ammonium salt, and more preferably tetramethylammonium hydroxide and choline.

[0178] Next, the resist pattern forming method of the present invention will be described. In the case of a substrate (e.g., a silicon wafer substrate, a silicon dioxide substrate (SiO 2After coating the resist underlayer film-forming composition on substrates, silicon nitride substrates (SiN substrates), silicon nitride oxide substrates (SiON substrates), titanium nitride substrates (TiN substrates), tungsten substrates (W substrates), glass substrates, ITO substrates, polyimide substrates, and low dielectric constant material (low-k material) coated substrates by a suitable coating method such as a spin coater or a coater, the composition is fired to solidify it to produce a coated underlayer film. As firing conditions, a firing temperature of 80°C to 600°C and a firing time of 0.3 to 60 minutes are appropriately selected in an atmosphere of an inert gas such as air or nitrogen or argon. Preferably, the firing temperature is 150°C to 400°C and the firing time is 0.5 to 2 minutes. Here, the film thickness of the formed underlayer film is, for example, 10 to 1000nm, or 20 to 500nm, or 30 to 400nm, or 50 to 300nm. Then, after forming a film of one to several layers of coating material directly on the resist lower film or on the coating type lower film as needed, a resist is applied, irradiated with light or electron beams through a specified mask, developed, rinsed, and dried to obtain a good resist pattern. Post-irradiation heating (PEB: PostExposureBake) of light or electron beams can also be performed as needed. Furthermore, the resist lower film where the resist is developed and removed by the above process can be removed by dry etching to form a desired pattern on the substrate.

[0179] The exposure light for the photoresist is a chemical radiation such as near ultraviolet, far ultraviolet, or extreme ultraviolet (e.g., EUV, wavelength 13.5 nm), for example, 248 nm (KrF laser), 193 nm (ArF laser), 157 nm (F 2 In the light irradiation, any method can be used without particular limitation as long as it can generate acid from the photoacid generator, and the exposure amount is 1 to 2000 mJ / cm 2 , or 10~1500mJ / cm 2 , or 50~1000mJ / cm 2 .

[0180] The electron beam resist can be irradiated with electron beams using, for example, an electron beam irradiation device.

[0181] In the present invention, a semiconductor device can be manufactured through the following steps: a step of forming a resist underlayer film on a semiconductor substrate using a resist underlayer film-forming composition; a step of forming a resist film on the above-mentioned resist underlayer film; a step of forming a resist pattern by light or electron beam irradiation and development; a step of etching the resist underlayer film using the resist pattern; and a step of processing a semiconductor substrate using the patterned resist underlayer film.

[0182] In the present invention, after forming the resist underlayer film of the present invention on the substrate, the resist can be applied after forming one to several layers of coating material directly on the resist underlayer film or as needed. The pattern width of the resist is thereby narrowed, and even when the resist is thinly coated to prevent pattern collapse, the substrate can be processed by selecting an appropriate etching gas.

[0183] That is, a semiconductor device can be manufactured through the following steps: a step of forming a resist underlayer film on a semiconductor substrate using a resist underlayer film-forming composition; a step of forming a hard mask formed of a coating material containing a silicon component or the like or a hard mask formed by vapor deposition (for example, silicon nitride oxide) on the above-mentioned resist underlayer film; a step of further forming a resist film on the hard mask; a step of forming a resist pattern by irradiation and development with light or electron beams; a step of etching the hard mask with a halogen-based gas through the resist pattern; a step of etching the resist underlayer film with an oxygen-based gas or a hydrogen-based gas through the patterned hard mask; and a step of processing the semiconductor substrate with a halogen-based gas through the patterned resist underlayer film.

