Graphene oxide layered film as well as preparation method and application thereof

Through the preparation of modified graphene oxide layered membranes, the problem of difficult adsorbent selection and preparation in the selective separation of rare earth ions is solved, efficient, economical and environmentally friendly extraction of rare earth elements is achieved, and the selective separation of rare earth elements is improved. performance and extraction efficiency.

CN118790986AActive Publication Date: 2024-10-18ZHENGZHOU UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410905201.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-18
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

Existing technologies face difficult adsorbent selection and preparation, limited adsorption capacity and rate, regeneration and life issues, high operation and maintenance costs, economic and sustainability challenges in the selective separation of rare earth ions, resulting in rare earth element extraction efficiency Low and high cost.

Method used

The graphene oxide layered membrane was prepared by ultrasonic treatment of GO nanosheets in water and then modified by adding propylenediamine, sodium hydroxide and amino acids, and the graphene oxide layered membrane was prepared by vacuum filtration. For dynamic adsorption of rare earth metal scandium ions.

Benefits of technology

It achieves efficient adsorption of low-concentration scandium ions in water. The process is simple to operate, has mild conditions, is highly selective and environmentally friendly, and improves the selective separation performance and extraction efficiency of rare earth elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118790986A_ABST
    Figure CN118790986A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of layered membranes, and discloses a graphene oxide layered membrane and a preparation method and application thereof.The preparation method comprises the following steps that GO nanosheets are evenly dispersed in water, then propylene diamine is added, and a GO suspension is obtained; heating and then cooling the GO suspension, adding sodium hydroxide and amino acid, stirring, carrying out solid-liquid separation to obtain a precipitate, and cleaning the precipitate to obtain a modified nanosheet; and preparing the graphene oxide layered film from the modified nanosheet through a vacuum filtration method. The method can efficiently adsorb scandium ions with lower concentration in water, and the whole adsorption process has the advantages of simplicity and convenience in operation, mild conditions, high selectivity, environmental friendliness and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of layered film preparation, and in particular to a graphene oxide layered film and a preparation method and application thereof. Background Art

[0002] Scandium and its compounds have become indispensable elements in the development of science and technology due to their excellent physical and chemical properties in aerospace, transportation, nuclear energy industry, fuel cells and as efficient catalysts. These high-end application fields have extremely high requirements for material performance. The introduction of scandium can greatly improve the temperature resistance, corrosion resistance and structural strength of the material, and promote technological innovation. The unique role of scandium is also reflected in environmental governance and energy conversion efficiency improvement, showing its broad application potential. The rapid development of these fields has promoted the continuous growth of demand for Sc(III). However, the current process of extracting scandium faces technical challenges and complexities, which not only makes the extraction cost of scandium high, but also leads to a situation of supply exceeding demand in the market. Although solvent extraction technology is widely recognized for its high production efficiency, excellent separation performance and fast mass transfer rate, its adverse impact on the environment cannot be ignored.

[0003] Thapa et al. prepared a new hybrid adsorbent BP-TCPSi by functionalizing bisphosphonate and grafting it on the surface of thermally carbonized mesoporous silicon. The separation factor of this material for Sc(III) is 13, which is three times that of the commercial ion exchange resin Dowex50WX8, showing significant selectivity. In addition, BP-TCPSi has high stability and still has good performance after 50 cycles of adsorption and desorption experiments; Zhong et al. synthesized a series of adsorbents with different functional extractants and carriers by vacuum impregnation method, among which trialkylphosphine oxide silicon-modified TRPO / SiO2-P showed excellent selective adsorption, and in the adsorption column experiment, the adsorption efficiency of Sc(III) reached 99.3%, and the characterization and DFT analysis showed that the P=O group was crucial for selective separation. These researchers provided certain references and theoretical basis for the research of adsorption materials, but there are still problems such as difficult material preparation, complex process, low success rate and high cost, which restrict the application of adsorption method in industry.

[0004] Membrane adsorbents are a promising solid phase technology in the field of adsorption. Membrane adsorbents consist of a microporous substrate coated with a micrometer or even nanometer-scale separation layer containing binding sites for molecules or ions. The selectivity of membrane adsorbents can be adjusted by changing the chemical properties of the membrane. Therefore, membrane adsorbent materials can replace traditional ion exchange resins, achieving the high throughput of nanofiltration membranes and the selectivity of ion exchange resins.

