A multifunctional coupled pre-coated ultrafiltration membrane and its preparation and application method
By double-layer coating of Bi2O3/TiO2 composite metal oxide and carbon-based materials on the ultrafiltration membrane, a multifunctional coupled ultrafiltration membrane that combines adsorption, photocatalytic oxidation and membrane retention functions, the removal of small and medium-sized molecules of the prior art was solved. The problem of membrane pollution improves the water treatment effect and membrane anti-pollution ability.
Patent Information
- Application Number
- CN202411282892.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-13
AI Technical Summary
Existing ultrafiltration technology has difficulties in removing small-molecular pollutants and membrane pollution in water, especially in photocatalytic reactions, where leakage risks of small-molecular-weight intermediate products and membrane pollution problems hinder the development of photocatalytic films.
Using a multifunctional coupled pre-coated ultrafiltration membrane, the pollutant removal effect is improved by double-layer coating Bi2O3/TiO2 composite metal oxide and carbon-based material on the ultrafiltration membrane, combining adsorption, photocatalytic oxidation and membrane retention functions. And slow down membrane contamination.
It significantly improves the removal rate of organic matter in water, the flux recovery rate is increased by more than 17%, and the removal rate of UV254 and DOC is increased by more than 20%, solving the problem of leakage of small molecular weight intermediate products, and enhancing the hydrophilic properties and anti-pollution ability of ultrafiltration membranes. .
Smart Images

Figure CN118788143B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of water treatment, and in particular to a multifunctional coupled pre-coated ultrafiltration membrane and a preparation and application method thereof. Background Art
[0002] In recent years, water pollution has become increasingly prominent, and various pollutants have been frequently detected, which are difficult to be effectively removed by conventional purification technology. In order to improve the safety of water supply, ultrafiltration technology has been promoted in drinking water plants. Ultrafiltration technology has the advantages of less dosage of reagents and stable operation, but the removal of small molecule pollutants and membrane pollution still hinder the widespread application of ultrafiltration membranes to a certain extent.
[0003] Membrane modification is an effective way to improve the removal effect of pollutants and control membrane pollution. Common modification methods include membrane surface modification and membrane material modification. In recent years, photocatalytic membranes that combine filter membranes with photocatalysis have become a research hotspot for multifunctional ultrafiltration membranes. On the one hand, photocatalytic membranes solve the problems of difficulty in separating nanocatalysts in water, low recycling rate, and secondary pollution; on the other hand, they slow down the formation of mud cake layer on the membrane surface and reduce the frequency of membrane cleaning. However, in the photocatalytic reaction, there is a risk of leakage of small molecular weight intermediates, which restricts the development of photocatalytic membranes. Summary of the invention
[0004] In view of the above analysis, the embodiments of the present invention aim to provide a multifunctional coupled pre-coated ultrafiltration membrane and a preparation and application method thereof, so as to solve the difficulty in removing small molecule pollutants and membrane pollution problems associated with existing ultrafiltration technology.
[0005] In one aspect, the present invention provides a multifunctional coupled pre-coated ultrafiltration membrane, which can be used to remove pollutants in water, at least can be used to remove organic matter in water, and the multifunctional coupled pre-coated ultrafiltration membrane comprises:
[0006] Ultrafiltration membrane;
[0007] The load is coated on the filter membrane, and the load amount of the load is 6~50g / m 2 ; The load includes Bi 2 O 3 / TiO 2 Composite metal oxide and carbon-based material, the carbon-based material, Bi 2 O 3 / TiO 2 The composite metal oxides are sequentially coated on the surface of the ultrafiltration membrane, and Bi 2 O 3 / TiO 2 The mass ratio of the composite metal oxide to the carbon-based material is 1:(1~3).
[0008] Furthermore, the material of the ultrafiltration membrane is one of polyvinylidene fluoride, polyether sulfone, polytetrafluoroethylene, polyamide, and ceramic membrane.
[0009] Furthermore, the Bi 2 O 3 / TiO 2 The molar ratio of Bi to Ti in the composite metal oxide is 0.04 to 0.10.
[0010] Furthermore, the carbon-based material is one or more of activated carbon, mesoporous carbon, and carbon nanotubes.
[0011] On the other hand, the present invention provides a method for preparing a multifunctional coupled pre-coated ultrafiltration membrane, which can at least be used to prepare the above-mentioned multifunctional coupled pre-coated ultrafiltration membrane, and the preparation method comprises the following steps:
[0012] S100: dispersing the load objects in water to obtain load suspensions;
[0013] S200: uniformly coating the load suspension on the surface of the ultrafiltration membrane in sequence to obtain a multifunctional coupled pre-coated ultrafiltration membrane;
[0014] The loading amount of the load is 6-50 g / m 2 ;
[0015] The load includes Bi 2 O 3 / TiO 2 Composite metal oxide and carbon-based material, the carbon-based material, Bi 2 O 3 / TiO 2 The composite metal oxides are sequentially coated on the surface of the ultrafiltration membrane, Bi 2 O 3 / TiO 2 The mass ratio of the composite metal oxide to the carbon-based material is 1:(1~3).
[0016] Furthermore, in step S100, the load is placed in water and dispersed by ultrasound, the frequency of the ultrasound is 30-50 kHz, and the ultrasound duration is 20-40 min.
