Preparation process of ultrahigh-toughness anti-fatigue high-adhesion eutectic gel

By introducing crystal structure and nanoparticle connection structure into the eutectic gel, and through specific component ratios and processing steps, the problems of eutectic gel's insufficient resistance to notch fatigue and energy dissipation are solved, and high strength, toughness, and energy dissipation are achieved. Eutectic gel material with fatigue resistance and conductivity, suitable for use in multiple deformations and complex environments.

CN118791815APending Publication Date: 2024-10-18HUNAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411156276.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Eutectic gel has deficiencies in notch fatigue resistance and energy dissipation capabilities, making it difficult to achieve high strength, toughness and fatigue resistance while maintaining conductivity and adhesion.

Method used

The crystal structure and nanoparticle connection structure are introduced into the eutectic gel, and a semi-fluid colloid is formed through a specific proportion of polyvinyl alcohol, nano-plant fiber and eutectic solvent, and a freezing-heat treatment step to further strengthen the strength and strength of the material. Anti-fatigue properties while maintaining conductivity and adhesion.

Benefits of technology

Eutectic gel materials that achieve high strength, toughness, fatigue resistance, conductivity and adhesion have excellent tensile strength, elongation at break, tear energy, fatigue threshold and conductivity, and are suitable for multiple deformations and Used in complex environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118791815A_ABST
    Figure CN118791815A_ABST
Patent Text Reader

Abstract

The invention relates to ultrahigh-toughness anti-fatigue high-adhesion eutectic gel, which is prepared from polyvinyl alcohol, nano plant fiber and a eutectic solvent and is prepared by circulating freezing-heat treatment after mutual dissolution of a water solvent and the eutectic solvent, the gel not only has a polyvinyl alcohol crystal region and hydrogen bond interaction between polyvinyl alcohol and a eutectic solvent, but also has combination and connection of nano plant fibers crossing a polyvinyl alcohol phase and a eutectic phase; the gel has excellent strength, toughness and fatigue resistance, has good cohesiveness to plastics and metals, has certain conductivity, can be used in a wide temperature range, and has wide application prospects in the fields of sensing, biological medicine and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a gel material, in particular to a gel material with ultra-high toughness, notch fatigue resistance, high adhesion, antifreeze and electrical conductivity. Background Art

[0002] With the rise of artificial intelligence and implantable and wearable electronic devices, gel, as a soft material, has natural advantages in morphology and performance, but its mechanical fragility seriously affects its application. In engineering applications, gel materials are often required to have excellent toughness to ensure their stability in large deformations, and also to have fatigue resistance so that their mechanical properties will not be reduced in repeated deformations; more importantly, they should be able to be used sustainably without failure after minor damage occurs, and all of this needs to be combined with functionality, which places high demands on the structural construction of gels.

[0003] A variety of strategies for strengthening the mechanical properties of gels have been proposed, and the core idea is to achieve structural uniformity and stress dispersion by constructing different topological structures, such as using a double network structure, a four-arm cross-linked balanced structure, adding nanoparticles, using a heterogeneous structure, and promoting polymer crystallization. However, the synergy of strength, toughness, and fatigue is difficult to achieve, and it is even more difficult to meet some functional requirements after achieving mechanical properties.

[0004] In recent years, the emergence of eutectic gels has provided a method for the design and development of ultra-high strength and toughness gels. Eutectic gels introduce eutectic solvents into polymer networks, which greatly improve strength and toughness by strengthening hydrogen bonds and combining the energy dissipation of organic solvents. At the same time, the ionic properties of the eutectic solvents themselves also give the gel a certain conductivity for use in fields such as sensing. For example, Wang et al. successfully synthesized a high-strength polyvinyl alcohol-based eutectic gel through solvent-induced microphase separation technology. During the preparation process, polyvinyl alcohol is first dissolved in water, and then an environmentally friendly deep eutectic solvent (DES, composed of choline chloride and glycerol) is added to promote the microphase separation of polyvinyl alcohol. The cross-linked structure formed in this process gives the eutectic gel excellent mechanical properties, with a tensile strength of up to 1.2 MPa and an elongation at break of up to 405%. At minus 40 °C, it maintains a good conductivity of 0.62 S / m ( Langmuir , 2022, 38(40): 12189). Chen et al. designed and fabricated a copolymer with super-strong and super-elastic properties in a deep eutectic solvent by using a waterborne polyurethane (WPU) network reinforced by two-dimensional nanosheets. The copolymer exhibited excellent elasticity and flexibility through non-covalent crosslinking induced by two-dimensional nanosheets, and its elongation at break increased to 2071%. In addition, the co-gel exhibited high ionic conductivity and high strain sensitivity (ACS Applied Materials & Interfaces, 2022, 14(35): 40276).