[0005] Membrane adsorption separation has become an ideal choice for water treatment systems due to its process structure, which has the advantages of no phase change, low energy consumption, environmental friendliness, simple operation, high separation efficiency and mild operating conditions. However, achieving selective separation of rare earth ions at the sub-nanometer scale has always been a huge challenge faced by traditional membrane separation technology. The emergence of layered membranes has made up for this deficiency and provided a good idea for the selective separation of a single type of ions in a mixed system. However, the existing technology faces many practical technical problems in practical applications, including high difficulty in adsorbent selection and preparation, limited adsorption capacity and rate, regeneration and life problems, difficulty in selective adsorption, high operation and maintenance costs, economic and sustainability challenges, and specific problems in the application field. These problems jointly affect the efficiency, cost and sustainable development of adsorption technology, and need to be solved through efforts in many aspects such as material optimization, regeneration technology improvement, system design innovation and economic improvement.

[0006] Therefore, there is an urgent need to develop a graphene oxide layered film with high efficiency and high stability and its preparation method and application to solve the above technical problems. Summary of the invention

[0007] The present invention aims to solve the existing technical problems and provide a graphene oxide layered film and a preparation method and application thereof.

[0008] To achieve the above object, the present invention is implemented according to the following technical solutions:

[0009] A method for preparing a graphene oxide layered film comprises the following steps:

[0010] S1, GO nanosheets are uniformly dispersed in water and then propylene diamine is added to obtain a GO suspension;

[0011] S2, the GO suspension is heated and then cooled, sodium hydroxide and amino acid are added and stirred, and then solid-liquid separation is performed to obtain a precipitate, and the precipitate is washed to obtain the modified nanosheets;

[0012] S3, preparing a graphene oxide layered membrane by vacuum filtration method using the modified nanosheets.

[0013] Specifically, the following steps are included:

[0014] S1, GO nanosheets are subjected to ultrasonic treatment in water to be uniformly dispersed, and propylene diamine is added and mixed to obtain a GO suspension;

[0015] S2, heating the GO suspension, adding a small amount of sodium hydroxide and phosphoserine and stirring at room temperature after cooling, centrifuging the resulting precipitate and washing and drying to obtain modified nanosheets;

[0016] S3, finally taking an appropriate amount of modified nanosheets to prepare a graphene oxide layered membrane through a vacuum filtration method.

[0017] Preferably, in step S1, the concentration of GO nanosheets in the GO suspension is 0.4 g L -1 .

[0018] Specifically, the GO suspension refers to a mixed solution of GO nanosheets, water, and propylenediamine; since the amount of propylenediamine added is small, the volume of propylenediamine is not calculated in the calculation process of the concentration of the GO suspension here.

[0019] Preferably, in step S1, the ratio of GO suspension to propylenediamine is 50:0.1, and the comparison unit is ml:mol.

[0020] Preferably, in step S2, the heating temperature of the GO suspension is 60-100° C., and the heating time is 1-3 h.

[0021] Preferably, in step S2, the ratio of GO suspension, sodium hydroxide and amino acid is 50:0.0015:0.1, and the comparison unit is ml:mol:mol; and the stirring time is 24h.

[0022] Specifically, since the amount of propylene diamine added is relatively small, the volume of propylene diamine is not calculated in the above data related to the volume of the GO suspension.

[0023] Preferably, in step S2, the amino acid is one of lysine, glutamic acid and phosphoserine.

[0024] Preferably, in step S3, the modified nanosheets are filtered in the form of an aqueous solution; the concentration of the aqueous solution of the modified nanosheets is 0.4 g L -1 .

[0025] Preferably, in step S3, the vacuum filtration pressure is -0.1 MPa and the time is 12 h.

[0026] Preferably, in step S3, the thickness of the obtained graphene oxide layered film is 1 μm.

[0027] The present invention also includes a graphene oxide layered film prepared by the above method.

[0028] An application of a graphene oxide layered film, wherein the graphene oxide layered film is used for adsorbing rare earth metal scandium.

[0029] Preferably, the graphene oxide layered film is used as an adsorbent to selectively adsorb scandium ions in the liquid;

[0030] The adsorption method is dynamic adsorption: the modified graphene oxide layered membrane is placed in a membrane pool, and the graphene oxide layered membrane is used to adsorb scandium ions in the liquid in a pressure-driven manner.