[0017] Furthermore, the Bi 2 O 3 / TiO 2 The preparation method of the composite metal oxide comprises the following steps:
[0018] S101: slowly pouring a titanium precursor compound into glacial acetic acid, and then pouring the mixture into anhydrous ethanol, stirring to obtain liquid A, wherein the volume ratio of the titanium precursor compound, glacial acetic acid and anhydrous ethanol is 2:1:8;
[0019] The precursor compound of bismuth is dissolved in water to obtain liquid B, and the molar concentration of bismuth is 0.02~0.04mol / L;
[0020] S102: Mix liquid A and liquid B in a volume ratio of 1: (0.9-1.5), perform a hydrothermal reaction, separate the product obtained by the hydrothermal reaction from the reaction solution, dry it, and calcine it to obtain Bi 2 O 3 / TiO 2 Composite metal oxides.
[0021] Furthermore, in step S200, the ultrafiltration membrane is pretreated before being coated, and the pretreatment process is as follows: the ultrafiltration membrane is first soaked in a 50% to 70% ethanol solution for 15 to 30 minutes, and then soaked in deionized water for 24 to 30 hours.
[0022] Furthermore, in step S200, the transmembrane pressure difference during the coating process of the load is constant at 20-30 kPa.
[0023] In another aspect, the present invention provides an application method of a multifunctional coupled pre-coated ultrafiltration membrane, which can be applied to at least the above-mentioned multifunctional coupled pre-coated ultrafiltration membrane, including dark treatment and / or light treatment;
[0024] The dark treatment is to fix the multifunctional coupled pre-coated ultrafiltration membrane on a membrane reactor containing the liquid to be treated to perform dark adsorption;
[0025] The light treatment is to fix the multifunctional coupled pre-coated ultrafiltration membrane on a membrane reactor containing the liquid to be treated, and use ultraviolet light to irradiate the multifunctional coupled pre-coated ultrafiltration membrane for photocatalytic oxidation;
[0026] When the DOC content in the liquid to be treated is <2 mg / L, dark treatment is used;
[0027] When the DOC content in the liquid to be treated is >3 mg / L, light treatment is used;
[0028] When the DOC content in the treated liquid is in the range of 2 to 3 mg / L, dark treatment and light treatment are performed alternately.
[0029] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:
[0030] (1) The present invention modifies the ultrafiltration membrane by organically combining photocatalytic materials and carbon-based materials, which is of great significance for the improvement of ultrafiltration technology and the guarantee of water supply safety; the multifunctional coupled pre-coated ultrafiltration membrane of the present invention is a double-layer pre-coated ultrafiltration membrane, which has the functions of adsorption, photocatalytic oxidation and interception, so that the adsorption effect of carbon-based materials, Bi 2 O3 / TiO 2 The photocatalytic oxidation degradation of the composite material and the interception of the filter membrane can be realized simultaneously in situ on the composite material, which can effectively remove organic matter in water. Compared with the unmodified ultrafiltration membrane, the flux recovery rate of the multifunctional coupled pre-coated ultrafiltration membrane of the present invention can be increased by more than 17%. 254 And DOC (dissolved organic carbon) removal rate can be increased by more than 20%;
[0031] (2) The present invention will Bi 2 O 3 / TiO 2 Composite metal oxides and carbon-based materials are pre-coated on ultrafiltration membranes to prepare Bi 2 O 3 / TiO 2 Double-layer pre-coated ultrafiltration membrane with carbon-based materials and applied to water treatment process; construct a coupling system with adsorption, photocatalytic oxidation and membrane interception functions, which has the dual beneficial effects of improving the removal effect of pollutants and reducing membrane pollution;
[0032] (3) The modified ultrafiltration membrane of the present invention has a good removal effect on organic matter of different molecular weights in water, solves the problem of leakage of small molecular weight intermediates in the photocatalytic oxidation process, enhances the hydrophilicity of the ultrafiltration membrane, slows down membrane pollution, and has simple preparation methods and conditions.
[0033] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.
[0035] Figure 1 Fourier infrared spectra of UF, BT / PAC-UF, BT / CMK-3-UF, and BT / CNTs-UF in a specific embodiment after filtering actual surface water under dark and light conditions (in the figure, BT / PAC-UF, BT / CMK-3-UF, BT / CNTs-UF, and UF are represented by Ⅰ, Ⅱ, Ⅲ, and Ⅳ, respectively);
[0036] Figure 2are scanning electron microscope images of UF, BT / PAC-UF, BT / CMK-3-UF, and BT / CNTs-UF in a specific embodiment, wherein a~c are scanning electron microscope images of original UF and UF after filtering actual surface water under dark and light conditions, d~f are scanning electron microscope images of BT / PAC-UF, BT / CMK-3-UF, and BT / CNTs-UF after filtering actual surface water under dark conditions, and g~i are scanning electron microscope images of BT / PAC-UF, BT / CMK-3-UF, and BT / CNTs-UF after filtering actual surface water under light conditions;
[0037] Figure 3 The contact angle bar graphs of UF, BT / PAC-UF, BT / CMK-3-UF, and BT / CNTs-UF in the specific implementation manner after filtering actual surface water under dark and light conditions (in the figure, BT / PAC-UF, BT / CMK-3-UF, BT / CNTs-UF, and UF are represented by Ⅰ, Ⅱ, Ⅲ, and Ⅳ, respectively);
[0038] Figure 4 The specific implementation methods of UF, BT / PAC-UF, BT / CMK-3-UF, and BT / CNTs-UF are shown in Figure 2 for the UV in actual surface water. 254 The removal effect bar graph (BT / PAC-UF, BT / CMK-3-UF, BT / CNTs-UF and UF are represented by Ⅰ, Ⅱ, Ⅲ and Ⅳ respectively in the figure);
[0039] Figure 5 It is a bar graph showing the removal effect of UF, BT / PAC-UF, BT / CMK-3-UF and BT / CNTs-UF in the specific implementation mode on DOC in actual surface water under dark and light conditions (in the figure, BT / PAC-UF, BT / CMK-3-UF, BT / CNTs-UF and UF are represented by Ⅰ, Ⅱ, Ⅲ and Ⅳ respectively);
[0040] Figure 6 It is a bar chart of the removal effect of UF, BT / PAC-UF, BT / CMK-3-UF and BT / CNTs-UF in the specific implementation method on organic matter of different molecular weight in actual surface water under dark conditions (in the figure, BT / PAC-UF, BT / CMK-3-UF, BT / CNTs-UF and UF are represented by Ⅰ, Ⅱ, Ⅲ and Ⅳ respectively);
[0041] Figure 7It is a bar chart of the removal effect of UF, BT / PAC-UF, BT / CMK-3-UF and BT / CNTs-UF in the specific implementation method on organic matter of different molecular weight in actual surface water under illumination conditions (in the figure, BT / PAC-UF, BT / CMK-3-UF, BT / CNTs-UF and UF are represented by Ⅰ, Ⅱ, Ⅲ and Ⅳ respectively);
[0042] Figure 8 The diagram is a diagram showing changes in membrane flux during treatment of slightly polluted water by the ultrafiltration membrane and pre-coated ultrafiltration membrane in a specific embodiment. DETAILED DESCRIPTION
[0043] The preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.
