Mixture for secondary battery, mixture sheet for secondary battery, method for producing same, and secondary battery

By subjecting polytetrafluoroethylene resin to high shear treatment, a mixture for secondary batteries with a fibrous structure with a maximum fibril diameter of 90 nm or more was prepared, solving the problem of insufficient fibrillation and realizing the mechanical improvement of secondary batteries. Features and softness are improved, improving battery performance.

CN118786545APending Publication Date: 2024-10-15DAIKIN INDUSTRIES LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380024610.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-02
Filing Date
2023-03-02
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

When existing mixtures for secondary batteries use fibrillar resins as binders, fibrillation is insufficient, resulting in poor secondary battery performance and difficulty in achieving good mechanical properties and flexibility.

Method used

By subjecting polytetrafluoroethylene resin to high shear treatment, a fibrous structure with a maximum fibril diameter of more than 90 nm is produced, and combined with solid electrolyte and electrode active material, a mixture for secondary batteries with excellent mechanical properties and flexibility is prepared. .

Benefits of technology

It is possible to obtain a flexible composite sheet for secondary batteries with excellent mechanical properties without using a support, which reduces the deterioration of the solid electrolyte and improves the flexibility of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005019445320000291
    Figure BDA0005019445320000291
Patent Text Reader

Abstract

Provided are: a mixture for secondary batteries, which has good properties; a mixture sheet for secondary batteries, which contains the mixture; and a secondary battery which uses the sheet for secondary batteries. A secondary battery mixture containing a solid electrolyte and / or an electrode active material and a binder, the secondary battery mixture being characterized in that the binder is a fibrillar resin, and the fibrillar resin has a fibrous structure having a maximum fibrillar diameter of 90 nm or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a mixture for a secondary battery, a mixture sheet for a secondary battery, a method for producing the same, and a secondary battery. Background Art

[0002] In lithium-ion secondary batteries, a secondary battery sheet is generally produced by mixing a binder and a solvent with powder components such as an electrode active material and a conductive aid, applying the resulting slurry, and drying it.

[0003] On the other hand, polytetrafluoroethylene resin is a polymer that is easily fibrillated, and is also used as a binder by fibrillating it.

[0004] Patent Document 1 discloses a method for producing an electrode, in which a mixture containing an active material and a polytetrafluoroethylene mixed binder material is subjected to a high shearing treatment using a jet mill, thereby fibrillating polytetrafluoroethylene.

[0005] Patent Document 2 discloses forming an electrode by extrusion molding of a paste using a polytetrafluoroethylene resin.

[0006] Non-Patent Document 1 discloses that an anode is formed from a composition containing an anode active material, a solid electrolyte, polytetrafluoroethylene, and xylene.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application No. 2017-517862

[0010] Patent Document 2: International Publication No. 2021 / 043493

[0011] Non-patent literature

[0012] Non-patent document 1: NATURE ENERGY 5, 299-308 (2020) Summary of the invention

[0013] Problems to be solved by the invention

[0014] An object of the present disclosure is to provide a secondary battery mixture having good properties, a secondary battery mixture sheet containing the mixture, and a secondary battery using the secondary battery mixture sheet.

[0015] Another object of the present disclosure is to provide a method for producing a secondary battery sheet containing a polytetrafluoroethylene resin having a fine fiber structure.

[0016] Means for solving problems

[0017] The present disclosure relates to a secondary battery mixture, which is a secondary battery mixture containing a solid electrolyte and / or an electrode active material, and a binder, and is characterized in that:

[0018] The binder is a fibrillar resin.

[0019] The fibrillar resin has a fibrous structure with a maximum fibril diameter of 90 nm or more.

[0020] The present disclosure relates to a secondary battery mixture, which is a secondary battery mixture containing a solid electrolyte and / or an electrode active material, and a binder, and is characterized in that:

[0021] The binder is a fibrillar resin.

[0022] The fibrillar resin has a fibrous structure in which the third quartile of the fibril diameter is 35 nm or more.

[0023] The fibrillar resin is preferably characterized by having a fibrous structure in which the median value of the fibril diameter is 100 nm or less.

[0024] The secondary battery mixture is preferably used in lithium ion secondary batteries.

[0025] The secondary battery mixture is a secondary battery mixture obtained by using a raw material composition containing a solid electrolyte and / or an electrode active material and a binder, wherein:

[0026] The binder of the raw material composition is preferably a powdered polytetrafluoroethylene resin.

[0027] The water content of the powdery fibrillar resin is preferably 500 ppm or less.

[0028] The standard specific gravity of the powdery polytetrafluoroethylene resin is preferably 2.12 to 2.20.

[0029] The powdery polytetrafluoroethylene resin preferably contains 50% by mass or more of a polytetrafluoroethylene resin having a secondary particle size of 450 μm or more.

[0030] The powdery polytetrafluoroethylene resin preferably contains 80% by mass or more of a polytetrafluoroethylene resin having a secondary particle size of 450 μm or more.

[0031] The secondary battery mixture of the present disclosure preferably further contains a positive electrode active material.

[0032] The secondary battery mixture is preferably used in a solid-state secondary battery.

[0033] The present disclosure also relates to a secondary battery mixture sheet, which includes the secondary battery mixture.

[0034] The present disclosure also relates to an electrode, which comprises the above-mentioned mixture sheet for secondary battery.

[0035] The present disclosure also relates to a method for manufacturing a secondary battery composite sheet, the method for manufacturing a secondary battery composite sheet comprising:

[0036] Step (1): applying shear force while mixing a raw material composition containing a solid electrolyte and / or an electrode active material and a binder;

[0037] Step (2): forming the secondary battery mixture obtained in the above step (1) into a block shape; and

[0038] Step (3): rolling the block-shaped secondary battery mixture obtained in the above step (2) into a sheet shape,

[0039] The invention is characterized in that the binder is a powdery fibrillar resin having a fibrous structure with a maximum fibril diameter of 90 nm or more.

[0040] The present disclosure also relates to a secondary battery comprising the above-mentioned secondary battery mixture sheet.

[0041] Effects of the Invention

[0042] According to the present disclosure, a secondary battery mixture sheet having excellent performance can be obtained. DETAILED DESCRIPTION

[0043] The present disclosure is described in detail below.

[0044] The present disclosure provides a secondary battery mixture that can be suitably used in a secondary battery and a mixture sheet containing the secondary battery mixture.

[0045] In the secondary battery mixture disclosed in the present invention and the mixture sheet containing the secondary battery mixture, a fibrillar resin is used as a binder. In the existing secondary battery mixture, the following method is usually adopted: a resin dissolved in a solvent such as a copolymer of vinylidene fluoride and hexafluoropropylene is used as a binder, and the secondary battery mixture is prepared by coating and drying a slurry containing the binder.

[0046] It is known that if a shear stress is applied to a fibrillar resin such as polytetrafluoroethylene resin (hereinafter referred to as PTFE) in a particle state, fibrillation occurs easily. By utilizing this fibrillation property, the fibrillar resin can be used as a binder. That is, the fibrillar resin is entangled with other powder components, so that the powder components are bonded, thereby being able to function as a binder when the powder components are molded.

[0047] However, even when a fibrillated resin is used as a binder, if the fibrillation is insufficient, good performance cannot be exerted when used as a secondary battery mixture. In the present disclosure, this point is studied, characterized in that the fibrillation of a fibrous structure with a maximum fibril diameter of 90nm or more is produced. It should be noted that the maximum fibril diameter refers to the value that becomes the maximum value in the determination of the fibril diameter for the fibrillated resin. More specifically, it is a value measured by the method described in the embodiment.

[0048] By having such a maximum fibril diameter, a sheet that is soft and excellent in mechanical properties and can be handled even without using a support can be obtained, and from this point of view, a preferred effect can be obtained.

[0049] The maximum fibril diameter is more preferably 90 nm or more, further preferably 100 nm or more, and particularly preferably 110 nm or more. The upper limit of the maximum fibril diameter is not particularly limited, and can be, for example, 400 nm or less.

[0050] In the secondary battery mixture of the second embodiment of the present disclosure, the third quartile of the fibril diameter is 35 nm or more. The third quartile of the fibril diameter is a value that includes the lower 75% when the values ​​are arranged in order of size in the determination of the fibril diameter. The third quartile of the fibril diameter is a value measured by the measurement method described in the embodiment.

[0051] The third quartile of the fibril diameter is more preferably 35 nm or more, and further preferably 40 nm or more. The upper limit of the maximum fibril diameter is not particularly limited, and can be, for example, 65 nm or less.

[0052] The secondary battery mixture disclosed in the present invention preferably has a median value of the fibril diameter of 100 nm or less. Within such a range, the fibrillated PTFE can reduce the degradation of the solid electrolyte as a binder of the secondary battery mixture and can exhibit good performance.

[0053] Furthermore, in the secondary battery mixture of the present disclosure, the average inter-fibril distance may be 0.25 μm or more and 10 μm or less.

[0054] The average inter-fibril distance refers to the average value of the distances between fibrils existing in the xy plane, and the average inter-fibril distance is determined from an image of a scanning electron microscope (SEM). Satisfying these values ​​is preferred in terms of good flexibility.

[0055] In the secondary battery mixture disclosed in the present invention, the average node area can be 0.5 μm 2 Above, it can be 2.0μm 2 the following.

[0056] The area of ​​the node can be measured from the SEM photograph. However, in the case where it is necessary to determine these values ​​more strictly, image processing can be performed. For example, image analysis software (e.g., "NanoHunter NS2K-Pro" manufactured by Nanosystem Corporation) can also be used to calculate the node area separately.

[0057] It should be noted that the area of ​​the node is preferably determined by measuring a region corresponding to at least 150 μm×100 μm within the sample surface.

[0058] In the present disclosure, the fibrillar resin refers to a resin that is easily fibrillated when shear stress is applied. By using such a fibrillar resin as a binder, the fibrillar resin is entangled with other powder components, thereby bonding the powder components, so that it can act as a binder when the powder components are molded. For example, as a fibrillar resin, LCP, cellulose, acrylic resin, ultra-high molecular weight polyethylene, PTFE, etc. can be cited, wherein PTFE is preferred from the aspects of chemical stability, thermal stability, and processability. It should be noted that in the present disclosure, the powder component refers to other powder components constituting the secondary battery mixture, specifically, preferably a solid electrolyte and / or an electrode active material.