[0031] Specifically, the following steps are included:

[0032] The graphene oxide layered film acts as an adsorbent to selectively adsorb scandium ions in water;

[0033] The adsorption method is dynamic adsorption: the graphene oxide layered membrane is placed in a membrane pool, the pH of a certain concentration of scandium ion-containing aqueous solution is adjusted to 5, and the scandium ions in the water are adsorbed by the layered membrane through a dead-end device pressure-driven method. Specifically, in the above-mentioned certain concentration of scandium ion-containing aqueous solution, the concentration of scandium ions is 10ppm. The graphene oxide layered membrane can also be directly placed in the scandium ion-containing aqueous solution for direct adsorption.

[0034] Working principle:

[0035] The present invention places a modified graphene oxide layered membrane in a membrane pool, prepares a certain concentration of an aqueous solution containing scandium ions and adjusts the pH to 5, and uses the layered membrane to adsorb the scandium ions in the water by a dead-end device pressure-driven method. The preparation method of the modified graphene oxide layered membrane of the present invention is: ultrasonically treat GO nanosheets in water to make them uniformly dispersed, add propylene diamine and mix, heat the suspension, add a small amount of sodium hydroxide and phosphoserine and stir at room temperature after cooling, centrifuge and wash the obtained precipitate, and finally take an appropriate amount of modified nanosheets and prepare the layered membrane by vacuum filtration.

[0036] As an important graphene derivative, GO is essentially a single layer of graphene oxide, which introduces a large number of oxygen-containing functional groups, which can serve as reaction sites for chemical reactions and as adsorption sites for metal ions.

[0037] The epoxy groups on the surface of the GO membrane react easily with alcohols, amines or alcohol salts, so that binding groups can be easily added. Through this functionalization strategy, amino acids, peptides and proteins can be fixed to achieve modification of the GO membrane surface. Amino acids, peptides and proteins are highly potential ligands for the adsorption of rare earth elements. Peptides with customized amino acid sequences and secondary structures can produce various functions and highly specific binding capabilities.

[0038] Layered membranes have the characteristics of nano-confinement, long-range confinement and easy modification. When the feed liquid passes through the membrane material, the unique interlayer channel structure of the layered membrane can remove hydrated ions through size screening at the nanoscale, so that the metal ions are exposed in the long-range channel as naked ions, increasing the contact probability and contact time with the active sites. In addition, by modifying the membrane surface and grafting specific functional groups to improve the channel microenvironment, the adsorption performance can be further improved and rapid selective separation can be achieved. By adjusting the interlayer spacing, surface functionalization and structural customization of the membrane, the membrane's recognition and separation performance for specific ions can be further enhanced, providing efficient separation solutions for the fields of fine chemicals, resource recovery and environmental governance.

[0039] The layered membrane has the characteristics of nano-confinement, long-range confinement and easy modification. When the feed liquid passes through the membrane material, the unique interlayer channel structure of the layered membrane can remove hydrated ions through size screening at the nanoscale, so that the metal ions are exposed in the long-range channel as naked ions, increasing the contact probability and contact time with the active sites. In addition, by modifying the membrane surface and grafting specific functional groups to improve the channel microenvironment, the adsorption performance can be further improved and rapid selective separation can be achieved. The layered membrane shows great potential for metal ion adsorption in terms of physical structure and chemical adsorption. The present invention deeply studies the channel structure of the layered membrane and its mass transfer behavior and adsorption mechanism for metal ions, as well as how to design and optimize the function of the layered membrane based on these mechanisms, which is of key significance for improving the selective capture and separation of specific metal ions. By adjusting the interlayer spacing, surface functionalization and structural customization of the membrane, the recognition and separation performance of the membrane for specific ions can be further enhanced, providing efficient separation solutions for the fields of fine chemicals, resource recovery and environmental governance.

[0040] The present invention successfully prepared a modified graphene oxide layered membrane by using inorganic small molecule diamine and organic small molecule amino acid to precisely control the interlayer spacing and the introduction of adsorption sites. The layered membrane exhibited excellent performance in the selective adsorption and separation of scandium, providing a feasible new strategy for the efficient extraction of rare earth elements.