[0044] In the description of the embodiments of the present invention, it should be noted that, unless otherwise clearly specified and limited, the term "connected" should be understood in a broad sense, for example, it can be a fixed connection, or a detachable connection, or an integral connection, which can be a mechanical connection, or an electrical connection, which can be a direct connection, or can be indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0045] The terms "top", "bottom", "above", "lower", and "on" used throughout the description are relative to the relative positions of components of a device, such as the relative positions of the top and bottom substrates within a device. It is understood that devices are multifunctional regardless of their orientation in space.
[0046] The common working surface of the present invention can be a plane or a curved surface, can be inclined, or can be horizontal. For the convenience of description, the embodiment of the present invention is placed on a horizontal plane and used on the horizontal plane, and "high and low" and "up and down" are defined in this way.
[0047] A specific embodiment of the present invention discloses a multifunctional coupled pre-coated ultrafiltration membrane, which can at least be used to remove organic matter (such as natural organic matter, macromolecular organic matter, etc.) in water. It has photocatalytic oxidation, adsorption and membrane retention functions, improves the pollution removal performance of the ultrafiltration membrane, and can slow down membrane pollution.
[0048] The multifunctional coupled pre-coated ultrafiltration membrane comprises:
[0049] Ultrafiltration membrane;
[0050] The load is coated on the filter membrane, and the load amount of the load is 6~50g / m 2 ; The load includes Bi2 O 3 / TiO 2 Composite metal oxide and carbon-based material, the carbon-based material, Bi 2 O 3 / TiO 2 The composite metal oxides are sequentially coated on the surface of the ultrafiltration membrane, and Bi 2 O 3 / TiO 2 The mass ratio of the composite metal oxide to the carbon-based material is 1:(1~3).
[0051] It should be noted that the pre-coating refers to pre-coating the functional material before filtration. The multifunctional coupled pre-coated ultrafiltration membrane of the present invention is not a disposable product, but can be filtered multiple times and can be used again after backwashing, and the load will hardly fall off.
[0052] Wherein, the material of the ultrafiltration membrane is one of polyvinylidene fluoride (PVDF), polyether sulfone, polytetrafluoroethylene, polyamide, ceramic membrane and the like.
[0053] The Bi 2 O 3 / TiO 2 The molar ratio of Bi to Ti in the composite metal oxide is 0.04 to 0.10.
[0054] The present invention adopts Bi 2 O 3 / TiO 2 The double-layer coating of composite metal oxides and carbon-based materials improves the removal effect of pollutants, enhances the hydrophilicity of ultrafiltration membranes, and effectively slows down membrane fouling. 2 Active substances generated by photocatalysis (such as photogenerated electrons, holes, hydroxyl radicals, etc., which have strong oxidizing properties and can degrade organic matter) remove organic matter, especially natural organic matter (such as humus, polysaccharides, organic acids, etc.) and difficult-to-degrade organic matter (such as antibiotics, endocrine disruptors, estrogen, etc.), improving the ultrafiltration membrane's decontamination performance and reducing membrane pollution. 2 O 3 Can improve the photocatalytic effect, bismuth-based semiconductor catalyst bismuth oxide (Bi 2 O 3 ) has excellent properties such as narrow band gap (2.8eV) and high dielectric constant, which is similar to TiO 2 After compounding, the recombination of photogenerated carriers can be effectively inhibited and the photocatalytic activity can be improved.
[0055] The carbon-based material of the present invention is placed in Bi 2 O 3 / TiO 2 The bottom of the composite metal oxide can absorb Bi 2 O3 / TiO 2 The small molecule intermediates of composite metal oxide photocatalysis avoid leakage caused by poor retention of small molecule organic matter by ultrafiltration membrane.