[0059] In the present disclosure, the PTFE resin is not particularly limited and may be a homopolymer or a fibrillable copolymer.

[0060] In the case of a copolymer, examples of the fluorine-containing monomer as a comonomer include chlorotrifluoroethylene, hexafluoropropylene, fluoroalkylethylene, perfluoroalkylethylene, fluoroalkyl / fluorovinyl ether and the like.

[0061] It should be noted that the above-mentioned "PTFE powder" refers to a solid state as a powder, rather than a dispersed state mixed with a liquid medium. By utilizing a substance in this state, using PTFE in a state without a liquid medium to manufacture a secondary battery mixture, the purpose of the present disclosure can be appropriately achieved.

[0062] The powdered PTFE as a raw material for producing the secondary battery mixture of the present disclosure preferably has a water content of 500 ppm or less.

[0063] By setting the water content to 500 ppm or less, it is preferable in terms of reducing the degradation of the solid electrolyte.

[0064] The water content is more preferably 300 ppm or less.

[0065] The standard specific gravity of the powdered PTFE is preferably 2.12 to 2.20. By making the standard specific gravity within this range, a secondary battery composite sheet with high strength can be produced, which has an advantage in this respect. The lower limit of the standard specific gravity is more preferably 2.13 or more. The upper limit of the standard specific gravity is more preferably 2.19 or less, and further preferably 2.18 or less.

[0066] Regarding the standard specific gravity [SSG], a sample was prepared in accordance with ASTM D-4895-89, and the specific gravity of the obtained sample was measured by the water displacement method.

[0067] The powdered PTFE as a raw material for manufacturing the secondary battery mixture disclosed herein preferably contains 50% by mass or more of polytetrafluoroethylene resin having a secondary particle size of 450 μm or more, and more preferably contains 80% by mass or more. By making the PTFE having a secondary particle size of 450 μm or more within this range, it has the advantage of being able to produce a high-strength mixture sheet.

[0068] By using PTFE having a secondary particle size of 450 μm or more, a composite sheet having lower electrical resistance and high toughness can be obtained.

[0069] The lower limit of the average secondary particle size of the powdered PTFE is more preferably 450 μm, and further preferably 500 μm. The upper limit of the secondary particle size is more preferably 700 μm or less, and further preferably 600 μm or less. The secondary particle size can be determined, for example, by sieving.

[0070] For the above-mentioned powdered PTFE as a raw material for manufacturing the secondary battery mixture disclosed in the present invention, the average primary particle size is preferably 150 nm or more, more preferably 180 nm or more, further preferably 210 nm or more, and particularly preferably 220 nm or more, because a secondary battery mixture sheet with higher strength and excellent homogeneity can be obtained.

[0071] The larger the average primary particle size of the powdered PTFE, the better the moldability. The upper limit is not particularly limited and may be 500 nm. From the perspective of productivity in the polymerization process, 350 nm is preferred.

[0072] Regarding the above-mentioned average primary particle size, a calibration curve of the average primary particle size determined by measuring the transmittance of 550nm projected light per unit length of an aqueous dispersion of PTFE obtained by polymerization and the oriented diameter in a transmission electron microscope photograph is prepared using an aqueous dispersion of PTFE obtained by polymerization. The transmittance is measured for the aqueous dispersion as the measurement object, and can be determined based on the above-mentioned calibration curve.

[0073] The above-mentioned powdered PTFE as the raw material for making the disclosed secondary battery mixture can have a core-shell structure. As the PTFE with a core-shell structure, for example, the core of the polytetrafluoroethylene containing high molecular weight and the polytetrafluoroethylene of a lower molecular weight or the polytetrafluoroethylene of the shell of modified polytetrafluoroethylene can be enumerated in the particle. As such modified polytetrafluoroethylene, the polytetrafluoroethylene etc. recorded in the Japanese Patent Table 2005-527652 communique can be enumerated.

[0074] The powdered PTFE satisfying the above parameters can be obtained by a conventional production method, for example, by the production method described in International Publication No. 2015-080291, International Publication No. 2012-086710, etc.

[0075] In the present disclosure, in the secondary battery mixture, the lower limit of the content of the binder is preferably 0.2% by mass or more, more preferably 0.3% by mass or more. It is further preferably more than 0.5% by mass. The upper limit of the content of the binder is preferably 10% by mass or less, more preferably 7% by mass or less, particularly preferably 6% by mass or less, further preferably 4% by mass or less, further preferably 1.7% by mass or less, and most preferably 1.0% by mass or less in the secondary battery mixture. If the binder is within the above range, it is possible to form a sheet with self-supporting properties that suppresses the rise in electrode resistance and has excellent operability.

[0076] The secondary battery mixture disclosed in the present invention can be used for electrodes for solid-state batteries, and can also be used for electrodes for batteries containing electrolytes. Furthermore, it can also be used for solid electrolyte layers in solid-state batteries. According to these uses, the components constituting the mixture are combined to produce fibrillation that meets the above parameters, thereby achieving the purpose of the present disclosure.

[0077] In the case where the electrode is an electrode for a solid-state battery, the secondary battery mixture also contains an electrode active material and a solid electrolyte, and in the case of an electrode for a battery containing an electrolyte, it contains an electrode active material. It may also contain an electrode auxiliary agent and other components as needed. Below, each component used to constitute the electrode is described in detail.

[0078] (Electrode Active Material)

[0079] When the secondary battery composite sheet disclosed in the present invention is used as a positive electrode sheet, a positive electrode active material is mixed in the secondary battery composite sheet. The positive electrode active material can be a positive electrode active material known as a positive electrode active material for a solid-state battery. It is particularly preferred to use a positive electrode active material that can contain / release lithium ions.

[0080] As the above-mentioned positive electrode active material, there is no particular restriction as long as it can electrochemically encapsulate / release alkali metal ions, for example, preferably a material containing an alkali metal and at least one transition metal. As specific examples, transition metal composite oxides containing alkali metals, transition metal phosphate compounds containing alkali metals, conductive polymers, etc. can be cited.

[0081] Among them, as the positive electrode active material, a transition metal composite oxide containing an alkali metal that can generate a high voltage is particularly preferred. As the above-mentioned alkali metal ion, lithium ion, sodium ion, potassium ion, etc. can be cited. In a preferred embodiment, the alkali metal ion can be a lithium ion. That is, in this embodiment, the alkali metal ion secondary battery is a lithium ion secondary battery.

[0082] Examples of the alkali metal-containing transition metal composite oxide include

[0083] Formula: M a Mn 2-b M 1 b O4

[0084] (wherein, M is at least one metal selected from the group consisting of Li, Na and K; 0.9≤a; 0≤b≤1.5; M 1 an alkali metal-manganese spinel composite oxide represented by at least one metal selected from the group consisting of Fe, Co, Ni, Cu, Zn, Al, Sn, Cr, V, Ti, Mg, Ca, Sr, B, Ga, In, Si and Ge,

[0085] Formula: MNi 1-c M 2 cO2

[0086] (wherein, M is at least one metal selected from the group consisting of Li, Na and K; 0≤c≤0.5; M 2 an alkali metal-nickel composite oxide represented by at least one metal selected from the group consisting of Fe, Co, Mn, Cu, Zn, Al, Sn, Cr, V, Ti, Mg, Ca, Sr, B, Ga, In, Si and Ge, or

[0087] Formula: MCo 1-d M 3 d O2

[0088] (wherein, M is at least one metal selected from the group consisting of Li, Na and K; 0≤d≤0.5; M 3The alkali metal-cobalt composite oxide is represented by at least one metal selected from the group consisting of Fe, Ni, Mn, Cu, Zn, Al, Sn, Cr, V, Ti, Mg, Ca, Sr, B, Ga, In, Si and Ge.

[0089] Among the above, M is preferably one metal selected from the group consisting of Li, Na and K, more preferably Li or Na, and further preferably Li.

[0090] Among them, MCoO2, MMnO2, MNiO2, MMn2O4, MNi 0.8 Co 0.15 Al 0.05 O2, or MNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, etc., preferably a compound represented by the following general formula (3).

[0091] MNi h Co i Mn j M 5 k O2(3)

[0092] (wherein, M is at least one metal selected from the group consisting of Li, Na and K, M 5 represents at least one selected from the group consisting of Fe, Cu, Zn, Al, Sn, Cr, V, Ti, Mg, Ca, Sr, B, Ga, In, Si and Ge, (h+i+j+k)=1.0, 0≤h≤1.0, 0≤i≤1.0, 0≤j≤1.5, 0≤k≤0.2.)

[0093] Examples of the alkali metal-containing transition metal phosphate compound include the following formula (4):

[0094] M e M 4 f (PO4) g (4)

[0095] (wherein, M is at least one metal selected from the group consisting of Li, Na and K, M 4 represents at least one selected from the group consisting of V, Ti, Cr, Mn, Fe, Co, Ni and Cu, 0.5≤e≤3, 1≤f≤2, 1≤g≤3). In the above, M is preferably a metal selected from the group consisting of Li, Na and K, more preferably Li or Na, and further preferably Li.

[0096] As the transition metal of the lithium-containing transition metal phosphate compound, V, Ti, Cr, Mn, Fe, Co, Ni, Cu and the like are preferred. Specific examples include iron phosphates such as LiFePO4, Li3Fe2(PO4)3, LiFeP2O7; cobalt phosphates such as LiCoPO4; substances obtained by replacing a part of the transition metal atoms serving as the main body of these lithium transition metal phosphate compounds with other metals such as Al, Ti, V, Cr, Mn, Fe, Co, Li, Ni, Cu, Zn, Mg, Ga, Zr, Nb, Si, etc.; and the like.

[0097] The lithium-containing transition metal phosphate compound preferably has an olivine structure.

[0098] As other positive electrode active materials, MFePO4, MNi 0.8 Co 0.2 O2, M 1.2 Fe 0.4 Mn 0.4 O2、MNi 0.5 Mn 1.5 O2, MV3O6, M2MnO3 (wherein M is at least one metal selected from the group consisting of Li, Na and K), etc. In particular, M2MnO3, MNi 0.5 Mn 1.5 When the positive electrode active material such as O2 operates the secondary battery at a voltage exceeding 4.4V or a voltage above 4.6V, the crystal structure will not collapse, which is preferred from this aspect. Therefore, even if the electrochemical device such as the secondary battery using the positive electrode material containing the positive electrode active material exemplified above is stored at high temperature, the residual capacity is not easy to decrease, the resistance increase rate is not easy to change, and even if it works at a high voltage, the battery performance will not deteriorate, so it is preferred.