[0041] Beneficial effects:

[0042] The present invention can efficiently adsorb scandium ions with low concentration in water, and the entire adsorption process has the advantages of simple operation, mild conditions, high selectivity and environmental friendliness. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is a process flow chart of Example 1 of the present invention;

[0044] Figure 2 Performance diagrams of different layered films obtained from the embodiments of the present invention and the comparative examples;

[0045] Figure 3 XRD images of the graphene oxide layered films obtained in Examples 1 to 3 of the present invention and the GO layered film obtained in Comparative Example 1 in a dry state;

[0046] Figure 4 XRD images of the graphene oxide layered film obtained in Example 1 of the present invention and the GO layered film obtained in Comparative Example 1 in a dry state;

[0047] Figure 5 This is a dynamic performance diagram of the graphene oxide layered film prepared in Example 1 of the present invention in adsorbing scandium ions in water. DETAILED DESCRIPTION

[0048] The present invention is further described below with reference to specific embodiments. The illustrative embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.

[0049] All raw materials of the present invention have no particular limitation on their sources, and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.

[0050] There is no particular limitation on the purity of all raw materials in the present invention. The present invention preferably uses industrial purity or conventional purity used in the art.

[0051] The devices used in the present invention are not particularly limited and can be any of the commonly used devices in the art.

[0052] Example 1

[0053] A method for preparing a graphene oxide layered film:

[0054] S1, GO nanosheets were evenly dispersed in water by ultrasonic treatment to obtain 50 ml of 0.4 g L -1 0.1 mol of propylene diamine was added to the aqueous solution of GO nanosheets to obtain a GO suspension; the concentration of GO nanosheets in the GO suspension was 0.4 g L -1 (The volume of propylene diamine is not included in the concentration calculation); the ratio of GO suspension to propylene diamine is 50:0.1, and the comparison unit is ml:mol.

[0055] S2, heating the GO suspension, adding sodium hydroxide and amino acid after cooling and stirring at room temperature, centrifuging the obtained precipitate and washing and drying to obtain modified nanosheets; the heating temperature of the GO suspension is 80°C, and the heating time is 1 h; the ratio of GO suspension (the volume of propylenediamine is not included in the volume calculation), sodium hydroxide, and amino acid is 50:0.0015:0.1, and the comparison unit is ml:mol:mol; the stirring time is 24 h.

[0056] S3, mixing the modified nanosheets obtained in step S2 with water to obtain a concentration of 0.4 g L -1 of modified nanosheet solution; take 5 ml of 0.4 g L -1 The modified nanosheet solution was used to prepare a graphene oxide layered film by vacuum filtration. The obtained graphene oxide layered film had a thickness of 1 μm and an area of ​​12.56 cm 2 ; The vacuum filtration pressure is -0.1MPa and the time is 12h.

[0057] In this embodiment, the amino acid is phosphoserine; the obtained graphene oxide layered film is denoted as GO-PDA@P.

[0058] like Figure 1 As shown, this is a process flow chart of Example 1 of the present invention.

[0059] Example 2

[0060] The difference between this embodiment and embodiment 1 is that the amino acid used is lysine, and the obtained graphene oxide layered film is recorded as GO-PDA@L.

[0061] Example 3

[0062] The difference between this embodiment and embodiment 1 is that the amino acid used is glutamic acid, and the obtained graphene oxide layered film is recorded as GO-PDA@G.

[0063] Example 4

[0064] The difference between this embodiment and embodiment 1 is that the heating time of step S2 is 2 hours, and the obtained layered film is recorded as Pho-2h.

[0065] Example 5

[0066] The difference between this embodiment and embodiment 1 is that the heating time of step S2 is 3 hours, and the obtained layered film is recorded as Pho-3h.

[0067] Example 6

[0068] The difference between this embodiment and embodiment 1 is that the heating temperature in step S2 is 60° C., and the obtained layered film is recorded as Pho-60° C.

[0069] Example 7

[0070] The difference between this embodiment and embodiment 1 is that the heating temperature in step S2 is 100°C, and the obtained layered film is recorded as Pho-100°C.

[0071] Comparative Example 1

[0072] S1, GO nanosheets were uniformly dispersed in water by ultrasonic treatment to obtain a concentration of 0.4 g L -1GO nanosheets aqueous solution.