[0005] Although the eutectic gel has demonstrated very excellent performance, its notch fatigue resistance is still poor and its energy dissipation capacity is still insufficient. In view of the above problems, the present invention further enhances the strength and fatigue resistance of the material by further introducing a crystalline structure and a nanoparticle connection structure into the eutectic, and maintains the conductivity and adhesion of the eutectic gel, making it more potential for application. Summary of the invention

[0006] The present invention is dedicated to overcoming at least one of the current technical difficulties and providing a eutectic gel material, in particular, providing a eutectic gel material with high toughness, high adhesion, high fatigue resistance and antifreeze.

[0007] The objective of the present invention is achieved through the following technical solutions: An ultra-high-toughness, fatigue-resistant and high-adhesion eutectic gel, composed of polyvinyl alcohol, nano-plant fibers and eutectic solvent, with the specific component ratio being: The mass concentration of the polyvinyl alcohol in the eutectic solvent is between 5-20%; the mass of the nano-plant fiber is between 8-30% of the polyvinyl alcohol; Preferably, the mass concentration of polyvinyl alcohol in the eutectic solvent is between 10-20%; the mass of the nano-plant fiber is between 12-24% of the polyvinyl alcohol; Further, the preparation process of the gel is: I: PVA is added into water, heated to the temperature at which PVA can be dissolved, and then stirred to form an aqueous solution with a mass concentration of 15%-25%. The aqueous solution is added into the eutectic solvent, and then the nanocellulose is added after rapid continuous stirring. The mixture is stirred at 300-600 rpm for 10-20 minutes, and then ultrasonically vibrated for 30-60 minutes, during which the temperature is kept constant, to obtain a semi-fluid colloid; II: After the semi-fluid colloid is cooled to room temperature, it is placed in a freezer at -30°C to -50°C for 8-12 hours, then taken out and placed in a 70-90°C oven, and heated until the water content in the gel is reduced by 15-25%; III: After taking out the gel, repeat the freezing-heat treatment steps of II 3-5 times until the water in the gel is completely evaporated to obtain the final gel material.

[0008] Furthermore, the dissolution temperature of A is between 50-100°C.

[0009] Furthermore, the viscosity of the semi-fluid gel is between 200-600 cp.

[0010] Furthermore, the semi-fluid gel is formed after being frozen at -30°C to -50°C for 8-12 hours for the first time, and the water content in the gel is reduced by about 10-25% during each subsequent heating process, which can be controlled according to the change in gel weight.

[0011] Furthermore, the molecular weight of the polyvinyl alcohol is between 10,000 and 80,000, and the alcoholysis degree is between 75 and 100%. Preferably, the molecular weight is between 20,000 and 50,000, and the alcoholysis degree is between 89 and 100%, and may be 89% or 99%.

[0012] Furthermore, the eutectic liquid phase includes a synthetic eutectic solvent and a natural eutectic solvent, both of which include a hydrogen bond acceptor and a hydrogen bond donor, wherein the molar ratio of the hydrogen bond acceptor to the hydrogen bond donor is between 1:1.5-1:2.5, preferably 1:2.

[0013] Furthermore, the hydrogen bond donor may be selected from polyols such as glycerol, urea, organic acids such as carboxylic acids, and natural ones such as glucose; the synthetic hydrogen bond acceptor may be selected from quaternary ammonium salts such as choline chloride, and natural ones such as menthol or thymol.

[0014] Furthermore, the particle size of the nano-plant fiber is between 20-100 nm, and the aspect ratio is between 10-100.

[0015] Furthermore, the nano-plant fibers may be derived from wood fibers, bamboo fibers, straw fibers, cotton fibers and other agricultural and forestry plant fibers.

[0016] Furthermore, the polyvinyl alcohol exists mainly in a crystalline form in the gel, and the crystallinity of the polyvinyl alcohol in the gel is between 25-40%; the crystallinity is determined by first determining the crystallinity and melting enthalpy of a polyvinyl alcohol gel standard sample prepared with an aqueous solution of the same concentration, then determining the melting peak of the prepared sample at the same temperature by DSC, and calculating the crystallinity by the ratio.