[0056] The carbon-based material is one or more of activated carbon (PAC), mesoporous carbon (CMK-3), and carbon nanotubes (CNTs) mixed in any proportion. The carbon-based material is in powder form. Specifically, the particle size of the carbon-based material ranges from 30 to 150 μm. The carbon-based material has good adsorption properties and has a strong adsorption capacity for natural organic matter in water and its byproducts of photocatalytic degradation (intermediates produced during the degradation of organic matter, such as small molecule intermediates), that is, it can intercept the byproducts brought about by photocatalytic degradation, reduce the membrane degradation caused by photocatalysis, and improve the membrane's anti-pollution ability. In addition, the introduction of carbon-based materials can effectively adsorb small molecular substances, effectively solving the problem that the filter membrane is difficult to intercept small molecular weight intermediates in the photocatalytic oxidation process.
[0057] The multifunctional coupled pre-coated ultrafiltration membrane of the present invention couples the adsorption, photocatalytic oxidation and membrane interception functions, and the carbon-based material layer can simultaneously adsorb organic matter in water and intermediate products produced by photocatalysis. 2 O 3 / TiO 2 The composite metal oxide photocatalytic process can simultaneously degrade organic matter in water and adsorbed in the carbon-based material layer. There is a dynamic balance between the two, which, combined with the membrane interception function, effectively improves the pollutant removal effect and reduces membrane pollution.
[0058] The load of the multifunctional coupled pre-coated ultrafiltration membrane of the present invention is loaded onto the ultrafiltration membrane by double-layer coating. Compared with simultaneous coating, double-layer coating can better intercept small molecule products generated by photocatalysis; compared with single coating of carbon-based materials, double-layer coating improves the removal effect of difficult-to-degrade substances; compared with single coating of BT oxide materials, double-layer coating reduces the risk of leakage of small molecule products generated by photocatalysis. Inserting the carbon-based material layer between the photocatalyst BT and the membrane surface can intercept the byproducts brought about by photocatalytic degradation on the one hand, and reduce the membrane degradation caused by photocatalysis on the other hand, thereby improving the anti-pollution ability of the membrane.
[0059] Inserting a carbon-based material layer between the photocatalyst BT and the membrane surface can, on the one hand, intercept the by-products brought about by photocatalytic degradation, and on the other hand, reduce the membrane degradation caused by photocatalysis, thereby improving the membrane's anti-pollution ability.
[0060] The removal rate of tetracycline by the multifunctional coupled pre-coated ultrafiltration membrane of the present invention can reach 92%.
[0061] The present invention also discloses a method for preparing a multifunctional coupled pre-coated ultrafiltration membrane, which can at least be used to prepare the above-mentioned multifunctional coupled pre-coated ultrafiltration membrane. The preparation method comprises the following steps:
[0062] S100: dispersing the load objects in water to obtain load suspensions;
[0063] S200: uniformly coating the load suspension on the surface of the ultrafiltration membrane in sequence to obtain a multifunctional coupled pre-coated ultrafiltration membrane;
[0064] The loading amount of the load is 6-50 g / m 2 ;
[0065] The load includes Bi 2 O 3 / TiO 2 Composite metal oxide and carbon-based material, the carbon-based material, Bi 2 O 3 / TiO 2 The composite metal oxides are sequentially coated on the surface of the ultrafiltration membrane, Bi 2 O 3 / TiO 2 The mass ratio of the composite metal oxide to the carbon-based material is 1:(1~3).
[0066] In S100, the load suspension includes a carbon-based material suspension and Bi 2 O 3 / TiO 2 Composite metal oxide suspension, that is, carbon-based material is dispersed in water to obtain carbon-based material suspension, Bi 2 O 3 / TiO 2 Composite metal oxides dispersed in water to obtain Bi 2 O 3 / TiO 2 Composite metal oxide suspension: The load is placed in water and dispersed by ultrasound (30-50 kHz) to form a load suspension, and the ultrasound duration is 20-40 minutes (preferably 30 minutes).
[0067] The Bi 2 O 3 / TiO 2 The composite metal oxide is prepared by a sol-impregnation-hydrothermal calcination method. Specifically, the Bi 2 O 3 / TiO 2 The preparation method of the composite metal oxide comprises the following steps:
[0068] S101: slowly pouring a titanium precursor compound into glacial acetic acid, and then pouring the mixture into anhydrous ethanol, stirring to obtain liquid A, wherein the volume ratio of the titanium precursor compound, glacial acetic acid and anhydrous ethanol is (2-3):1:(6-9) (preferably 2:1:8);
[0069] The precursor compound of bismuth is dissolved in water to obtain liquid B, and the molar concentration of bismuth is 0.02-0.04 mol / L, that is, the concentration of bismuth element in the liquid B obtained by dissolving the precursor compound of bismuth in water is 0.02-0.04 mol / L;
[0070] S102: Mix liquid A and liquid B in a volume ratio of 1: (0.9-1.5), perform a hydrothermal reaction, separate the product obtained by the hydrothermal reaction from the reaction solution, dry it, and calcine it to obtain Bi 2 O 3 / TiO 2 Composite metal oxides.
[0071] In step S101, the precursor compound of titanium is tetrabutyl titanate, the precursor compound of bismuth is bismuth nitrate pentahydrate, and the molar ratio of Bi in the bismuth precursor compound to Ti in the titanium precursor compound is 0.04-0.10. Exemplarily, every 0.5-1 g of bismuth nitrate pentahydrate corresponds to about 50 mL of water to obtain liquid B.
[0072] The glacial acetic acid refers to acetic acid with a very high purity of more than 99.5%, that is, pure anhydrous acetic acid.