[0099] Other positive electrode active materials include M2MnO3 and MM 6 O2 (wherein, M is at least one metal selected from the group consisting of Li, Na and K, M 6 Solid solution materials of transition metals such as Co, Ni, Mn, Fe, etc.

[0100] As the above-mentioned solid solution material, for example, a general formula M x [Mn (1-y) M 7 y ]O z Here, M in the formula is at least one metal selected from the group consisting of Li, Na and K, and M 7It is composed of at least one metal element other than M and Mn, for example, it contains one or more elements selected from the group consisting of Co, Ni, Fe, Ti, Mo, W, Cr, Zr, and Sn. In addition, the values of x, y, and z in the formula are in the range of 1 < x < 2, 0 ≤ y < 1, and 1.5 < z < 3. Among them, Li 1.2 Mn 0.5 Co 0.14 Ni 0.14 A manganese-containing solid solution material such as Li2MnO3-based and solid-solved with LiNiO2 and LiCoO2 like Li 1.2 Mn 0.5 Co 0.14 Ni 0.14 O2 can provide an alkali metal ion secondary battery with high energy density and is preferred in this regard.

[0101] In addition, if the positive electrode active material contains lithium phosphate, the continuous charging characteristics are improved, so it is preferred. The use of lithium phosphate is not limited, and it is preferably used by mixing with the above positive electrode active material. The amount of lithium phosphate used is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, and further preferably 0.5% by mass or more with respect to the total lower limit of the above positive electrode active material and lithium phosphate, and the upper limit is preferably 10% by mass or less, more preferably 8% by mass or less, and further preferably 5% by mass or less.

[0102] Examples of the above conductive polymer include p-doped conductive polymers and n-doped conductive polymers. Examples of conductive polymers include polyacetylene-based, polyphenylene-based, heterocyclic polymers, ionic polymers, ladder and network polymers, etc.

[0103] In addition, a substance having a different composition from the above positive electrode active material may be attached to the surface of the positive electrode active material, and the positive electrode active material thus obtained is used. Examples of the surface-attached substance include oxides such as alumina, silica, titanium oxide, zirconium oxide, magnesium oxide, calcium oxide, boron oxide, antimony oxide, and bismuth oxide; sulfates such as lithium sulfate, sodium sulfate, potassium sulfate, magnesium sulfate, calcium sulfate, and aluminum sulfate; carbonates such as lithium carbonate, calcium carbonate, and magnesium carbonate; carbon; and the like.

[0104] These surface-attached substances can be attached to the surface of the positive electrode active material, for example, by the following methods: a method of dissolving or suspending in a solvent, infiltrating or adding to the positive electrode active material and then drying; a method of dissolving or suspending the surface-attached substance precursor in a solvent, infiltrating and adding to the positive electrode active material, and then reacting it by heating or the like; a method of adding to the positive electrode active material precursor and firing simultaneously; and the like. It should be noted that in the case of attaching carbon, a method of mechanically attaching carbonaceous materials such as activated carbon can also be used.

[0105] The amount of the surface-attached substance is preferably 0.1 ppm or more, more preferably 1 ppm or more, and further preferably 10 ppm or more, as the lower limit, and preferably 20% or less, more preferably 10% or less, and further preferably 5% or less, relative to the above-mentioned positive electrode active material, as the upper limit. The surface-attached substance can inhibit the oxidation reaction of the solid electrolyte on the surface of the positive electrode active material, and can improve the battery life. If the amount of attachment is too small, the effect cannot be fully demonstrated; if the amount of attachment is too large, it will hinder the entry and exit of lithium ions, so the resistance may increase.

[0106] The shape of the particles of the positive electrode active material may be a block shape, a polyhedron shape, a sphere shape, an ellipsoidal sphere shape, a plate shape, a needle shape, a column shape, etc. The primary particles may be aggregated to form secondary particles.

[0107] The tap density of the positive electrode active material is preferably 0.5 g / cm 3 More preferably, 0.8 g / cm 3 More preferably, 1.0 g / cm 3 Above. If the tap density of the positive electrode active material is less than the above lower limit, the amount of dispersion medium required when the positive electrode active material layer is formed increases, and the required amount of conductive material or binder increases. Sometimes the filling rate of the positive electrode active material in the positive electrode active material layer will be limited, and the battery capacity will be limited. By using a composite oxide powder with a high tap density, a high-density positive electrode active material layer can be formed. The larger the tap density is, the better, and there is no particular upper limit. However, if it is too large, the diffusion of lithium ions in the positive electrode active material layer with the solid electrolyte as the medium becomes rate-limiting, and sometimes the load characteristics are easily reduced. Therefore, the upper limit is preferably 4.0g / cm 3 Below, more preferably 3.7 g / cm 3 Below, more preferably 3.5 g / cm 3 the following.

[0108] It should be noted that in the present disclosure, the tap density is the powder packing density (tap density) g / cm2 when 5 g to 10 g of the positive electrode active material powder is placed in a 10 ml glass measuring cylinder and vibrated 200 times with a stroke of about 20 mm. 3 Find out.

[0109] The median diameter d50 of the particles of the positive electrode active material (secondary particle diameter when the primary particles agglomerate to form secondary particles) is preferably 0.3 μm or more, more preferably 0.5 μm or more, further preferably 0.8 μm or more, and most preferably 1.0 μm or more, and preferably 30 μm or less, more preferably 27 μm or less, further preferably 25 μm or less, and most preferably 22 μm or less. If it is less than the above lower limit, a high tap density product may not be obtained; if it exceeds the upper limit, the diffusion of lithium in the particles takes time, which may cause a decrease in battery performance, or when the positive electrode of the battery is made, that is, the active material and the conductive material, the binder, etc. are made into a slurry using a solvent and applied in a thin film, stripes and other problems may sometimes occur. Here, by mixing two or more of the above-mentioned positive electrode active materials with different median diameters d50, the filling property during the production of the positive electrode can be further improved.

[0110] It should be noted that in the present disclosure, the median diameter d50 is measured using a known laser diffraction / scattering particle size distribution measuring device. When using LA-920 manufactured by HORIBA as a particle size distribution meter, as a dispersion medium used during measurement, a 0.1% by mass sodium hexametaphosphate aqueous solution is used, and after 5 minutes of ultrasonic dispersion, the measured refractive index is set to 1.24 for measurement.

[0111] In the case where the primary particles are agglomerated to form secondary particles, the average primary particle size of the positive electrode active material is preferably 0.05 μm or more, more preferably 0.1 μm or more, and further preferably 0.2 μm or more, and the upper limit is preferably 5 μm or less, more preferably 4 μm or less, further preferably 3 μm or less, and most preferably 2 μm or less. If the upper limit is exceeded, it is difficult to form spherical secondary particles, which has an adverse effect on the powder filling property, or the specific surface area is greatly reduced, so the possibility of reduced battery performance such as output characteristics is sometimes increased. On the contrary, if it is less than the lower limit, problems such as poor reversibility of charge and discharge are usually caused due to poor crystallization.

[0112] It should be noted that in the present disclosure, the average primary particle size of the above-mentioned positive electrode active material is measured by observation using a scanning electron microscope (SEM). Specifically, in a photo with a magnification of 10,000 times, the longest value of the slice generated by the left and right boundary lines of the primary particles relative to the straight line in the horizontal direction is obtained for any 50 primary particles, and the average value is taken to obtain the average primary particle size.

[0113] The BET specific surface area of ​​the positive electrode active material is preferably 0.1 m 2 / g or more, more preferably 0.2m 2 / g or more, more preferably 0.3m 2 / g or more, and the upper limit is preferably 50m2 / g or less, more preferably 40m 2 / g or less, more preferably 30m 2 If the BET specific surface area is smaller than this range, the battery performance is likely to be reduced; if the BET specific surface area is larger than this range, it is difficult to increase the tap density, and the coating property when the positive electrode active material layer is formed may be problematic.

[0114] It should be noted that in the present disclosure, the BET specific surface area is defined as follows: using a surface area meter (for example, a fully automatic surface area measuring device manufactured by Okura Riken Co., Ltd.), the sample is pre-dried at 150°C for 30 minutes under nitrogen flow, and then a nitrogen-helium mixed gas accurately adjusted to a relative pressure value of 0.3 relative to atmospheric pressure is used to measure the sample by the nitrogen adsorption BET single-point method based on the gas flow method, and the obtained value is used to define the BET specific surface area.

[0115] When the secondary battery of the present disclosure is used as a large lithium ion secondary battery for hybrid vehicles or distributed power sources, high output is required, so the particles of the positive electrode active material preferably mainly contain secondary particles.

[0116] The particles of the positive electrode active material preferably have an average particle size of secondary particles of 40 μm or less, and contain 0.5% to 7.0% by volume of microparticles having an average primary particle size of 1 μm or less. By containing microparticles having an average primary particle size of 1 μm or less, the contact area with the electrolyte becomes larger, which can further accelerate the diffusion of lithium ions between the secondary battery sheet and the electrolyte, and as a result, the output performance of the battery can be improved.

[0117] As a method for manufacturing positive electrode active materials, a common method for manufacturing inorganic compounds is used. In particular, various methods are considered for making spherical or ellipsoidal active materials, for example, the following methods can be cited: dissolving or crushing the raw material of the transition metal and dispersing it in a solvent such as water, adjusting the pH under stirring, making a spherical precursor and recovering it, drying it as needed, then adding LiOH, Li2CO3, LiNO3 and other Li sources and firing at high temperature to obtain the active material.

[0118] In order to manufacture the positive electrode, the above-mentioned positive electrode active materials can be used alone, or two or more of different compositions can be used together in any combination or ratio. As a preferred combination in this case, LiCoO2 and LiNi 0.33 Co 0.33 Mn 0.33A combination of ternary systems such as O2, a combination of LiCoO2 and LiMn2O4 or a material in which a portion of Mn is replaced by other transition metals, or a combination of LiFePO4 and LiCoO2 or a material in which a portion of Co is replaced by other transition metals.