[0017] Furthermore, the process of forming crystals of polyvinyl alcohol in the gel is formed through freezing and heat treatment processes, mainly through the freezing process.

[0018] Furthermore, in the gel, both the polyvinyl alcohol phase and the eutectic phase exist as continuous phases.

[0019] Further, the performance of the gel and the corresponding test method are as follows: The test method for the tensile strength and elongation at break of the gel is as follows: the gel is prepared into a dumbbell-shaped standard sample with a thickness of 1 mm, and tested by a universal mechanical testing instrument at a tensile rate of 10 mm / min.

[0020] The tearing energy test method of gel is as follows: prepare a trouser leg-shaped sample (50×20×1 mm), cut a 20 mm long notch before testing, fix the two trouser legs on the two tensile arms of the universal testing machine, and stretch them at a speed of 100 mm / min until the two trouser legs are completely pulled apart. Tear energy (J / m 2 ) is calculated as: T=2Fmax / w, where Fmax is the maximum tensile force during the tearing process and w is the thickness of the hydrogel sample.

[0021] The fatigue threshold of the gel is measured and calculated as follows: in the multi-cycle peeling test, a cyclic peeling force less than the stable peeling force is applied, and the change of the interface crack extension c during the N cycles of this force is recorded; at the same time, the energy release rate is recorded and calculated as G = Fa / W, where Fa is the stable peeling force and W is the width of the sample; with the interface crack propagation rate dc / dN as the vertical coordinate and G = Fa / W as the horizontal coordinate, the focus of the recorded point and the x-axis is the fatigue threshold of the gel. G 0 , the unit is J m −2 .

[0022] The adhesion test method is as follows: 80 mm × 15 mm × 1.5 mm gel is adhered to the surface of different substrates, and peeled off at 90° using a universal mechanical tester at a rate of 10 mm / min. The maximum peel force (N / m) is obtained as follows: maximum peel force in the curve / sample width, and the toughness of the bonding interface is obtained as follows: area under the peeling curve / peeling area, in J m −2 .

[0023] The conductivity test method of the gel is as follows: the gel sample is cut into blocks of 1 cm×1 cm×1 mm, and an electrochemical workstation is used to test at room temperature to obtain a Nyquist curve, and the conductivity (S / m) is calculated.

[0024] All the above tests were carried out under constant temperature conditions, and the o C and -20 o C. Since the properties of the adhered material also change under freezing conditions, no adhesion data are provided.

[0025] Further, the gel has very excellent properties; Its tensile strength is between 3.6-9.8MPa; Its elongation at break is between 900-2500%; Its toughness ranges from 21.2-36.8MJ / m 3 between; Repeated stretching 500 times at 200% deformation does not cause damage, and the strength reduction value is within 20%; Fatigue threshold of gel G 0 Between 124-236 J m −2 between; The gel is electrically conductive, with a conductivity ranging from 0.42 to 0.87 S / m. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 is the tensile curve of the gel prepared in Example 1; Figure 2 The peeling force curves of the gel prepared in Example 1 adhered to different substrate surfaces; Figure 3 This is the Nyquist curve of the gel prepared in Example 1, which is used to calculate the conductivity of the gel. DETAILED DESCRIPTION

[0027] The embodiments of the present application will be described in detail below in conjunction with examples, but those skilled in the art will understand that the following examples are only used to illustrate the present application and should not be construed as limiting the scope of the present application.

[0028] Example 1 An ultra-high-toughness, fatigue-resistant and high-adhesion eutectic gel, composed of polyvinyl alcohol, nano-plant fibers and eutectic solvent, with the specific component ratio being: The mass concentration of the polyvinyl alcohol in the eutectic solvent is 12%; the mass of the nano-plant fiber is between 25% of the polyvinyl alcohol; The preparation process of the gel is: I: PVA was added into water, heated to the temperature at which PVA can be dissolved, and then stirred to form an aqueous solution with a mass concentration of 20%. The aqueous solution was added into the eutectic solvent, and then the nanocellulose was added after rapid continuous stirring. The mixture was stirred at 450 rpm for 15 minutes, and then ultrasonically vibrated for 40 minutes, during which the temperature was kept constant, to obtain a 320 cp semi-fluid colloid. II: After the semi-fluid colloid is cooled to room temperature, it is placed in a -40°C freezer for 10 hours, then taken out and placed in an 80°C oven and heated until the water content in the gel is reduced by 22%; III: After taking out the gel, repeat the freezing-heat treatment steps of II for 4 times, evaporating the water in the gel evenly each time until the water in the gel is completely evaporated to obtain the final gel material.