[0073] The stirring of liquid A is performed by stirring with a magnetic stirrer at room temperature, the room temperature is 25±5°C, the stirring speed is 300-400 rpm, and the stirring time is 100-150 min. For example, 10 mL of tetrabutyl titanate is slowly poured into 5 mL of glacial acetic acid, and then the mixture is simultaneously poured into 40 mL of anhydrous ethanol, and stirred at room temperature with a magnetic stirrer at 350 rpm for 120 min to obtain liquid A.
[0074] In the process of obtaining liquid B, the bismuth precursor compound is dissolved in deionized water under the action of ultrasound, and then stirred with a magnetic stirrer at room temperature to obtain liquid B. Specifically, the bismuth precursor compound is dissolved under ultrasound (30-50 kHz) for 20-40 min, and then stirred with a magnetic stirrer at 100-150 rpm at room temperature for 100-150 min to obtain liquid B. For example, 556 mg of Bi(NO 3 ) 3 ·5H 2 Solution O was dissolved in 50 mL of deionized water and dissolved under 40 kHz ultrasound for 30 min, and then stirred at 120 rpm for 120 min at room temperature using a magnetic stirrer to obtain solution B.
[0075] In step S102, preferably, the liquid B is dropped into the liquid A to obtain the liquid C, the liquid C is stirred at room temperature with a magnetic stirrer (stirring speed is 300-400 rpm, stirring time is 7-9 hours) into a sol, and then the sol is transferred to a stainless steel autoclave reactor to perform a hydrothermal reaction, the reaction temperature of the hydrothermal reaction is 150-180°C, and the reaction time is 10-14 hours.
[0076] The separation is carried out by ultrafiltration membrane filtration or centrifugal separation, and the filtration condition is 0.1Mpa pressure; the centrifugal separation condition is 3000~5000 rpm, 5~10 min. Drying is carried out in an oven at 120~130℃ for 3~4h. Calcination is carried out in a tubular furnace, the calcination temperature is 300~800℃, and the calcination time is 2~4h.
[0077] For example, solution B was dropped into solution A to prepare solution C, which was stirred at room temperature with a magnetic stirrer at 350 rpm for 8 h. The resulting sol was transferred to a stainless steel autoclave reactor and hydrothermally treated at 150 °C for 12 h. The resulting precipitate was dried at 125 °C (oven), and the composite material was calcined in air at 300 °C (tube furnace) for 2 h to obtain Bi 2 O 3 / TiO 2 Composite metal oxides.
[0078] In step S200, the load is coated sequentially through an ultrafiltration cup filtration system, and the ultrafiltration cup filtration system includes a nitrogen bottle, a pressure controller, an ultrafiltration cup, an electronic balance and a collection system. Coating through the ultrafiltration cup filtration system belongs to the prior art and is not described in detail here. The transmembrane pressure difference during the coating process is constant at 20-30 kPa. The filtration method is dead-end filtration.
[0079] The ultrafiltration membrane needs to be pretreated before coating. Specifically, the pretreatment process is as follows: the ultrafiltration membrane is first soaked in a 50% to 70% ethanol solution for 15 to 30 minutes, and then soaked in deionized water for 24 to 30 hours to completely remove the preservatives and impurities on the surface.
[0080] The present invention also discloses an application method of a multifunctional coupled pre-coated ultrafiltration membrane, including dark treatment and / or light treatment.
[0081] The dark treatment comprises fixing the multifunctional coupled pre-coated ultrafiltration membrane on a membrane reactor containing the liquid to be treated, and performing dark adsorption. Preferably, the dark adsorption time is 20 to 40 minutes.
[0082] The light treatment includes fixing the multifunctional coupled pre-coated ultrafiltration membrane on a membrane reactor containing the liquid to be treated, and irradiating the multifunctional coupled pre-coated ultrafiltration membrane with ultraviolet light for photocatalytic oxidation. The wavelength of the ultraviolet light is 280-400nm, and the light power density is 200-400mW / cm 2 .
[0083] The filter membrane in the membrane reactor is a flat membrane. The flow rate of the membrane reactor is controlled at 100-250 mL / min by a pressure controller.
[0084] The dark treatment conditions are darkness, light shielding, and room temperature (20±5° C.).
[0085] Specifically, the application method includes the following three application modes:
[0086] 1) Only dark treatment is performed, that is, the multifunctional coupled pre-coated ultrafiltration membrane is applied under dark conditions. For example, when the organic matter content of the influent is low (DOC < 2 mg / L), the dark filtration method can be used preferentially. Keep the UV light off and the filtration is operated under dark conditions, mainly using Bi 2 O 3 / TiO 2 The adsorption function of composite metal oxides and carbon-based materials and the retention function of ultrafiltration membranes achieve organic matter removal and reduce irreversible contamination on the surface of ultrafiltration membranes through pre-adsorption; when the membrane flux drops below 20% of the initial flux, backwashing is performed.
[0087] 2) Only light treatment is performed, that is, the multifunctional coupled pre-coated ultrafiltration membrane is applied under light conditions. For example, when the organic matter content of the influent is high (DOC>3 mg / L), light filtration method can be used preferentially. Turn on the ultraviolet light and filter under light conditions, mainly using Bi-based 2 O 3 / TiO 2 The coupling functions of composite metal oxide photocatalysis, carbon-based material adsorption and ultrafiltration membrane retention realize the removal of organic matter, and mitigate the reversible and irreversible pollution on the surface of the ultrafiltration membrane through the dynamic coupling of photocatalysis and adsorption functions; when the membrane flux drops to less than 20% of the initial flux, backwashing is carried out.