[0119] From the viewpoint of high battery capacity, the content of the positive electrode active material in the positive electrode mixture is preferably 50 to 99.5 mass %, more preferably 60 to 99 mass %, and even more preferably 69 to 96.7 mass %.

[0120] In addition, the content of the positive electrode active material is preferably 80% by mass or more, more preferably 82% by mass or more, and particularly preferably 84% by mass or more. In addition, the upper limit is preferably 99% by mass or less, more preferably 98% by mass or less. If the content of the positive electrode active material in the positive electrode mixture is low, the capacitance is sometimes insufficient. On the contrary, if the content is too high, the electron / ion conduction and strength of the positive electrode are sometimes insufficient.

[0121] In the case where the secondary battery composite sheet of the present invention is used as a negative electrode sheet, a negative electrode active material is mixed in the secondary battery composite sheet. The above-mentioned negative electrode active material is not particularly limited, and examples thereof include materials selected from lithium metal, artificial graphite, graphite carbon fiber, resin-fired carbon, thermal decomposition vapor-grown carbon, coke, mesocarbon microbeads (MCMB), furfuryl alcohol resin-fired carbon, polyacene, pitch-based carbon fiber, vapor-grown carbon fiber, natural graphite and non-graphitizable carbon, silicon-containing compounds such as silicon and silicon alloys, Li4Ti5O 12 Among them, a substance containing at least a part of a carbonaceous material or a silicon-containing compound can be particularly preferably used.

[0122] From the viewpoint of high battery capacity, the content of the negative electrode active material in the negative electrode mixture is preferably 50 to 99.5% by mass, more preferably 60 to 99% by mass, and even more preferably 69 to 96.7% by mass.

[0123] In addition, the content of the negative electrode active material is preferably 80% by mass or more, more preferably 82% by mass or more, and particularly preferably 84% by mass or more. In addition, the upper limit is preferably 99% by mass or less, more preferably 98% by mass or less. If the content of the negative electrode active material in the negative electrode mixture is low, the capacitance sometimes becomes insufficient. On the contrary, if the content is too high, the electron / ion conduction and strength of the negative electrode are sometimes insufficient.

[0124] (Solid Electrolyte)

[0125] As the solid electrolyte, either a sulfide-based solid electrolyte or an oxide-based solid electrolyte can be used.

[0126] (Sulfide-based solid electrolyte)

[0127] Examples of the sulfide-based solid electrolyte include lithium ion conductive inorganic solid electrolytes having a composition represented by the following formula (1).

[0128] Li a1 M b1 P c1 S d1 A e1 (1)

[0129] In the formula, M represents an element selected from B, Zn, Sn, Si, Cu, Ga, Sb, Al, Ti and Ge. A represents an element selected from I, Br, Cl and F. a1 to e1 represent the composition ratio of each element, and a1:b1:c1:d1:e1 satisfies 1 to 12:0 to 5:1:2 to 12:0 to 10. a1 is preferably 1 to 9, more preferably 1.5 to 7.5. b1 is preferably 0 to 3, more preferably 0 to 1. d1 is preferably 2.5 to 10, more preferably 3.0 to 8.5. e1 is preferably 0 to 5, more preferably 0 to 3.

[0130] In the present disclosure, the sulfide-based solid electrolyte preferably contains lithium. The sulfide-based solid electrolyte containing lithium is used for solid-state batteries using lithium ions as carriers, and is particularly preferred from the perspective of electrochemical devices having high energy density.

[0131] As described below, the composition ratio of each element can be controlled by adjusting the blending amount of the raw material compound when producing the sulfide-based inorganic solid electrolyte.

[0132] The sulfide-based inorganic solid electrolyte may be amorphous (glass), crystallized (glass ceramic), or only partially crystallized. For example, Li-PS-based glass containing Li, P, and S, or Li-PS-based glass ceramic containing Li, P, and S may be used.

[0133] Sulfide-based inorganic solid electrolytes can be manufactured, for example, by reacting at least two or more raw materials including lithium sulfide (Li2S), phosphorus sulfide (e.g., phosphorus pentasulfide (P2S5)), elemental phosphorus, elemental sulfur, sodium sulfide, hydrogen sulfide, lithium halide (e.g., LiI, LiBr, LiCl) and sulfides of the elements represented by M above (e.g., SiS2, SnS, GeS2).

[0134] As specific examples of sulfide-based inorganic solid electrolytes, examples of raw material combinations are shown below. Examples include Li2S-P2S5-LiCl, Li2S-P2S5-H2S, Li2S-P2S5-H2S-LiCl, Li2S-LiI-P2S5, Li2S-LiI-Li2O-P2S5, Li2S-LiBr-P2S5, Li2S-Li2O-P2S5, Li2S-Li3PO4-P2S5, Li2S-P2S5-P2O5, Li2S-P2S5-SiS2, Li2S-P2S5-SiS2-LiCl, Li2S-P2S5-SnS, Li2S-P2S5-Al2S3, Li2S- S-GeS2, Li2S-GeS2-ZnS, Li2S-Ga2S3, Li2S-GeS2-Ga2S3, Li2S-GeS2-P2S5, Li2S-GeS2-Sb2S5, Li2S-GeS2-Al2S3, Li2S-SiS2, Li2 S-Al2S3, Li2S-SiS2-Al2S3, Li2S-SiS2-P2S5, Li2S-SiS2-P2S5-LiI, Li2S-SiS2-LiI, Li2S-SiS2-Li4SiO4, Li2S-SiS2-Li3PO4, Li 10 GeP2S 12 Etc. However, there is no limitation on the mixing ratio of each raw material.

[0135] In particular, the sulfide-based solid electrolyte is preferably a sulfide-based solid electrolyte satisfying a composition represented by the following formula (A).

[0136] aLi2S-bX 1 S2-cLiX 2 -(1-abc)P2S5(A)

[0137] (where 0.6≤a≤0.86, 0≤b≤0.333, 0≤c≤0.3, 0.05≤b+c≤0.4, X 1 represents Ge, Sn, Ti or Si, X 2 represents Cl, Br or I. wherein either b or c is not 0. )

[0138] As an example of the sulfide-based solid electrolyte represented by the above formula (A), specifically, a sulfide-based solid electrolyte selected from 0.714Li2S-0.143SnS2-0.143P2S5 (Li 10 SnP2S 12(LSPS)), 0.625Li2S-0.25LiCl-0.125P2S5(Li6PS5Cl(LPSCl)), 0.715Li2S-0.143GeS2-0.142P2S5(Li 10 GeP2S 12 (LGPS)) etc. or a mixture of two or more thereof.

[0139] The average particle size of the sulfide-based solid electrolyte is preferably 0.1 μm or more and 20 μm or less. As a lower limit, it is more preferably 0.2 μm or more, and further preferably 0.3 μm or more. As an upper limit, it is more preferably 18 μm or less, and further preferably 15 μm or less.

[0140] If the average particle size of the sulfide-based solid electrolyte is less than 0.1 μm, handling of the powder may become difficult. On the other hand, if the average particle size of the sulfide-based solid electrolyte exceeds 20 μm, press moldability may deteriorate.

[0141] It should be noted that the average particle size of the sulfide-based solid electrolyte particles was measured according to the following procedure.

[0142] In a 20 ml sample bottle, the sulfide-based solid electrolyte particles are diluted with water (heptane is used in the case of substances that are unstable to water) to adjust to a 1% dispersion by mass. The diluted dispersed sample is irradiated with 1 kHz ultrasound for 10 minutes and then used in the test immediately. Using the dispersion sample, a laser diffraction / scattering particle size distribution analyzer LA-920 (manufactured by HORIBA) is used to acquire data 50 times at a temperature of 25°C using a measuring quartz dish to obtain the volume average particle size. For other detailed conditions, refer to the description of JIS Z8828: 2013 "Particle Size Analysis-Dynamic Light Scattering Method" as needed. Prepare 5 samples for each level and use the average value.

[0143] The method for adjusting the average particle size of the sulfide solid electrolyte is not particularly limited, and is performed, for example, as follows. A known pulverizer or classifier is used. For example, a mortar, a sand mill, a ball mill, a jet mill or a sieve is preferably used. Depending on the properties of the solid electrolyte, a solvent such as water or ethanol may be added during pulverization. In order to form a desired particle size, classification is preferably performed. Classification is not particularly limited, and may be performed using a sieve, a wind classifier, or the like.

[0144] Regarding the content of the sulfide-based solid electrolyte in the solid component of the secondary battery mixture, when considering the reduction of the interface resistance when used in the secondary battery and the maintenance of the reduced interface resistance, in the electrode, out of 100% by mass of the solid component, it is preferably 3% by mass or more, more preferably 4% by mass or more, and particularly preferably 5% by mass or more. As the upper limit, from the same aspect, it is preferably 99% by mass or less, more preferably 90% by mass or less, and particularly preferably 80% by mass or less.

[0145] In addition, in the solid electrolyte layer disposed between the positive electrode and the negative electrode, preferably 50 mass % or more, more preferably 60 mass % or more, particularly preferably 70 mass % or more. As the upper limit, from the same aspect, preferably 99.9 mass % or less, more preferably 99.8 mass % or less, particularly preferably 99.7 mass % or less.

[0146] The above-mentioned sulfide-based solid electrolyte can be used alone or in combination of two or more. It should be noted that in this specification, the solid component (solid content) refers to the component that does not volatilize or evaporate and disappear when dried at 170°C for 6 hours in a nitrogen atmosphere. Typically, it refers to the component other than the dispersion medium described later.

[0147] (Oxide-based solid electrolyte)

[0148] The oxide-based solid electrolyte is preferably a compound containing oxygen atoms (O), having ion conductivity of a metal belonging to Group 1 or Group 2 of the periodic table, and having electron insulating properties.