[0073] S2, take 5ml 0.4g L -1 GO nanosheet aqueous solution, the layered membrane prepared by vacuum filtration is denoted as GO; the vacuum filtration pressure is -0.1MPa, and the time is 12h.

[0074] Comparative Example 2

[0075] S1, GO nanosheets were ultrasonically treated in water to make them uniformly dispersed, and a GO nanosheet aqueous solution was obtained with a concentration of 0.4 g L -1 .

[0076] S2, heat the GO nanosheet aqueous solution of S1, add sodium hydroxide and amino acid after cooling and stir at room temperature, centrifuge the obtained precipitate and wash and dry to obtain modified nanosheets; the heating temperature of the GO nanosheet suspension is 80°C, and the heating time is 1h; the ratio of GO nanosheet aqueous solution, sodium hydroxide and amino acid is 50:0.0015:0.1, and the comparison unit is ml:mol:mol; the stirring time is 24h.

[0077] S3, mixing the modified nanosheets obtained in step S2 with water to obtain a concentration of 0.4 g L -1 5 ml of the modified nanosheet solution was taken and a layered membrane was prepared by vacuum filtration; the vacuum filtration pressure was -0.1 MPa and the time was 12 h.

[0078] In this comparative example, the amino acid is phosphoserine.

[0079] The obtained graphene oxide layered film is recorded as GO-Pho.

[0080] Comparative Example 3

[0081] S1, preparing a GO suspension according to step S1 of Example 1, filtering the GO suspension and drying it to obtain GO-PDA modified nanosheets;

[0082] S2, preparing a modified nanosheet according to steps S1 and S2 of comparative example 2, namely a GO-Pho modified nanosheet;

[0083] S3, mixing the GO-PDA modified nanosheets and GO-Pho modified nanosheets obtained in steps S1 and S2 with water, wherein the mass ratio of the GO-PDA modified nanosheets to the GO-Pho modified nanosheets is 1:1; obtaining a concentration of 0.4 g L -1 5 ml of the mixed modified nanosheet solution was taken and a layered membrane was prepared by vacuum filtration; the vacuum filtration pressure was -0.1 MPa and the time was 12 h.

[0084] The obtained graphene oxide layered film is recorded as GO-PDA / Pho.

[0085] like Figure 2 Shown are performance diagrams of different layered films obtained from the embodiments of the present invention and the comparative examples.

[0086] The graphene oxide layered membranes obtained in the above-mentioned Examples 1 to 3 and the layered membrane obtained in Comparative Example 1 were subjected to adsorption tests using a feed solution; the feed solution used in the test was a scandium single ion solution, in which the scandium ion concentration was 100 ppm and the volume was 100 mL; the test conditions were: at pH = 5, 0.15 g of the layered membrane was placed in 100 mL of the scandium single ion solution, stirred at room temperature for 24 h, and the stirring speed was 130 rpm. The data obtained are as follows Figure 2 As shown in a, the adsorption amount and removal rate of Sc by GO material were greatly improved after the introduction of three different amino acids. Among them, the adsorption amount of GO-PDA@P was 44.64 mg g-1, which was slightly lower than the adsorption amount of GO-PDA@L (48.78 mg g-1). -1 , but the removal efficiency of GO-PDA@P was 99.87%, which was higher than that of GO-PDA@L (99.72%).

[0087] The graphene oxide layered membrane obtained in the above Example 1, and the layered membranes obtained in Comparative Examples 2 and 3 were subjected to adsorption tests using a feed solution. The feed solution used in the test was a scandium-aluminum mixed ion solution. In the scandium-aluminum mixed ion solution, the Sc ion concentration was 100ppm, and the Al ion concentration was 100ppm; the volume of the scandium-aluminum mixed ion solution was 100mL; the test conditions were: at pH = 5, 0.15g of the layered membrane was placed in 100mL of the scandium-aluminum mixed ion solution, stirred at room temperature for 24h, and the stirring speed was 130rpm. The data obtained are as follows Figure 2 As shown in (b), the adsorption capacity and separation factor of GO-PDA@P are greatly improved, which is due to the combined effect of amino and phosphate groups.