[0088] 3) Dark treatment and light treatment are carried out alternately, that is, the multifunctional coupled pre-coated ultrafiltration membrane is first applied under the conditions of darkness (10~30 min) and light (10~30 min) alternately; for example, when the influent DOC content is in the range of 2~3 mg / L, the dark and light alternating filtration method can be used preferentially. First, keep the UV light off and let the filtration run under dark conditions for 10~30min; when the membrane flux drops to less than 20% of the initial flux, turn on the UV light filtration and run under light conditions, using Bi 2 O 3 / TiO 2 The photocatalytic function of the composite metal oxide degrades the organic matter adsorbed by the carbon-based material and retained by the membrane pores, playing an in-situ light cleaning role; when the membrane flux recovers to more than 80% of the initial flux or after running for 30 minutes, turn off the UV lamp; when the membrane flux recovers to more than 80% of the initial flux or after running for 30 minutes, turn off the UV lamp; repeat this cycle so that the filtration operates under alternating dark and light conditions; after running under light conditions for 30 minutes, the membrane flux is still lower than 20% of the initial flux, and backwashing is performed.
[0089] Backwashing conditions: Use deionized water to hydraulically backwash the contaminated ultrafiltration membrane at a transmembrane pressure difference of 0.08~0.10 MPa, and the backwashing time is 3~5 min.
[0090] [Example] A method for preparing a multifunctional coupled pre-coated ultrafiltration membrane comprises the following steps:
[0091] S100: 11 mg of powdered activated carbon (PAC) and 11 mg of Bi 2 O 3 / TiO 2 The composite metal oxides were dispersed in deionized water and dispersed by ultrasound (40kHz) for 30 min to obtain activated carbon suspension and Bi 2 O 3 / TiO 2 Composite metal oxide suspension;
[0092] S200: Activated carbon suspension and Bi 2 O 3 / TiO 2 The composite metal oxide suspension is uniformly coated on the surface of the PVDF ultrafiltration membrane (UF) through the ultrafiltration cup filtration system in turn to obtain a multifunctional coupled pre-coated ultrafiltration membrane, denoted as BT / PAC-UF (indicated by Ⅰ in the accompanying drawings of the specification), wherein the loading amount of the load is 6 g / m 2 ,Bi 2 O 3 / TiO 2The mass ratio of composite metal oxide to PAC is 1:1;
[0093] Among them, the Bi 2 O 3 / TiO 2 The preparation method of the composite metal oxide comprises the following steps:
[0094] S101: Slowly pour 10 mL of tetrabutyl titanate into 5 mL of glacial acetic acid, and then pour the mixture into 40 mL of anhydrous ethanol at the same time, and stir with a magnetic stirrer at 350 rpm for 120 min at room temperature to obtain liquid A;
[0095] 556 mg of Bi(NO 3 ) 3 •5H 2 O was dissolved in 50 mL of deionized water and dissolved under 40 kHz ultrasound for 30 min, and then stirred at 120 rpm for 120 min at room temperature using a magnetic stirrer to obtain solution B;
[0096] S102: Liquid B was dropped into liquid A to obtain liquid C. Liquid C was stirred at room temperature with a magnetic stirrer at 350 rpm for 8 h. The obtained sol was transferred to a stainless steel autoclave reactor and hydrothermally treated at 150°C for 12 h. The precipitate obtained by the hydrothermal reaction was dried in an oven at 125°C, taken out and ground into powder. The powder was placed in a tubular furnace and calcined at 300°C in air atmosphere for 2 h to obtain Bi 2 O 3 / TiO 2 Composite metal oxide powder.
[0097] The above-mentioned carbon-based materials are replaced with mesoporous carbon (CMK-3) and carbon nanotubes (CNTs), and the other conditions remain unchanged. The prepared multifunctional coupled pre-coated ultrafiltration membranes are respectively denoted as BT / CMK-3-UF (indicated by Ⅱ in the accompanying drawings of the specification) and BT / CNTs-UF (indicated by Ⅲ in the accompanying drawings of the specification).
[0098] Figure 1 Fourier infrared spectra of BT / PAC-UF, BT / CMK-3-UF, BT / CNTs-UF, and UF (ultrafiltration membrane alone as a control) prepared in the above examples after filtering actual surface water under dark and light conditions. Figure 1 It can be seen that the membrane surface is at 1655cm -1 , 1400cm -1 , 1180 cm -1 , 1070cm -1 , 837cm -1 ~877cm -1There are obvious adsorption peaks at 1655cm -1 and 1076 cm -1 The peak at 1400 cm is mainly caused by the vibration contraction of the carboxyl group, revealing the deposition of carbohydrates on the membrane; -1 The peak at 837 is mainly the polysaccharide peak on the membrane surface; -1 ~877cm -1 The peak can be attributed to the aromatic peak, which indicates that the humic acid substance is attached to the membrane surface. Compared with UF (indicated by Ⅳ in the attached figure of the specification), each coating membrane has a peak at the same wavelength, but the peak value is significantly reduced, indicating that the deposits on the membrane surface are reduced and the membrane pollution is effectively alleviated.