[0184] The miniaturization of the resist pattern is carried out, and the thin film of the resist is desired. Therefore, it is necessary to make not only the resist pattern but also the resist underlayer film produced between the resist and the semiconductor substrate to be processed have the function of a mask during substrate processing. The process is a photolithography process that forms at least two layers of resist underlayer films and uses the resist underlayer films as a mask material. As materials for forming the above-mentioned at least two layers, organic resins (for example, acrylic resins, novolac resins, polyester resins, polyether resins, PEEK resins, maleimide resins, etc.), organic compounds (for example, amorphous carbon, etc.), silicone resins (for example, organopolysiloxanes, etc.), inorganic silicon compounds (for example, SiON, SiO 2 , SiN, etc.). When dry etching is performed using a pattern formed by the above-mentioned organic layer as a mask, it has excellent etching resistance to etching gases (such as fluorocarbons, oxygen, etc.). In addition, due to the diversification of semiconductor manufacturing processes, the resist underlayer film used in such a process not only shows the above-mentioned characteristics, but also shows small film thickness difference and good coverage characteristics (flattening characteristics) relative to various layouts in high-low difference substrates, embedding characteristics for fine patterns, and sufficient curing characteristics under a nitrogen atmosphere. In addition, such a resist underlayer film can also be given the ability to effectively absorb reflected light from the substrate when irradiation light of wavelengths such as 248nm, 193nm, and 157nm is used for micro-processing, and can have the function of a conventional anti-reflection film.

[0185] The composition for forming a resist underlayer film for lithography of the present invention takes into account the effect as an anti-reflective film. Since the light absorbing part is introduced into the skeleton, there is no diffusion into the photoresist during heating and drying. In addition, since the light absorbing part has a sufficiently large light absorbing performance, the reflected light prevention effect is high.

[0186] The resist underlayer film-forming composition for lithography of the present invention has high thermal stability, can prevent contamination of the upper layer film by decomposition products during firing, and can provide a temperature margin for the firing step.

[0187] Furthermore, the resist underlayer film composition for lithography of the present invention can be used as a film having the function of preventing reflection of light, and further preventing interaction between the substrate and the photoresist or preventing the adverse effects of materials used in the photoresist or substances generated during exposure of the photoresist on the substrate, depending on the process conditions.

[0188] The process of forming the resist underlayer film can also be performed by a nanoimprint method. The method includes: applying a curable composition to the formed resist underlayer film; bringing the curable composition into contact with a mold; irradiating the curable composition with light or electron beams to form a cured film; and separating the cured film from the mold.

[0189] Example

[0190] Hereinafter, the present invention will be described in more detail with reference to synthesis examples, examples and comparative examples, but the present invention is not limited to the following examples.

[0191] [Synthesis of polymer]

[0192] The synthesis of polymers of structural formulas (S1) to (S25) used as resist underlayer films and the synthesis of structural formulas (S'1) to (S'25) as comparative examples used the following compound group A, compound group B, compound group C, catalyst group D, solvent group E, and reprecipitation solvent group F.

[0193] (Compound Groups A to C)

[0194]

[0195] (Catalyst Group D)

[0196] Methanesulfonic acid: D1

[0197] 3-Mercaptopropionic acid: D2

[0198] Tetrabutylammonium iodide: D3

[0199] (Solvent Group E)

[0200] Propylene glycol monomethyl ether acetate (=PGMEA): E1 N-methylpyrrolidone: E2

[0201] Tetrahydrofuran: E3

[0202] Sodium hydroxide aqueous solution: E4

[0203] (Reprecipitation Solvent Group F)

[0204] Methanol: F1

[0205] Methanol / water: F2

[0206] (Separation solvent group G)

[0207] Butyl acetate / water: G1

[0208] Synthesis example 1

[0209] 50.0 g of phenylindole (A1), 46.7 g of 9-fluorenone (C1), 12.5 g of methanesulfonic acid (D1), and 109.1 g of PGMEA (E1) were added to a flask. Then, it was heated to reflux under nitrogen and reacted for about 16 hours. After the reaction stopped, it was reprecipitated with methanol (G1) and dried to obtain a resin (S'1). The weight average molecular weight Mw measured by GPC in terms of polystyrene was about 1,400. The obtained resin was dissolved in PGMEA, and ion exchange was performed for 4 hours using a cation exchange resin and an anion exchange resin to obtain the target compound solution.

[0210]

[0211] The weight average molecular weight of the polymer is a measurement result obtained by gel permeation chromatography (hereinafter, abbreviated as GPC). The measurement was performed using a GPC apparatus manufactured by Tosoh Corporation, and the measurement conditions and the like were as follows.

[0212] Device: HLC-8320GPC manufactured by Higashikata Co., Ltd.