[0088] The graphene oxide layered membrane obtained in the above Example 1, and the layered membranes obtained in Examples 4 and 5 were subjected to adsorption tests using a feed solution. The feed solution used in the test was a scandium-aluminum mixed ion solution. In the scandium-aluminum mixed ion solution, the Sc ion concentration was 100ppm, and the Al ion concentration was 100ppm; the volume of the scandium-aluminum mixed ion solution was 100mL; the test conditions were: at pH = 5, 0.15g of the layered membrane was placed in 100mL of the scandium-aluminum mixed ion solution, stirred at room temperature for 24h, and the stirring speed was 130rpm. The data obtained are as follows Figure 2c is the performance diagram of the membrane under different heating times. With the increase of heating time, the adsorption amount and separation factor show a downward trend, and the separation factor is greatly reduced at 3h. This is mainly because the amino acid molecules are inactivated for a long time under high temperature environment, and the coordination effect is not fully exerted in the interlayer channel, which weakens the membrane selectivity.

[0089] The graphene oxide layered membrane obtained in the above Example 1, and the layered membranes obtained in Examples 6 and 7 were subjected to adsorption tests using a feed solution. The feed solution used in the test was a scandium-aluminum mixed ion solution. In the scandium-aluminum mixed ion solution, the Sc ion concentration was 100ppm, and the Al ion concentration was 100ppm; the volume of the scandium-aluminum mixed ion solution was 100mL; the test conditions were: at pH = 5, 0.15g of the layered membrane was placed in 100mL of the scandium-aluminum mixed ion solution, stirred at room temperature for 24h, and the stirring speed was 130rpm. The data obtained are as follows Figure 2 d shows the membrane performance at different temperatures. When the modification temperature is 60°C, the adsorption amount is the highest, but the separation factor is low, which is mainly because the amino acid molecules are not fully grafted. When the modification temperature is 100°C, the adsorption amount and separation factor are the lowest, which is mainly because the grafted amino acid molecules are inactivated at high temperatures, resulting in a decrease in performance.

[0090] like Figure 3 , which are XRD images of the graphene oxide layered film obtained in the embodiment of the present invention and the GO layered film obtained in Comparative Example 1 in a dry state.

[0091] In order to characterize the structural differences between different layered films, the XRD image changes of the graphene oxide layered films obtained in Examples 1 to 3 and the GO layered film obtained in Comparative Example 1 under dry conditions were tested by X-ray diffraction characterization technology, and the interlayer spacing d was calculated by the Bragg equation.

[0092] Depend on Figure 3 , Figure 4It can be seen that the characteristic peak positions of the GO (001) layer of the GO, GO-PDA@G, GO-PDA@P and GO-PDA@L layered membranes are 11.48°, 10.13°, 10.48° and 11.8°, respectively, and the corresponding interlayer spacing d is 0.77nm, 0.88nm, 0.84nm and 0.75nm, respectively. The relative atomic masses of the three different amino acids are lysine, glutamic acid and phosphoserine from small to large, but the actual measured interlayer spacing is inconsistent, mainly because the interlayer spacing of the phosphoserine modified GO membrane is between the other two. This is mainly because the electronegativity of the four oxygen atoms in the phosphate group is strong, and the electrostatic force will make the atoms in the phosphate group more closely arranged together, making the overall scale relatively small. At the same time, there are no other miscellaneous peaks in the XRD image, indicating that the membrane material has a high degree of regularity and still retains the structure of the GO layered membrane, which is conducive to the adsorption of the membrane adsorbent when the metal ions are transferred in the interlayer channel.

[0093] like Figure 5 As shown, it is a dynamic performance diagram of the graphene oxide layered membrane prepared in Example 1 of the present invention in adsorbing scandium ions in water.

[0094] The graphene oxide layered membrane obtained in Example 1 was used as an adsorbent to selectively adsorb scandium ions in water; the adsorption method was dynamic adsorption: the graphene oxide layered membrane was placed in a membrane pool, the pH of an aqueous solution containing scandium ions (the concentration of scandium ions was 10 ppm) was adjusted to 5, and the layered membrane was used to adsorb scandium ions in water by driving with different pressures through a dead-end device. Different feed flow rates were obtained by driving the dead-end device with different pressures, and relevant data were measured under different feed flow rates.