[0099] Figure 2 The scanning electron microscope images of UF, BT / PAC-UF, BT / CMK-3-UF, and BT / CNTs-UF, where a~c are the original UF and the UF after filtering actual surface water under dark and light conditions, d~f are the BT / PAC-UF, BT / CMK-3-UF, and BT / CNTs-UF after filtering actual surface water under dark conditions, and g~i are the BT / PAC-UF, BT / CMK-3-UF, and BT / CNTs-UF after filtering actual surface water under light conditions. Figure 2 It can be seen that compared with the unfiltered UF (a), the surface of the filtered UF accumulates dirt, forming a cake layer, and the clogging phenomenon is serious. Under dark conditions (d~f), after filtering surface water, a large number of aggregates gathered on the coating on the surface of the membrane of the three coated membranes, indicating that the presence of the coating can prevent pollutants from directly contacting the membrane surface. Under light conditions (g~i), the aggregates on the coating on the membrane surface are significantly reduced. This is because BT has excellent photocatalytic properties and decomposes and removes large molecular weight substances. In general, the presence of the coating can adsorb large molecular substances, and the pollutants deposited on the membrane surface can be further removed by light, thereby effectively alleviating membrane pollution.
[0100] Figure 3 The contact angles of UF, BT / PAC-UF, BT / CMK-3-UF, and BT / CNTs-UF after filtering actual surface water under dark and light conditions are shown in the figure as the average of the measured values at three different locations on the membrane surface. Figure 3It can be seen that under dark conditions, the contact angle of UF is 96.5°, indicating that the membrane surface is covered with hydrophobic pollutants, while the contact angles of BT / PAC-UF, BT / CMK-3-UF and BT / CNTs-UF are 52.7°, 54.1° and 52.8° respectively. This is because BT material is a hydrophilic material, and BT attached to the membrane surface will reduce the contact angle of the membrane. Under light conditions, the contact angles of the three coated films are reduced to 50.3°, 43.6° and 51.4°, which indicates that the photocatalyst BT and carbon-based materials can effectively oxidize and adsorb hydrophobic substances on the membrane surface, thereby reducing membrane pollution.
[0101] The decontamination effects of BT / PAC-UF, BT / CMK-3-UF, and BT / CNTs-UF obtained in the above examples were tested. Specifically, actual surface water was used as the inlet water of the membrane reactor, and the multifunctional coupled pre-coated ultrafiltration membrane was fixed in the membrane reactor. First, dark adsorption was performed for 30 min under dark conditions at room temperature of 25°C; then, ultraviolet light was irradiated at an optical power density of 400 mW / cm 2 The photocatalytic oxidation was carried out for 2 h.
[0102] Figure 4 and Figure 5 The BT / PAC-UF, BT / CMK-3-UF, and BT / CNTs-UF prepared for the example were subjected to UV light in the dark and under light conditions. 254 The removal effect of UV and DOC is compared with that of UF. 254 The removal rate of BT / PAC-UF, BT / CMK-3-UF and BT / CNTs-UF was only 22.5%, while the removal rates of BT / PAC-UF, BT / CMK-3-UF and BT / CNTs-UF were 32.6%, 40.0% and 36.3% respectively. Under light conditions, the three pre-coated ultrafiltration membranes BT / PAC-UF, BT / CMK-3-UF and BT / CNTs-UF had a significant effect on UV 254 The removal rates of DOC increased to 47.0%, 55.2% and 51.2%. The removal pattern of DOC was similar to that of UV254. The removal rates of DOC by the three photocatalytic membranes increased from 45.6%, 72.7%, 59% to 66.1%, 77.9% and 70.8%.
[0103] Figure 6 and Figure 7The removal effect diagram of BT / PAC-UF, BT / CMK-3-UF, and BT / CNTs-UF for different molecular weight organic matter under dark and light conditions is shown in the figure, and compared with UF. It can be seen from the figure that under dark conditions, UF has limited removal of humic acid, humic acid conjugates, low molecular weight acids and low molecular weight neutrals, with removal rates of 10.7%, 5.9%, 28.7% and 69.1% respectively. Compared with UF, BT / PAC-UF, BT / CMK-3-UF, and BT / CNTs-UF have further removed different molecular organic matter, among which BT / CMK-3-UF has the most obvious treatment effect, and the removal rates of humic acid, humic acid conjugates, low molecular weight acids and low molecular weight neutrals are increased by 7.6%, 10.1%, 5.2% and 20.6% respectively. Under light conditions, the removal rate of UF for organic matter of different molecular weights was not significantly different from that under dark conditions. The removal rate of humic acid by BT / CMK-3-UF increased to 24.1%, and the removal rate of humic acid complexes increased to 17.8%. The removal rates of low molecular weight neutrals by BT / PAC-UF, BT / CMK-3-UF, and BT / CNTs-UF were further improved, reaching 83.9%, 93.7%, and 86.4%, respectively.
[0104] Figure 8 Schematic diagram of membrane flux change of ultrafiltration membrane (UF) and pre-coated ultrafiltration membrane (BT / PAC-UF) under the filtration condition of transmembrane pressure difference of 0.1 ± 0.01 MPa. Figure 8 It can be seen that the J / J0 of BT / PAC-UF decreased by 0.65, 0.19 and 0.13 in the 1st, 2nd and 3rd cycles respectively. The flux decreased more significantly in the first cycle, which was due to the formation of a dense cake layer on the membrane surface and the relative stability of the flux. In addition, the J / J0 of BT / PAC-UF decreased to 0.35 at the end of the first filtration cycle, which was 0.07 higher than the J / J0 of UF (0.28), indicating that the UF flux decreased seriously, and BT / PAC-UF effectively alleviated the decline in membrane flux. In addition, after the saturated self-cleaning treatment in the first filtration cycle, the J / J0 of UF and BT / PAC-UF increased to 0.35 and 0.44, respectively, and increased to 0.26 and 0.31, respectively, after the saturated self-cleaning treatment in the second filtration cycle. The J / J0 of BT / PAC-UF was always higher than that of the original ultrafiltration membrane, indicating that the light cleaning effect alleviated the membrane fouling of BT / PAC-UF and effectively extended the service life of the ultrafiltration membrane.