[0213] GPC column: TSKgel Super-MultiporeHZ-N (2 columns)

[0214] Column temperature: 40°C

[0215] Flow rate: 0.35mL / min

[0216] Eluent: THF

[0217] Standard sample: polystyrene

[0218] Synthesis Examples 2 to 25

[0219] The polymer used for the resist underlayer film was synthesized by changing compound group A, compound group B, compound group C, catalyst group D, solvent group E, and reprecipitation solvent group F. Otherwise, the experimental operation was the same as that of Synthesis Example 1. Comparative example polymers (S'2) to (S'25) and their solutions were synthesized under the following conditions.

[0220] Table 1

[0221]

[0222]

[0223] Synthesis Example 26

[0224] In a flask, 10.0 g of the reprecipitated resin (S'1) obtained in Synthesis Example 1, 10.4 g of propargyl bromide (C15), 0.5 g of tetrabutylammonium iodide (D3), 27.9 g of tetrahydrofuran (E3), and 9.0 g of a 25% aqueous sodium hydroxide solution (E4) were added. Then, the mixture was heated to 55°C under nitrogen and reacted for about 24 hours. After the reaction was stopped, the liquid separation operation was repeated with butyl acetate and water (G1), the organic layer was concentrated, redissolved in PGMEA, reprecipitated with methanol (F1), and dried to obtain a resin (S1). The weight average molecular weight Mw measured by GPC in terms of polystyrene was about 1,600. The obtained resin was dissolved in PGMEA, and ion exchange was performed for 4 hours using a cation exchange resin and an anion exchange resin to obtain a target compound solution.

[0225]

[0226] Synthesis Examples 27 to 50

[0227] The polymers used for the resist underlayer film were synthesized by changing the polymers (S'1) to (S'25), the catalyst group D, the solvent group E, the reprecipitation solvent group F, and the separation solvent group G. Otherwise, the experimental operation was the same as that of Synthesis Example 26. The Example polymers (S2) to (S25) and their solutions were synthesized under the following conditions.

[0228] Table 2

[0229]

[0230]

[0231] [Preparation of Resist Underlayer Film]

[0232] Polymers (S1) to (S25), (S'1) to (S'25), a crosslinking agent (CR1), an acid generator (Ad1), a solvent (propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monomethyl ether (PGME), cyclohexanone (CYH)), and a surfactant, Megaphak R-40 (manufactured by DIC Corporation, R-40), were mixed in the proportions shown in the following table, and filtered using a 0.1 μm polytetrafluoroethylene microfilter to prepare an anti-etching agent underlayer film material (Examples M1-M25, Comparative Examples M1-M50).

[0233]

[0234] Table 3

[0235]

[0236]

[0237]

[0238] [Sublimation determination]

[0239] The resist underlayer film materials of Comparative Examples M1-M25 and Examples M1-M25 were fired at 400°C for 60 seconds, and the concentration was adjusted to about 100 nm, and then coated on a silicon wafer using a spin coater. The wafer was placed in a sublimation measuring device integrated with a hot plate adjusted at 300°C, baked for 60 seconds, and the sublimation was captured and quantified using a QCM sensor. For the measurement, the hot plate was heated to 300°C, and the pump flow rate was set to 0.24 m 3 / s, the first 60 seconds were left for aging, and then the film-coated wafer was quickly placed on the hot plate (mounted with the measured object) from the slide port, and the sublimates were captured from 60 seconds to 120 seconds (60 seconds). The QCM sensor used an electrode made of a material containing a compound of silicon and aluminum, a quartz resonator diameter (sensor diameter) of 14mm, an electrode diameter of 5mm on the surface of the quartz resonator, and a resonance frequency of 9MHz. The composition of the sublimates detected in Examples M1-M25 after the introduction of propargyl groups was smaller than the sublimates of Comparative Examples M1-M25 before the introduction of propargyl groups was judged as ○ (Table 4).