[0029] The molecular weight of the polyvinyl alcohol is between 40,000 and 60,000, and the alcoholysis degree is 89%.

[0030] The eutectic liquid phase includes a synthetic eutectic solvent, which is composed of glycerol and choline chloride, and the molar ratio of the two is 1:2.

[0031] The nano-plant fiber is derived from straw fiber, has a particle size between 40-80nm, and an aspect ratio between 20-50.

[0032] The polyvinyl alcohol exists mainly in the form of crystals in the gel, and the proportion of polyvinyl alcohol involved in crystallization accounts for about 32% of the total amount of polyvinyl alcohol.

[0033] The properties of the prepared gels are shown in Table 1.

[0034] At the same time, if Figure 1 The tensile curve of the gel prepared in Example 1 shows that it has excellent tensile strength and great deformation resistance, and its tensile strength and elongation at break are 4.2 MPa and 1460% respectively; Figure 2 The peeling curves (peeling force / sample width, in N / m) of the gel prepared in Example 1 adhered to different substrate surfaces. It can be seen from the figure that it has better adhesion on the glass surface due to hydrogen bonding; Figure 3 The Nyquist curve of the gel prepared in Example 1 was obtained by testing with an electrochemical workstation, and the calculated conductivity was 0.42 S / m.

[0035] Example 2 An ultra-high-toughness, fatigue-resistant and high-adhesion eutectic gel, composed of polyvinyl alcohol, nano-plant fibers and eutectic solvent, with the specific component ratio being: The mass concentration of the polyvinyl alcohol in the eutectic solvent is 16%; the mass of the nano-plant fiber is between 18% of the polyvinyl alcohol; The preparation process of the gel is: I: PVA was added into water, heated to the temperature at which PVA can be dissolved, and then stirred to form an aqueous solution with a mass concentration of 18%. The aqueous solution was added into the eutectic solvent, and then the nanocellulose was added after rapid continuous stirring. The mixture was stirred at 500 rpm for 12 minutes, and then ultrasonically vibrated for 45 minutes, during which the temperature was kept constant, to obtain a 440 cp semi-fluid colloid. II: After the semi-fluid colloid is cooled to room temperature, it is placed in a -40°C freezer for 12 hours, then taken out and placed in a 90°C oven and heated until the water content in the gel is reduced by 20%; III: After taking out the gel, repeat the freezing-heat treatment steps of II for 5 times, evaporating the water in the gel evenly each time until the water in the gel is completely evaporated to obtain the final gel material.

[0036] The molecular weight of the polyvinyl alcohol is between 60,000 and 80,000, and the alcoholysis degree is 99%.

[0037] The eutectic liquid phase includes a synthetic natural eutectic solvent, which is composed of carboxylic acid and menthol, and the molar ratio of the two is 1:2.

[0038] The nano-plant fiber is derived from straw fiber, has a particle size between 50-100 nm, and an aspect ratio between 30-80.

[0039] The polyvinyl alcohol exists mainly in the form of crystals in the gel, and the proportion of polyvinyl alcohol involved in crystallization accounts for about 32% of the total amount of polyvinyl alcohol.

[0040] The properties of the prepared gels are shown in Table 1.

[0041] Example 3 An ultra-high-toughness, fatigue-resistant and high-adhesion eutectic gel, composed of polyvinyl alcohol, nano-plant fibers and eutectic solvent, with the specific component ratio being: The mass concentration of the polyvinyl alcohol in the eutectic solvent is 18%; the mass of the nano-plant fiber is between 12% of the polyvinyl alcohol; The preparation process of the gel is: I: PVA was added into water, heated to the temperature at which PVA can be dissolved, and then stirred to form an aqueous solution with a mass concentration of 22%. The aqueous solution was added into the eutectic solvent, and then the nanocellulose was added after rapid continuous stirring. The mixture was stirred at 350 rpm for 18 minutes, and then ultrasonically vibrated for 50 minutes, during which the temperature was kept constant, to obtain a 480 cp semi-fluid colloid. II: After the semi-fluid colloid is cooled to room temperature, it is placed in a -45°C freezer for 10 hours, then taken out and placed in an 85°C oven and heated until the water content in the gel is reduced by 20%; III: After taking out the gel, repeat the freezing-heat treatment steps of II for 4 times, evaporating the water in the gel evenly each time until the water in the gel is completely evaporated to obtain the final gel material.