[0149] As specific examples of compounds, for example, Li xa La ya TiO3[xa=0.3~0.7, ya=0.3~0.7](LLT), Li xb La yb Zr zb M bb mb O nb (M bb is at least one element selected from the group consisting of Al, Mg, Ca, Sr, V, Nb, Ta, Ti, Ge, In, and Sn, xb satisfies 5≤xb≤10, yb satisfies 1≤yb≤4, zb satisfies 1≤zb≤4, mb satisfies 0≤mb≤2, and nb satisfies 5≤nb≤20. ), Li xc B yc M cc zc O nc (M ccis at least one element selected from C, S, Al, Si, Ga, Ge, In, and Sn, xc satisfies 0≤xc≤5, yc satisfies 0≤yc≤1, zc satisfies 0≤zc≤1, and nc satisfies 0≤nc≤6. ), Li xd (Al,Ga) yd (Ti,Ge) zd Si ad P md O nd (where 1≤xd≤3, 0≤yd≤2, 0≤zd≤2, 0≤ad≤2, 1≤md≤7, 3≤nd≤15), Li (3-2xe) M ee xe D ee O(xe represents a number greater than 0 and less than 0.1, M ee Represents a divalent metal atom. ee represents a halogen atom or a combination of two or more halogen atoms. ), Li xf Si yf O zf (1≤xf≤5,0 <yf≤3,1≤zf≤10)、Li xg S yg O zg (1≤xg≤3,0 <yg≤2,1≤zg≤10)、Li3BO3-Li2SO4、Li2O-B2O3-P2O5、Li2O-SiO2、Li6BaLa2Ta2O 12 、Li3PO (4-3 / 2w) N w (w satisfies w<1) and has a LISICON (Lithium super ionic conductor) type crystal structure 3.5 Zn 0.25 GeO4, La with perovskite crystal structure 0.51 Li 0.34 TiO 2.94 ,La 0.55 Li 0.35 TiO3, LiTi2P3O with NASICON (Natrium super ionic conductor) crystal structure 12 , Li 1+xh+yh (Al,Ga) xh (Ti,Ge) 2-xh Si yh P 3-yh O 12 (where 0≤xh≤1, 0≤yh≤1), Li7La3Zr2O with garnet crystal structure12 (LLZ), etc. In addition, ceramic materials in which LLZ has been elementally substituted are also known. For example, LLZ can also be exemplified as an LLZ-based ceramic material in which at least one element of Mg (magnesium) and A (A is at least one element selected from the group consisting of Ca (calcium), Sr (strontium), and Ba (barium)) has been substituted.

[0150] In addition, phosphorus compounds containing Li, P and O are also preferred. Examples thereof include lithium phosphate (Li3PO4), LiPON in which a portion of oxygen in lithium phosphate is replaced with nitrogen, and LiPOD 1 (D 1 is at least one selected from Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zr, Nb, Mo, Ru, Ag, Ta, W, Pt, Au, etc. In addition, LiA 1 ON(A 1 is at least one selected from Si, B, Ge, Al, C, Ga, etc.) and the like.

[0151] Specific examples include Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2, Li2O-Al2O3-SiO2-P2O5-TiO2, etc.

[0152] The oxide-based solid electrolyte preferably contains lithium. The oxide-based solid electrolyte containing lithium is used in solid-state batteries using lithium ions as carriers, and is particularly preferred from the perspective of electrochemical devices having high energy density.

[0153] The oxide-based solid electrolyte is preferably an oxide having a crystalline structure. In terms of good Li ion conductivity, an oxide having a crystalline structure is particularly preferred.

[0154] Examples of oxides having a crystal structure include perovskite-type (La 0.51 Li 0.34 TiO 2.94 etc.), NASICON type (Li 1.3 Al 0.3 Ti 1.7 (PO4)3, etc.), garnet type (Li7La3Zr2O 12 (LLZ) etc. Among them, NASICON type is preferred.

[0155] The volume average particle size of the oxide-based solid electrolyte is not particularly limited, but is preferably 0.01 μm or more, and more preferably 0.03 μm or more. As an upper limit, it is preferably 100 μm or less, and more preferably 50 μm or less. It should be noted that the average particle size of the oxide-based solid electrolyte particles is measured in the following order. The oxide-based solid electrolyte particles are diluted with water (heptane in the case of substances unstable to water) in a 20 ml sample bottle to adjust to a 1% dispersion by mass. The diluted dispersed sample is irradiated with 1 kHz ultrasound for 10 minutes and then used in the test immediately. Using the dispersion sample, a laser diffraction / scattering particle size distribution measuring device LA-920 (manufactured by HORIBA) is used to obtain data 50 times at a temperature of 25°C using a measuring quartz dish to obtain the volume average particle size. Other detailed conditions, etc., are described in JIS Z8828:2013 "Particle Size Analysis-Dynamic Light Scattering Method" as needed. Five samples are prepared for each level, and their average value is adopted.

[0156] (Conductive additive)

[0157] As the above-mentioned conductive auxiliary agent, any known conductive material can be used. As specific examples, metal materials such as copper and nickel, graphite (graphite) such as natural graphite and artificial graphite, carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, needle coke, carbon nanotubes, fullerene, carbon materials such as amorphous carbon such as VGCF, etc. can be cited. It should be noted that they can be used alone or in any combination and ratio. Two or more kinds can be used together.

[0158] The conductive aid is used in an amount of 0.01% by mass or more, preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and usually 50% by mass or less, preferably 30% by mass or less, more preferably 15% by mass or less in the electrode active material layer. If the content is lower than this range, the conductivity is sometimes insufficient. On the contrary, if the content is higher than this range, the battery capacity is sometimes reduced.

[0159] (Other ingredients)

[0160] The secondary battery mixture sheet may further contain a thermoplastic resin.

[0161] Examples of the thermoplastic resin include polyvinylidene fluoride, polypropylene, polyethylene, polystyrene, polyethylene terephthalate, and polyoxyethylene, etc. One type may be used alone, or two or more types may be used in any combination and ratio.

[0162] The ratio of thermoplastic resin to electrode active material is usually more than 0.01 mass %, preferably more than 0.05 mass %, more preferably more than 0.10 mass %, and usually less than 3.0 mass %, preferably less than 2.5 mass %, more preferably less than 2.0 mass %. By adding thermoplastic resin, the mechanical strength of electrode can be improved. If it exceeds this scope, the ratio of active material in secondary battery mixture is reduced, and sometimes the problem of reduced capacity of battery or the problem of increased resistance between active material is generated.

[0163] The secondary battery mixture disclosed in the present invention is particularly suitable for lithium-ion solid-state secondary batteries.

[0164] In addition, it is suitable for sulfide-based solid-state secondary batteries.

[0165] When used in a solid-state secondary battery, the secondary battery mixture of the present disclosure is usually used in a sheet form.

[0166] The secondary battery composite sheet disclosed in the present invention can be made into a positive electrode sheet or a negative electrode sheet. In addition, it can also be made into a solid electrolyte layer sheet. Among these, when it is made into an electrode sheet, it also contains active material particles. The active material particles can be made into positive electrode active materials and negative electrode active materials. The secondary battery sheet disclosed in the present invention can be more suitable as a positive electrode sheet using a positive electrode active material. In addition, when it is made into an electrode sheet, it can contain a conductive auxiliary agent as needed.

[0167] (Non-aqueous electrolyte)

[0168] When the secondary battery mixture of the present disclosure is used in a battery having a non-aqueous electrolyte, the non-aqueous electrolyte is not particularly limited, and one or more of the known solvents such as propylene carbonate, ethylene carbonate, butylene carbonate, γ-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, etc. can be used. The electrolyte can also use any existing known electrolyte, and LiClO4, LiAsF6, LiPF6, LiBF4, LiCl, LiBr, CH3SO3Li, CF3SO3Li, cesium carbonate, etc. can be used.

[0169] (Manufacturing method)

[0170] The manufacturing method of the secondary battery composite sheet disclosed in the present invention preferably uses the raw material composition obtained by mixing the above-mentioned components and sheets it. In sheeting, in order to save the drying process, it is preferably a method of applying shear stress to the raw material composition as a powder by reducing or completely not using the amount of liquid medium, not preparing slurry, and performing the process. In addition, in order to reduce the load of the device, a small amount of solvent can also be added as a lubricant. The solvent is preferably an organic solvent, and as the amount of solvent contained, it is preferably 10% by mass or less, more preferably 5% by mass or less, and further preferably 3% by mass or less relative to the raw material composition.

[0171] The secondary battery mixture sheet disclosed in the present invention can also be obtained by a method for producing a secondary battery mixture sheet having the following steps:

[0172] Step (1), applying shear force while mixing a raw material composition containing a solid electrolyte and / or an electrode active material and a binder;

[0173] Step (2), forming the secondary battery mixture obtained in the above step (1) into a block shape; and

[0174] Step (3) is to roll the block-shaped secondary battery mixture obtained in the step (2) into a sheet.

[0175] In the above-mentioned step (1), in the stage of imparting shear force while mixing the raw material composition, the obtained secondary battery mixture exists in a state where solid electrolytes, binders, etc. are only mixed without a certain form. As a specific mixing method, a method for mixing using a W-type mixer, a V-type mixer, a drum mixer, a ribbon mixer, a conical screw mixer, a single screw mixer, a twin screw mixer, a milling machine, a stirring mixer, a planetary mixer, a Henschel mixer, a high-speed mixer, etc. can be cited.

[0176] In the above-mentioned step (1), the mixing conditions only need to set the rotation speed and mixing time appropriately. For example, the rotation speed is suitably below 15000rpm. It is preferably above 10rpm, more preferably above 1000rpm, and further preferably above 3000rpm, and preferably below 12000rpm, more preferably below 11000rpm, and further preferably within the range of 10000rpm. If it is lower than the above-mentioned range, mixing takes time and productivity is affected. In addition, if it exceeds the above-mentioned range, fibrillation is excessively performed, and it is possible to form an electrode mixture sheet with poor strength.

[0177] In the above step (1), the temperature is preferably 30°C or higher, more preferably 60°C or higher.

[0178] In addition, it is preferred that a step (A) of mixing and dispersing the raw material composition is included before the step (1). In the step (A), mixing is preferably performed with as small a shear force as possible.

[0179] In the above-mentioned step (A), the mixing conditions only need to appropriately set the rotation speed and mixing time. For example, the rotation speed is preferably below 1000rpm. In addition, it is more preferably below 500rpm. The lower limit is preferably above 10rpm, more preferably above 15rpm, and further preferably above 20rpm. If it is lower than the above-mentioned range, mixing takes time and productivity is affected. In addition, if it exceeds the above-mentioned range, fibrillation is excessively carried out, and it is possible to become an electrode mixture sheet with poor strength. In addition, by mixing below room temperature, the raw material composition can be dispersed while suppressing fibrillation.