[0240] [Dissolution test of resist solvent]

[0241] The resist underlayer film materials of comparative examples M1-M50 and embodiments M1-M25 were coated on silicon wafers using ACT-8 manufactured by Tokyo Electron Co., Ltd., respectively, and fired at the specified temperature / specified time described in the table under the atmosphere and N2 to form a 100nm resist underlayer film. The formed resist underlayer film was immersed in PGME / PGMEA=7 / 3 as a general diluent for 60 seconds to confirm the resistance to solvents. The case where the reduction rate of the film thickness before and after the diluent immersion is less than 1% is judged as ○ (Table 4). In addition, samples that do not show solvent resistance under the firing conditions under the atmosphere and N2 are difficult to evaluate as resist underlayer films, so they are not evaluated in the following tests.

[0242] [Measurement of etching rate]

[0243] The etcher and etching gas used in the etching measurement are as follows.

[0244] RIE-200NL (manufactured by SAMU): CF 4 50sccm

[0245] The resist underlayer film materials of Comparative Examples M26-M50 and Examples M1-M25 were coated on silicon wafers using a spin coater. The resist underlayer films were fired on a hot plate at the specified temperature / prescribed time as shown in the table to form a 100 nm resist underlayer film. 4 For each polymer, compositions whose etching resistance after propargyl group introduction of Examples M1 to M25 was greater than that of Comparative Examples M26 to M50 cured by a crosslinking agent / acid catalyst before propargyl group introduction were judged as ○ (Table 4).

[0246] [Embedding test for uneven substrates]

[0247] As a coating test for uneven substrates, it was confirmed that SiO 2 In the substrate, whether the open area (OPEN) where no pattern is formed and the groove width 50nm are filled with the resist underlayer film. After the resist underlayer film forming composition of Comparative Examples M26-M29 and Examples M1-M25 is applied to the above-mentioned substrate, it is fired at 400°C for 60 seconds to form a resist underlayer film of about 100nm. The flatness of the substrate was observed using a scanning electron microscope (S-4800) manufactured by Hitachi High-Tech Nologis Co., Ltd., and the case where it was filled without gaps was considered to be good in embedding, and it was judged as ○ (Table 4).

[0248] Table 4

[0249]

[0250]

[0251] As described above, the propargyl group functions as a crosslinking group, thereby suppressing the sublimation product compared with the original polymer. In addition, the polymer into which the propargyl group is introduced not only exhibits sufficient solvent resistance in the atmosphere, regardless of the presence or absence of a crosslinking agent or an acid catalyst, but also exhibits good solvent resistance even in N 2 It is also considered to be an advantage that the polymer exhibits good solvent resistance even under high temperatures, so it is also considered to have sufficient curability as a resist underlayer film. In addition, by introducing the propargyl group, it exhibits sufficient etching resistance to F-based gases, which are general-purpose etching gases. In addition, the propargyl group in the polymer can increase the crosslinking start temperature, thereby obtaining sufficient reflowability and having good embedding properties in substrates with patterns. From these viewpoints, it can be expected to be widely used in semiconductor devices.

[0252] Industrial Availability

[0253] The resist underlayer film material used in the photolithography process using the multilayer film of the present invention can provide a resist underlayer film that exhibits excellent etching resistance, has good flattening and embedding properties in a micro-processed substrate, obtains an excellent resist pattern, and has resistance to solvents even in a nitrogen atmosphere, exhibits sufficient curing properties, and further can also have the effect of an anti-reflective film. In addition, it is determined that the underlayer film material of the present invention has heat resistance that allows a hard mask to be formed by vapor deposition on the upper layer.