[0095] Depend on Figure 5 It can be seen that the feed flow rate is 50L m -2 h -1 When the C of the breakthrough curve v The rise of / C0 started early, that is, the concentration of Sc(III) in the filtrate increased significantly when the filtration volume was greater than 5 mL. The adsorption capacity of Sc(III) by the membrane in this process was 48.97 mg g -1 , which reflects that the removal of Sc(III) mainly depends on adsorption, while the contribution of size screening is almost non-existent. In addition, the feed flux of 10 L m -2 h -1 and 30L m -2 h -1 The breakthrough curve is slightly different, with a flow rate of 30 L m -2 h -1The breakthrough curve shows that when the membrane treats 30 mL of solution, the permeate concentration just reaches 5% of the initial concentration. Then, as the volume of treated filtrate increases, the breakthrough curve suddenly becomes steeper and finally reaches the value of the feed concentration. When the dynamic adsorption equilibrium is reached, their adsorption amounts are basically the same, both 62.68 mg g -1 This indicates that GO-PDA@P has a high affinity for Sc(III) and can bind to Sc(III) at a flow rate of 30 L m -2 h -1 The adsorption capacity was not affected when the flow rate was 50 L m -2 h -1 The adsorption capacity decreases when the feed liquid flows faster, which is mainly because the fast flow rate of the feed liquid creates a dead zone in the interlayer channel, or the adsorption site is in the topological structure and cannot achieve rapid adsorption. Therefore, the initial flow rate of the feed liquid in the dynamic operation experiment is 30L m -2 h -1 .

[0096] The technical solution of the present invention is not limited to the above-mentioned specific embodiments. All technical variations made according to the technical solution of the present invention fall within the protection scope of the present invention.

Claims

1. A method for preparing a graphene oxide layered film, characterized in that: The following steps are involved: S1, GO nanosheets are uniformly dispersed in water and then propylene diamine is added to obtain a GO suspension; S2, the GO suspension is heated and then cooled, sodium hydroxide and amino acid are added and stirred, and then solid-liquid separation is performed to obtain a precipitate, and the precipitate is washed to obtain the modified nanosheets; S3, preparing a graphene oxide layered membrane by vacuum filtration method using the modified nanosheets.

2. The method for preparing a graphene oxide layered film according to claim 1, characterized in that: In step S1, the concentration of GO nanosheets in the GO suspension is 0.4 g L -1 .

3. The method for preparing a graphene oxide layered film according to claim 2, characterized in that: In the step S1, the ratio of GO suspension to propylenediamine is 50:0.1, and the comparison unit is ml:mol.

4. The method for preparing a graphene oxide layered film according to claim 1, characterized in that: In step S2, the heating temperature of the GO suspension is 60-100° C., and the heating time is 1-3 h.

5. The method for preparing a graphene oxide layered film according to claim 1, characterized in that: In step S2, the ratio of GO suspension, sodium hydroxide and amino acid is 50:0.0015:0.1, and the comparison unit is ml:mol:mol.

6. The method for preparing a graphene oxide layered film according to claim 1, characterized in that: In step S2, the amino acid is one of lysine, glutamic acid and phosphoserine.

7. A graphene oxide layered film prepared by the method according to any one of claims 1 to 6.

8. The use of a graphene oxide layered film according to claim 7, characterized in that: The graphene oxide layered film is used for adsorbing rare earth metal scandium.

9. The use of a graphene oxide layered film according to claim 8, characterized in that: The graphene oxide layered film acts as an adsorbent to selectively adsorb scandium ions in the liquid.

10. The use of a graphene oxide layered film according to claim 9, characterized in that: The adsorption method is dynamic adsorption: the modified graphene oxide layered membrane is placed in a membrane pool, and the graphene oxide layered membrane is used to adsorb scandium ions in the liquid in a pressure-driven manner.

Citation Information

Patent Citations

  • Preparation method of graphene oxide / amino acid composite material with adsorption effect on heavy metal ions

    CN104437390A

  • Method for preparing graphene oxide sponge by utilizing glutathione and application of method

    CN108275679A

  • Application of amino acid modified graphene oxide in water-base drilling fluid as coating agent

    CN110373165A

  • Amino acid-metal complex bonded graphene oxide composite ultrafiltration membrane and preparation method thereof

    CN111841341A

  • Membrane catalytic material for rapidly catalyzing Knoevenagel condensation reaction at room temperature with high conversion rate

    CN114618583A