[0180] In the above step (A), the mixing temperature is preferably 19° C. or lower.

[0181] By adopting such a temperature range, it is possible to process into a desired sheet shape in a shorter time.

[0182] PTFE has two transition temperatures at about 19°C and about 30°C. At less than 19°C, PTFE can be easily mixed while maintaining its shape. However, if it exceeds 19°C, the structure of the PTFE particles becomes loose and becomes more sensitive to mechanical shear. At a temperature exceeding 30°C, a higher degree of fibrillation occurs.

[0183] Therefore, when a PTFE resin is used as the fibrillar resin, the step (A) is preferably carried out at a temperature of 19°C or lower, preferably 0°C to 19°C.

[0184] That is, in such step (A), it is preferred to mix and homogenize without causing fibrillation. Then, it is preferred to perform fibrillation in the subsequent steps (1) to (5).

[0185] In the above step (2), forming into a block shape means forming the secondary battery mixture into one block.

[0186] Specific examples of the method for forming the block include extrusion molding, press molding, and the like.

[0187] In addition, the so-called "block-shaped" is not a particularly specific shape, as long as it is in a block-shaped state, including rod-shaped, sheet-shaped, spherical, cubic and other forms. The size of the block is preferably such that the diameter of the cross section or the smallest side is 10000 μm or more, and more preferably 20000 μm or more.

[0188] As a specific rolling method in the above step (3), a method of rolling using a roll press, a flat plate press, a calender roll machine or the like can be mentioned.

[0189] In addition, after step (3), it is also preferred to have step (4): applying a greater load to the obtained calendered sheet to calender it into a thinner sheet. It is also preferred to repeat step (4). In this way, the calendered sheet is not thinned all at once, but is calendered little by little in stages, thereby making the softness better.

[0190] The number of times of performing step (4) is preferably 2 to 10 times, and more preferably 3 to 9 times.

[0191] As a specific calendering method, for example, there is a method in which two or more rolls are rotated and a calendered sheet is passed between the rolls to thereby process the sheet into a thinner sheet.

[0192] In addition, from the perspective of adjusting the diameter of the fibrils, it is also preferred to have a step (5) after the step (3) or the step (4): the rolled sheet is roughly crushed and then re-molded into a block shape, and rolled into a sheet shape. It is also preferred to repeat the step (5). The number of times of the step (5) is preferably 1 to 12 times, and more preferably 2 to 11 times.

[0193] In step (5), as a specific method for roughly crushing the rolled sheet and forming it into a block, there can be cited a method of folding the rolled sheet, a method of forming it into a rod or a film sheet, a method of forming it into a chip, etc. In the present disclosure, "roughly crushing" means changing the shape of the rolled sheet obtained in step (3) or step (4) into another shape in order to roll it into a sheet in the next step, and also includes the case of simply folding the rolled sheet.

[0194] In addition, step (4) may be performed after step (5), or the steps may be performed repeatedly.

[0195] Furthermore, uniaxial stretching or biaxial stretching may be performed in step (2) or (3), (4), or (5).

[0196] In addition, the fibril diameter (median value) can also be adjusted by adjusting the degree of coarse pulverization in step (5).

[0197] In the above steps (3), (4) or (5), the calendering rate is preferably 10% or more, more preferably 20% or more, and preferably 80% or less, more preferably 65% ​​or less, and more preferably 50% or less. If it is less than the above range, it takes time as the number of calendering increases, which affects productivity. In addition, if it exceeds the above range, fibrillation is excessively performed, and it is possible to form a secondary battery composite sheet with poor strength and flexibility.

[0198] It should be noted that the rolling rate mentioned here refers to the reduction rate of the thickness of the sample after processing relative to the thickness before the rolling process. The sample before rolling can be a block-shaped raw material composition or a sheet-shaped raw material composition. The thickness of the sample refers to the thickness in the direction of applying the load during rolling.

[0199] As mentioned above, PTFE powder is fibrillated by applying shear stress. And, in order to have the fibrous structure that fibril diameter (median value) is below 100nm, excessive shear stress can excessively promote fibrillation, sometimes damages flexibility. In addition, in terms of intensity, weak shear stress is sometimes insufficient. Therefore, when mixing or calendering, by applying appropriate shear stress to PTFE in the above-mentioned scope to promote fibrillation, calendering resin and extend into the operation of lamellar, it is possible to have the fibrous structure that fibril diameter (median value) is 100nm.

[0200] In the above steps (3), (4) or (5), the calendering rate is preferably 10% or more, more preferably 20% or more, and preferably 80% or less, more preferably 65% ​​or less, and more preferably 50% or less. If it is less than the above range, it takes time as the number of calendering increases, which affects productivity. In addition, if it exceeds the above range, fibrillation is excessively performed, and it is possible to form an electrode mixture sheet with poor strength and flexibility.

[0201] It should be noted that the rolling rate mentioned here refers to the reduction rate of the thickness of the sample after processing relative to the thickness before the rolling process. The sample before rolling can be a block-shaped raw material composition or a sheet-shaped raw material composition. The thickness of the sample refers to the thickness in the direction of applying the load during rolling.

[0202] Steps (2) to (5) are preferably performed at 30°C or higher, more preferably 60°C or higher.

[0203] As mentioned above, PTFE powder is fibrillated by applying shearing force. And, in order to have the fibrous structure that fibril diameter (median value) is below 100nm, excessive shearing stress can excessively promote fibrillation, sometimes damages flexibility. In addition, in terms of intensity, weak shearing stress is insufficient sometimes. Therefore, when mixing or during calendering, by applying appropriate shearing stress to PTFE in the above-mentioned scope to promote fibrillation, calendering resin and extend into the operation of lamellar, it is possible to have the fibrous structure that fibril diameter (median value) is 100nm.

[0204] As described above, the secondary battery composite sheet disclosed in the present invention can be made into any one of a positive electrode sheet and a negative electrode sheet. In the case of making a positive electrode composite sheet or a negative electrode sheet, in the manufacture of the secondary battery composite sheet, the positive electrode active material or the negative electrode active material is mixed with a solid electrolyte and a binder.

[0205] Hereinafter, the positive electrode and the negative electrode will be described.

[0206] (positive electrode)

[0207] In the present disclosure, the positive electrode is preferably composed of a current collector and the positive electrode sheet described above.

[0208] Examples of the material of the positive electrode current collector include metals such as aluminum, titanium, tantalum, stainless steel, nickel, or alloys thereof, and carbon materials such as carbon cloth and carbon paper. Among them, metal materials, particularly aluminum or alloys thereof, are preferred.

[0209] As the shape of the current collector, in the case of metal materials, metal foil, metal cylinder, metal coil, metal plate, metal plate net, stamping metal, foamed metal, etc. can be enumerated, and in the case of carbon materials, carbon plate, carbon film, carbon cylinder, etc. can be enumerated. Among these, metal foil is preferred. It should be noted that metal foil can be suitably formed into a mesh.

[0210] The thickness of the metal foil is arbitrary, usually 1 μm or more, preferably 3 μm or more, more preferably 5 μm or more, and usually 1 mm or less, preferably 100 μm or less, more preferably 50 μm or less. If the metal foil is thinner than this range, the strength required as a current collector is sometimes insufficient. On the contrary, if the metal foil is thicker than this range, the handling property is sometimes impaired.

[0211] In addition, from the perspective of reducing the electrical contact resistance between the current collector and the positive electrode mixture sheet, it is also preferred that a conductive auxiliary agent is coated on the surface of the current collector. Examples of the conductive auxiliary agent include carbon or precious metals such as gold, platinum, and silver.

[0212] The positive electrode may be produced by a conventional method, for example, a method in which the positive electrode sheet and the current collector are laminated with a binder and then dried.

[0213] The density of the positive electrode sheet is preferably 2.0 g / cm 3 More preferably, 2.1 g / cm 3 More preferably, 2.3 g / cm 3 Above, and preferably 4.0 g / cm 3 Below, more preferably 3.9 g / cm 3 Below, more preferably 3.8 g / cm 3 If the range is exceeded, the conductivity between the active materials decreases, and sometimes the battery resistance increases and high output cannot be obtained. If it is less than this range, the content of hard and easily broken active materials is low, and sometimes the battery has a low capacity.

[0214] The thickness of the positive electrode is not particularly limited. From the perspective of high capacity and high output, the thickness of the composite sheet after subtracting the thickness of the collector is preferably 10 μm or more, more preferably 20 μm or more, and preferably 500 μm or less, more preferably 450 μm or less, relative to a single side of the collector as a lower limit.

[0215] In addition, a positive electrode having a substance having a different composition attached to the surface of the positive electrode may also be used. Examples of the surface-attached substance include oxides such as aluminum oxide, silicon oxide, titanium oxide, zirconium oxide, magnesium oxide, calcium oxide, boron oxide, antimony oxide, and bismuth oxide; sulfates such as lithium sulfate, sodium sulfate, potassium sulfate, magnesium sulfate, calcium sulfate, and aluminum sulfate; carbonates such as lithium carbonate, calcium carbonate, and magnesium carbonate; carbon; and the like.

[0216] (negative electrode)

[0217] In the present disclosure, the negative electrode is preferably composed of a current collector and the negative electrode sheet described above.

[0218] The material of the negative electrode current collector includes metals such as copper, nickel, titanium, tantalum, stainless steel, or alloys thereof; and carbon materials such as carbon cloth and carbon paper. Among them, metal materials are preferred, and copper, nickel, or alloys thereof are particularly preferred.

[0219] As the shape of the current collector, in the case of metal materials, metal foil, metal cylinder, metal coil, metal plate, metal plate mesh, stamping metal, foamed metal, etc. can be cited, and in the case of carbon materials, carbon plate, carbon film, carbon cylinder, etc. can be cited. Among these, metal foil is preferred. It should be noted that the metal foil can be suitably formed into a mesh. The thickness of the metal foil is arbitrary, usually more than 1 μm, preferably more than 3 μm, more preferably more than 5 μm, and usually less than 1 mm, preferably less than 100 μm, more preferably less than 50 μm. If the metal foil is thinner than this range, the strength required as a current collector is sometimes insufficient. On the contrary, if the metal foil is thicker than this range, the handleability is sometimes impaired.

[0220] The negative electrode may be produced by a conventional method, for example, a method in which the negative electrode sheet and the current collector are laminated with a binder and then dried.