[0105] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A multifunctional coupled pre-coated ultrafiltration membrane, characterized in that: Capable of removing pollutants from water, the multifunctional coupled pre-coated ultrafiltration membrane comprises: Ultrafiltration membrane; The load is coated on the ultrafiltration membrane, and the load amount of the load is 6-50g / m 2 ; The load includes Bi2O3 / TiO2 composite metal oxide and carbon-based material, and the carbon-based material and Bi2O3 / TiO2 composite metal oxide are sequentially coated on the surface of the ultrafiltration membrane, and the mass ratio of Bi2O3 / TiO2 composite metal oxide to carbon-based material is 1: (1~3).
2. The multifunctional coupled pre-coated ultrafiltration membrane according to claim 1, characterized in that: The material of the ultrafiltration membrane is one of polyvinylidene fluoride, polyether sulfone, polytetrafluoroethylene and polyamide.
3. The multifunctional coupled pre-coated ultrafiltration membrane according to claim 1, characterized in that: The molar ratio of Bi to Ti in the Bi2O3 / TiO2 composite metal oxide is 0.04-0.
10.
4. The multifunctional coupled pre-coated ultrafiltration membrane according to claim 1, characterized in that: The carbon-based material is one or more of activated carbon, mesoporous carbon and carbon nanotubes.
5. A method for preparing a multifunctional coupled pre-coated ultrafiltration membrane, characterized in that: At least it can be used to prepare the multifunctional coupled pre-coated ultrafiltration membrane as claimed in any one of claims 1 to 4, and the preparation method comprises the following steps: S100: dispersing the load objects in water to obtain load suspensions; S200: uniformly coating the load suspension on the surface of the ultrafiltration membrane in sequence to obtain a multifunctional coupled pre-coated ultrafiltration membrane; The loading amount of the load is 6-50 g / m 2 ; The load includes Bi2O3 / TiO2 composite metal oxide and carbon-based material. The carbon-based material and Bi2O3 / TiO2 composite metal oxide are sequentially coated on the surface of the ultrafiltration membrane. The mass ratio of Bi2O3 / TiO2 composite metal oxide to carbon-based material is 1:(1-3).
6. The preparation method according to claim 5, characterized in that: In step S100, the load is placed in water and dispersed by ultrasound, wherein the frequency of the ultrasound is 30-50 kHz and the duration of the ultrasound is 20-40 min.
7. The preparation method according to claim 5, characterized in that: The preparation method of the Bi2O3 / TiO2 composite metal oxide comprises the following steps: S101: slowly pouring a titanium precursor compound into glacial acetic acid, and then pouring the mixture into anhydrous ethanol, stirring to obtain liquid A, wherein the volume ratio of the titanium precursor compound, glacial acetic acid and anhydrous ethanol is 2:1:8; The precursor compound of bismuth is dissolved in water to obtain liquid B, and the molar concentration of bismuth is 0.02~0.04mol / L; S102: Liquid A and liquid B are mixed in a volume ratio of 1: (0.9-1.5), and a hydrothermal reaction is performed. The product obtained by the hydrothermal reaction is separated from the reaction liquid, dried, and calcined to obtain a Bi2O3 / TiO2 composite metal oxide.
8. The preparation method according to claim 5, characterized in that: In step S200, the ultrafiltration membrane is pretreated before being coated. The pretreatment process is as follows: the ultrafiltration membrane is first soaked in a 50% to 70% ethanol solution for 15 to 30 minutes, and then soaked in deionized water for 24 to 30 hours.
9. The preparation method according to claim 5, characterized in that: In step S200, the transmembrane pressure difference during the coating process of the load is constant at 20-30 kPa.
10. A method for applying a multifunctional coupled pre-coated ultrafiltration membrane, characterized in that: At least capable of being applied to the multifunctional coupled pre-coated ultrafiltration membrane as claimed in any one of claims 1 to 4, including dark treatment and / or light treatment; The dark treatment is to fix the multifunctional coupled pre-coated ultrafiltration membrane on a membrane reactor containing the liquid to be treated to perform dark adsorption; The light treatment is to fix the multifunctional coupled pre-coated ultrafiltration membrane on a membrane reactor containing the liquid to be treated, and use ultraviolet light to irradiate the multifunctional coupled pre-coated ultrafiltration membrane for photocatalytic oxidation; When the DOC content in the liquid to be treated is < 2 mg / L, dark treatment is used; When the DOC content in the liquid to be treated is > 3 mg / L, light treatment is used; When the DOC content in the treated liquid is in the range of 2 to 3 mg / L, dark treatment and light treatment are performed alternately.
Citation Information
Patent Citations
Method for relieving pollution to ultrafiltration membrane under joint action of pre-oxidation and membrane modification
CN104230056A
Silver-loaded active carbon / titanium dioxide coupling and ultrafiltration combination apparatus, and method for controlling organic matters and pathogenic microorganisms in water
CN104773868A