Claims

1. A resist underlayer film-forming composition comprising a polymer having a unit structure represented by the following formula (I) or formula (I'), In formula (I) or formula (I'), ring A and ring B are aryl groups having 6 to 80 carbon atoms which may contain heteroatoms and may have a cyclic structure containing an alkyl chain; R 1 , R 2 and R 3 is a substituent of a hydrogen atom of the ring, and each is independently a halogen atom, a nitro group, a cyano group, an amino group, a hydroxyl group, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an alkynyl group having 2 to 10 carbon atoms, an aryl group having 6 to 80 carbon atoms, or a combination of these groups which may include an ether bond, a keto bond, a sulfide bond, a sulfonyl group, a carboxyl group or an ester bond; R 4 is an alkynyl group having 2 to 10 carbon atoms; n1, n2, and n3 are each an integer greater than or equal to 0 and less than or equal to the maximum number of substitutions that can be made on the ring; D represents a divalent organic group having a structure represented by the following formula (II) and / or formula (III); In formula (II), R and R' each independently represent a hydrogen atom, an aromatic hydrocarbon group having 6 to 30 carbon atoms which may have a substituent, a heterocyclic group having 3 to 30 carbon atoms which may have a substituent, or a linear, branched or cyclic alkyl group having 10 or less carbon atoms which may have a substituent; In formula (III), X and Y may be bonded to the same carbon on Z or to different carbons, and each independently represents an aromatic hydrocarbon group having 6 to 30 carbon atoms which may have a substituent, or a linear, branched or cyclic alkyl group having 10 or less carbon atoms which may have a heteroatom or a substituent; Z forms a 4 to 12-membered monocyclic, bicyclic or tricyclic aromatic ring which may be fused, may have a substituent, or may contain a heteroatom; i and j each independently represent 0 or 1; p, q and k represent the number of bonds; p and q each independently represent 0 or 1; p and q are not 0 at the same time; and k represents an integer from 0 to 2.

2. The resist underlayer film forming composition according to claim 1, wherein ring A and ring B are benzene rings or naphthalene rings, n1+n2+n3 is 0 to 2, and R 4 It is propargyl. 3 . The resist underlayer film-forming composition according to claim 2 , wherein D is a divalent organic group including a fluorene or fluorene derivative structure and / or an aromatic hydrocarbon group having 6 to 30 carbon atoms which may have a substituent. The resist underlayer film forming composition according to claim 1 , further comprising a surfactant. 5 . The resist underlayer film-forming composition according to claim 1 , further comprising a cross-linking agent. 6 . The resist underlayer film forming composition according to claim 1 , further comprising a surfactant and a crosslinking agent. 7 . The resist underlayer film-forming composition according to claim 1 , further comprising an acid and / or a salt thereof and / or an acid generator. 8 . The resist underlayer film-forming composition according to claim 1 , further comprising a surfactant, and an acid and / or a salt thereof and / or an acid generator. 9 . The resist underlayer film-forming composition according to claim 1 , further comprising a crosslinking agent, and an acid and / or a salt thereof and / or an acid generator. 10 . The resist underlayer film-forming composition according to claim 1 , further comprising a surfactant and a cross-linking agent, and an acid and / or a salt thereof and / or an acid generator. 11 . A resist underlayer film obtained by applying the resist underlayer film-forming composition according to claim 1 onto a semiconductor substrate and firing the coating.

12. A method for manufacturing a semiconductor device, comprising: a step of forming an underlayer film on a semiconductor substrate using the resist underlayer film forming composition described in any one of claims 1 to 10; a step of forming a resist film on the underlayer film; a step of forming a resist pattern by irradiating and developing with light or electron beams; a step of etching the underlayer film using the resist pattern; and a step of processing the semiconductor substrate using the patterned underlayer film. 13 . The method for manufacturing a semiconductor device according to claim 12 , wherein the resist film is patterned by a nanoimprint method or a self-assembled film.

14. A method for manufacturing a semiconductor device, comprising: a process of forming an underlayer film on a semiconductor substrate using the resist underlayer film forming composition described in any one of claims 1 to 10; a process of forming a hard mask on the underlayer film; a process of further forming a resist film on the hard mask; a process of forming a resist pattern by irradiating and developing with light or electron beams; a process of etching the hard mask using the resist pattern; a process of etching the underlayer film using the patterned hard mask; a process of removing the hard mask; and a process of processing the semiconductor substrate using the patterned underlayer film. 15 . The method for manufacturing a semiconductor device according to claim 14 , wherein the resist film is patterned by a nanoimprint method or a self-assembled film.

16. The method for manufacturing a semiconductor device according to claim 15 further comprises: a step of forming a vapor-deposited film, i.e., a spacer, on the lower film from which the hard mask has been removed; a step of processing the formed vapor-deposited film, i.e., the spacer, by etching; a step of removing the lower film; and a step of processing the semiconductor substrate through the spacer. 17 . The method for manufacturing a semiconductor device according to claim 16 , wherein the step of removing the hard mask is performed by etching or an alkaline chemical solution.