[0221] The density of the negative electrode sheet is preferably 1.3 g / cm 3 More preferably, 1.4 g / cm 3 More preferably, 1.5 g / cm 3 Above, and preferably 2.0 g / cm 3 Below, more preferably 1.9 g / cm 3 Below, more preferably 1.8 g / cm 3If the range is exceeded, the permeability of the solid electrolyte to the interface between the current collector and the active material is reduced, and the charge-discharge characteristics under high current density are reduced, and sometimes high output cannot be obtained. In addition, if it is less than this range, the conductivity between the active materials is reduced, and sometimes the battery resistance increases and high output cannot be obtained.

[0222] The thickness of the negative electrode is not particularly limited. From the perspective of high capacity and high output, the thickness of the composite sheet after deducting the thickness of the metal foil of the collector is preferably 10 μm or more, more preferably 20 μm or more, and preferably 500 μm or less, more preferably 450 μm or less, relative to a single side of the collector.

[0223] (Secondary battery)

[0224] The present disclosure also relates to a secondary battery using the secondary battery mixture sheet.

[0225] The secondary battery is preferably a lithium ion battery. In addition, the secondary battery can be a solid-state battery or a secondary battery containing a liquid electrolyte.

[0226] The secondary battery of the present disclosure is a secondary battery having the above-mentioned secondary battery mixture sheet of the present disclosure as a positive electrode. Here, there are no particular limitations on the negative electrode and the solid electrolyte layer, and any known materials can be used.

[0227] Hereinafter, the separator and the battery case used in the secondary battery of the present disclosure will be described in detail.

[0228] The method for manufacturing a secondary battery disclosed herein can be, for example, firstly stacking the above-mentioned positive electrode, solid electrolyte layer sheet, and negative electrode in order and pressing them to manufacture a secondary battery.

[0229] By using the secondary battery mixture sheet of the present disclosure, it is possible to manufacture a secondary battery with a low water content in the system, and it is possible to manufacture a secondary battery with good performance, which is suitable.

[0230] (Secondary battery using electrolyte)

[0231] The electrode produced using the secondary battery mixture sheet of the present disclosure can be used as a positive electrode or a negative electrode in various secondary batteries using an electrolyte. The secondary battery is a battery using a non-aqueous electrolyte, and an example of the secondary battery is a lithium ion battery.

[0232] (Electrolyte)

[0233] As the non-aqueous electrolyte solution, a non-aqueous electrolyte solution prepared by dissolving a known electrolyte salt in a known organic solvent for dissolving the electrolyte salt can be used.

[0234] There are no particular limitations on the organic solvent used to dissolve the electrolyte salt, and known hydrocarbon solvents such as propylene carbonate, ethylene carbonate, butylene carbonate, γ-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate can be used; and one or more of fluorine-based solvents such as fluoroethylene carbonate, fluoroethers, and fluorinated carbonates can be used.

[0235] As electrolyte salts, for example, LiClO4, LiAsF6, LiBF4, LiPF6, LiN(SO2CF3)2, LiN(SO2C2F5)2, etc. can be mentioned. From the perspective of good cycle characteristics, LiPF6, LiBF4, LiN(SO2CF3)2, LiN(SO2C2F5)2 or a combination thereof is particularly preferred.

[0236] The concentration of the electrolyte salt is preferably 0.8 mol / L or more, more preferably 1.0 mol / L or more. The upper limit depends on the organic solvent for dissolving the electrolyte salt, but is usually 1.5 mol / L.

[0237] (Battery Design)

[0238] The electrode mixture group may be any one of an electrode mixture group having a layered structure in which a separator is interposed between the positive electrode and the negative electrode, and an electrode mixture group having a structure in which the positive electrode and the negative electrode are spirally wound with the separator interposed therebetween.

[0239] (Diaphragm)

[0240] The material and shape of the above-mentioned separator are not particularly limited as long as the electrolyte is stable and the liquid retention is excellent, and known separators can be used. For example, it is preferred to use a porous sheet or non-woven fabric-like material with excellent liquid retention, such as resin, glass fiber, inorganic material, etc.

[0241] As materials for resin and glass fiber separators, polyolefins such as polyethylene and polypropylene, aromatic polyamides, PTFE, polyethersulfone, glass filters, etc. can be used. These materials such as polypropylene / polyethylene two-layer membranes and polypropylene / polyethylene / polypropylene three-layer membranes can be used alone or in any combination and ratio.

[0242] Among them, the separator is preferably a porous sheet or nonwoven fabric made of polyolefin such as polyethylene or polypropylene from the viewpoint of good electrolyte permeability and shutdown effect.

[0243] In addition, when a porous material such as a porous sheet or nonwoven fabric is used as a diaphragm, the porosity of the diaphragm is arbitrary, usually 20% or more, preferably 35% or more, more preferably 45% or more, and usually 90% or less, preferably 85% or less, more preferably 75% or less. If the porosity is too small compared to the above range, there is a tendency for the membrane resistance to increase and the rate characteristics to deteriorate. In addition, if it is too large compared to the above range, there is a tendency for the mechanical strength of the diaphragm to decrease and the insulation to decrease.

[0244] In addition, the average pore size of the diaphragm is also arbitrary, usually 0.5 μm or less, preferably 0.2 μm or less, and usually 0.05 μm or more. If the average pore size exceeds the above range, short circuit is likely to occur. In addition, if it is less than the above range, the membrane resistance sometimes increases and the rate characteristics decrease.

[0245] On the other hand, as inorganic materials, oxides such as aluminum oxide and silicon dioxide, nitrides such as aluminum nitride and silicon nitride, and sulfates such as barium sulfate and calcium sulfate are used, and materials in the form of particles or fibers are used.

[0246] As a form, a non-woven fabric, a woven fabric, a microporous film or other thin film-shaped material is used. In the case of a thin film, a film with a pore size of 0.01 μm to 1 μm and a thickness of 5 μm to 50 μm is preferably used. In addition to the above-mentioned independent thin film shape, a separator formed by forming a composite porous layer containing particles of the above-mentioned inorganic substance on the surface of the positive electrode and / or the negative electrode using a resin binder can also be used.

[0247] For example, a fluororesin is used as a binder, and alumina particles having a particle size of 90% less than 1 μm are formed into a porous layer on both sides of the positive electrode.

[0248] The material of the housing is not particularly limited as long as it is a material that is stable to the electrolyte used. Specifically, metals such as nickel-plated steel, stainless steel, aluminum or aluminum alloy, magnesium alloy, or a laminated film (laminated film) of resin and aluminum foil are used. From the perspective of lightweight, it is preferred to use a metal such as aluminum or an aluminum alloy, or a laminated film.

[0249] In the case of using metal, there can be mentioned a case in which metals are welded together by laser welding, resistance welding, or ultrasonic welding to form a sealed package structure; or a case in which the above metals are used to form a riveted structure through a resin gasket. In the case of using the above laminated film, there can be mentioned a case in which a sealed package structure is formed by thermally bonding resin layers to each other. In order to improve the sealing performance, a resin different from the resin used in the laminated film can also be sandwiched between the above resin layers. In particular, in the case of forming a sealed structure by thermally bonding the resin layers through the collector terminal, since the metal is bonded to the resin, it is preferred to use a resin having a polar group or a modified resin into which a polar group is introduced as the sandwiched resin.

[0250] The secondary battery may have any shape, and examples thereof include cylindrical, rectangular, laminated, button, and large shapes. The shape and structure of the positive electrode, negative electrode, and separator may be changed according to the shape of each battery.

[0251] Example

[0252] The present disclosure will be specifically described below based on examples.

[0253] In the following examples, "part" and "%" mean "part by mass" and "mass %", respectively, unless otherwise specified.

[0254] [Production example 1]

[0255] At the moment when 367g of TFE is consumed from the start of polymerization (35.6% by mass relative to the total polymerization amount of 1032g of TFE), an aqueous solution (concentration of 4.0ppm relative to the aqueous medium) obtained by dissolving 12.0mg of hydroquinone as a free radical scavenger in 20ml of water is pressed into TFE. After that, the polymerization is continued. When the polymerization amount of TFE reaches 1000g from the start of polymerization, the supply of TFE is stopped, and the gas in the system is immediately released to reach normal pressure, and the polymerization reaction is terminated to obtain a polytetrafluoroethylene aqueous dispersion (solid content 31.2% by mass). The obtained polytetrafluoroethylene aqueous dispersion is diluted to a solid content concentration of 15%, and slowly stirred in a container with a stirrer in the presence of nitric acid to solidify the polytetrafluoroethylene. The solidified polytetrafluoroethylene is separated and dried at 160°C for 18 hours to obtain powdered PTFE-1.

[0256] [Production example 2]

[0257] With reference to Preparation Example 3 of International Publication No. 2015-080291, powdered PTFE-2 was prepared.

[0258] [Production example 3]

[0259] With reference to Preparation Example 1 of International Publication No. 2012 / 086710, powdered PTFE-3 was prepared.

[0260] [Production example 4]

[0261] With reference to Preparation Example 1 of International Patent No. 2012-063622, powdered PTFE-4 was prepared.

[0262] Table 1 shows the physical properties of the produced PTFE.

[0263] [Table 1]

[0264] Making PTFE Standard specific gravity Moisture content after drying (ppm) PTFE-1 2.16 <250 PTFE-2 2.15 <250 PTFE-3 2.16 <250 PTFE-4 2.19 <250

[0265] (Example 1)

[0266] Weighing the positive electrode active material LiNi 0.8 Mn 0.1 Co 0.1 O2, conductive additive (carbon black: Super P Li) and powdered PTFE-1 were mixed using a high-speed mixer (500 rpm, 1 minute). The container was cooled to 10°C and stirred. Thereafter, the mixture was stirred using a high-speed mixer (10000 rpm, 3 minutes) to obtain a mixture. The container was heated to 60°C and stirred.

[0267] The powdered PTFE-1 was dried in a vacuum dryer at 50°C for 1 hour before use. The powdered PTFE used was PTFE that was previously sieved with a stainless steel sieve with a mesh size of 500 μm and remained on the sieve. The composition ratio was adjusted as shown in Table 2.

[0268] The obtained mixture was formed into a block, rolled into a sheet, and heated to 80°C for rolling.

[0269] Afterwards, the calendered sheet just obtained is folded in half and roughly crushed, and after being formed into a block again, it is rolled into a sheet with a metal roller on a flat plate, thereby promoting fibrillation, and the above process is repeated 4 times. Afterwards, by further rolling, a secondary battery composite sheet with a thickness of 500μm is obtained. Then, the secondary battery composite sheet is cut out and put into a press for rolling. Then, a load of 5kN is repeatedly applied to adjust the thickness. The gap is adjusted in such a way that the thickness of the final secondary battery composite sheet becomes 150μm. The initial rolling rate is the largest, which is 39%.

[0270] (Example 2)

[0271] Using powdered PTFE-3, the composition ratio was adjusted to that shown in Table 2, and a sheet was formed in the same manner as in Example 1.

[0272] (Example 3)

[0273] Using powdered PTFE-2, the composition ratio was adjusted to that shown in Table 2, and a sheet was formed in the same manner as in Example 1.

[0274] (Example 4)

[0275] Using powdered PTFE-4, the composition ratio was adjusted to that shown in Table 2, and a sheet was formed in the same manner as in Example 1.

[0276] (Example 5)

[0277] Using powdered PTFE-1, the composition ratio described in Table 2 was adjusted, and a sheet was formed in the same manner as in Example 1.

[0278] (Example 6)

[0279] Instead of the conductive additive, a sulfide-based solid electrolyte (0.75Li2S·0.25P2S5) and a positive electrode active material LiNi were weighed. 0.8 Mn 0.1 Co 0.1 O2, powdered PTFE-1, using powdered PTFE-1 adjusted to the composition ratio described in Table 2, according to the same procedure as Example 1 to form a sheet.

[0280] (Example 7)

[0281] Instead of the conductive additive, a sulfide-based solid electrolyte (0.75Li2S·0.25P2S5) and a positive electrode active material LiNi were weighed. 0.8 Mn 0.1 Co 0.1 O2, powdered PTFE-4, using powdered PTFE-4 adjusted to the composition ratio described in Table 2, according to the same procedure as Example 1 to form a sheet.

[0282] (Example 8)

[0283] Weighing sulfide solid electrolyte Li 10 GeP2S 12 and positive electrode active material LiNi 0.8 Mn 0.1 Co 0.1 O2, a conductive additive, and powdered PTFE-4 were adjusted to have the composition ratio shown in Table 2 using powdered PTFE-4, and a sheet was formed in the same manner as in Example 1.

[0284] (Comparative Example 1)

[0285] Weighing the positive electrode active material LiNi 0.8 Mn 0.1 Co0.1 O2, a conductive additive (carbon black: Super P Li) and powdered PTFE-4 were stirred using a high-speed mixer (10,000 rpm, 4 minutes) to obtain a mixture, and the container was heated to 60°C for stirring.

[0286] It should be noted that the powdered PTFE-4 was dried at 50°C for 1 hour in a vacuum dryer before use. The powdered PTFE was sieved in advance with stainless steel sieves of 425 μm and 355 μm, and the PTFE that passed through the 425 μm sieve and remained on the 355 μm sieve was used. The composition ratio was adjusted as described in Table 2.

[0287] The obtained mixture is formed into a block and rolled into a sheet. The rolling is carried out at room temperature.

[0288] Afterwards, the calendered sheet just obtained is folded in half and roughly crushed, and after being formed into a block again, it is rolled into a sheet with a metal roller on a flat plate, thereby promoting fibrillation, and the above process is repeated 3 times. Afterwards, by further rolling, a secondary battery composite sheet with a thickness of 500μm is obtained. Then, the secondary battery composite sheet is cut out and put into a press for rolling. Then, a load of 5kN is repeatedly applied to adjust the thickness. The gap is adjusted in such a way that the thickness of the final secondary battery composite sheet becomes 150μm.

[0289] Each test was performed by the following method.

[0290] [Determination of water content]

[0291] The powdered PTFE was dried at 50°C for 1 hour in a vacuum dryer before use. Regarding the moisture content of the vacuum-dried PTFE, a Karl Fischer moisture meter (ADP-511 / MKC-510N manufactured by Kyoto Electronics Industry Co., Ltd.) with a boat-type moisture vaporizer was used, and the moisture vaporizer was heated to 210°C to measure the vaporized moisture. As a carrier gas, nitrogen was circulated at a flow rate of 200 mL / min, and the measurement time was set to 30 minutes. In addition, Chem-Aqua was used as a Karl Fischer reagent. The sample amount was set to 1.5 g.

[0292] [PTFE fibril diameter (maximum fibril diameter, median value, third quartile of fibril diameter)]

[0293] (1) Using a scanning electron microscope (S-4800, manufactured by Hitachi, Ltd.), a magnified photograph (7000 times) of the sheet-like solid electrolyte layer was taken to obtain an image.

[0294] (2) Draw two lines at equal intervals horizontally on the image to divide the image into three equal parts.

[0295] (3) For all PTFE fibers located on the upper straight line, measure the diameter of each PTFE fiber at three locations, and take the average value as the diameter of the PTFE fiber. The three locations to be measured are the intersection of the PTFE fiber and the straight line, and the locations offset 0.5 μm upward and downward from the intersection. (Not including unfiberized PTFE primary particles).

[0296] (4) The above-mentioned operation (3) is performed on all PTFE fibers located on the lower straight line.

[0297] (5) Starting from the first image, move 1 mm to the right of the screen and take another photo, and measure the diameter of the PTFE fiber using the above (3) and (4). Repeat this operation until the number of measured fibers exceeds 80.

[0298] (6) The median value of the diameter of all PTFE fibers measured above is taken as the size of the original fiber diameter. The mean value, standard deviation, third quartile, and maximum value are determined in the same manner. It should be noted that the maximum value refers to the maximum value when 80 fibers are measured.

[0299] [Softness evaluation]

[0300] The prepared solid electrolyte sheet was cut into 2 cm long and 6 cm wide as a test piece. After being wound onto a round rod with a diameter of 4 mm, the test piece was visually inspected and evaluated according to the following criteria. The case where no damage or cracks were confirmed was evaluated as ○, and the case where cracks were confirmed was evaluated as ×.

[0301] [Strength measurement]

[0302] A digital dynamometer (ZTS-20N manufactured by IMADA) was used to measure the strength of each sample using a 4 mm wide strip electrode mixture test piece at 100 mm / min. The distance between the chucks was set to 30 mm. Displacement was given until fracture, and the maximum stress of the measurement result was used as the strength of each sample. The test was performed 5 times, and the average value was used as the strength.

[0303] Table 2 shows the test results.

[0304]

[0305] Next, a gold electrode was formed on the surface of the positive electrode mixture sheet prepared in Example 7 by sputtering.

[0306] Next, a sulfide-based solid electrolyte (0.75Li2S·0.25P2S5) and PTFE-4 were mixed at a ratio of 98:2 to prepare a solid electrolyte sheet having a thickness of 200 μm.

[0307] The prepared solid electrolyte sheet was overlapped with the Li foil and the insulating sheet, and uniaxial molding was performed for 3 minutes at a load of 60 kN to integrate them, and a punched half-cell with a diameter of 10 mm was produced. The prepared half-cell was placed in a flat battery and placed in a tank at 45°C for 12 hours. The charge and discharge were performed at 0.1C (0.05C cutoff).

[0308] As a result of performing eight cycles of charge and discharge, when the third cycle was regarded as 100%, the capacity retention rate at the eighth cycle was 98.6%.

[0309] According to the results in Table 2, the sheet-like solid electrolyte layer of the example is excellent in physical properties.

[0310] Industrial Applicability

[0311] The secondary battery mixture disclosed in the present invention and the secondary battery mixture sheet containing the same can be used for the production of a solid-state secondary battery.

Claims

1. A secondary battery mixture, comprising a solid electrolyte and / or an electrode active material, and a binder, characterized in that: The binder is a fibrillar resin. The fibrillar resin has a fibrous structure with a maximum fibril diameter of 90 nm or more.

2. A secondary battery mixture, comprising a solid electrolyte and / or an electrode active material, and a binder, characterized in that: The binder is a fibrillar resin. The fibrillar resin has a fibrous structure in which the third quartile of the fibril diameter is 35 nm or more.

3. The secondary battery mixture according to claim 1 or 2, characterized in that: The fibrillar resin has a fibrous structure in which the median value of the fibril diameter is 100 nm or less. 4 . The secondary battery mixture according to claim 1 , which is used for a lithium ion secondary battery.

5. The secondary battery mixture according to any one of claims 1 to 4, which is a secondary battery mixture obtained using a raw material composition containing a solid electrolyte and / or an electrode active material, and a binder, wherein: The binder of the raw material composition is a powdered polytetrafluoroethylene resin.

6. The secondary battery mixture according to claim 5, wherein The water content of the powdered polytetrafluoroethylene resin is 500 ppm or less.

7. The secondary battery mixture according to claim 5 or 6, wherein The standard specific gravity of powdered polytetrafluoroethylene resin is 2.12 to 2.

20.

8. The secondary battery mixture according to any one of claims 5 to 7, wherein The powdery polytetrafluoroethylene resin contains 50 mass % or more of a polytetrafluoroethylene resin having a secondary particle size of 450 μm or more.

9. The secondary battery mixture according to any one of claims 5 to 8, wherein The powdery polytetrafluoroethylene resin contains 80 mass % or more of a polytetrafluoroethylene resin having a secondary particle size of 450 μm or more.

10. The secondary battery mixture according to any one of claims 1 to 9, wherein The electrode active material is a positive electrode active material. 11 . The secondary battery mixture according to claim 1 , which is used for a solid-state secondary battery. 12 . A secondary battery mixture sheet comprising the secondary battery mixture according to claim 1 . 13 . An electrode comprising the secondary battery mixture sheet according to claim 12 .

14. A method for manufacturing a secondary battery composite sheet, the method comprising: Step (1): applying shear force while mixing a raw material composition containing a solid electrolyte and / or an electrode active material and a binder; Step (2): forming the secondary battery mixture obtained in the step (1) into a block shape; and Step (3): rolling the block-shaped secondary battery mixture obtained in the step (2) into a sheet shape, in, The binder is a powdery fibrillar resin having a fibrous structure with a maximum fibril diameter of 90 nm or more. 15 . A secondary battery comprising the secondary battery mixture sheet according to claim 12 .