[0042] The molecular weight of the polyvinyl alcohol is between 40,000 and 60,000, and the alcoholysis degree is 99%.

[0043] The eutectic liquid phase includes a synthetic natural eutectic solvent, which is composed of urea and thymol, and the molar ratio of the two is 1:2.2.

[0044] The nano plant fiber is sourced from bamboo fiber, has a particle size between 40-80nm, and an aspect ratio between 10-50.

[0045] The polyvinyl alcohol exists mainly in the form of crystals in the gel, and the proportion of polyvinyl alcohol involved in crystallization accounts for about 34% of the total amount of polyvinyl alcohol.

[0046] The properties of the prepared gels are shown in Table 1.

[0047] Example 4 An ultra-high-toughness, fatigue-resistant and high-adhesion eutectic gel, composed of polyvinyl alcohol, nano-plant fibers and eutectic solvent, with the specific component ratio being: The mass concentration of the polyvinyl alcohol in the eutectic solvent is 10%; the mass of the nano-plant fiber is between 28% of the polyvinyl alcohol; The preparation process of the gel is: I: PVA was added into water, heated to the temperature at which PVA can be dissolved, and then stirred to form an aqueous solution with a mass concentration of 18%. The aqueous solution was added into the eutectic solvent, and then the nanocellulose was added after rapid continuous stirring. The mixture was stirred at 500 rpm for 15 minutes, and then ultrasonically vibrated for 40 minutes, during which the temperature was kept constant, to obtain a 360 cp semi-fluid colloid. II: After the semi-fluid colloid is cooled to room temperature, it is placed in a -50°C freezer for 8 hours, then taken out and placed in an 80°C oven and heated until the water content in the gel is reduced by 24%; III: After taking out the gel, repeat the freezing-heat treatment steps of II for 5 times, evaporating the water in the gel evenly each time until the water in the gel is completely evaporated to obtain the final gel material.

[0048] The molecular weight of the polyvinyl alcohol is between 20,000 and 40,000, and the alcoholysis degree is 79%.

[0049] The eutectic liquid phase includes a synthetic natural eutectic solvent, which is composed of glucose and menthol, and the molar ratio of the two is 1:2.4.

[0050] The nano plant fiber is sourced from bamboo fiber, has a particle size between 30-100 nm, and an aspect ratio between 20-60.

[0051] The polyvinyl alcohol exists mainly in the form of crystals in the gel, and the proportion of polyvinyl alcohol involved in crystallization accounts for about 36% of the total amount of polyvinyl alcohol.

[0052] The properties of the prepared gels are shown in Table 1.

[0053] Example 5 An ultra-high-toughness, fatigue-resistant and high-adhesion eutectic gel, composed of polyvinyl alcohol, nano-plant fibers and eutectic solvent, with the specific component ratio being: The mass concentration of the polyvinyl alcohol in the eutectic solvent is 8%; the mass of the nano-plant fiber is 30% of the polyvinyl alcohol; The preparation process of the gel is: I: PVA was added into water, heated to the temperature at which PVA can be dissolved, and then stirred to form an aqueous solution with a mass concentration of 22%. The aqueous solution was added into the eutectic solvent, and then the nanocellulose was added after rapid continuous stirring. The mixture was stirred at 480 rpm for 18 minutes, and then ultrasonically vibrated for 35 minutes, during which the temperature was kept constant, to obtain a 280 cp semi-fluid colloid. II: After the semi-fluid colloid is cooled to room temperature, it is placed in a -45°C freezer for 10 hours, then taken out and placed in an 85°C oven and heated until the water content in the gel is reduced by 20%; III: After taking out the gel, repeat the freezing-heat treatment steps of II for 5 times, evaporating the water in the gel evenly each time until the water in the gel is completely evaporated to obtain the final gel material.

[0054] The molecular weight of the polyvinyl alcohol is between 35000 and 45000, and the alcoholysis degree is 89%.

[0055] The eutectic liquid phase includes a synthetic natural eutectic solvent, which is composed of urea and choline chloride, and the molar ratio of the two is 1:1.8.

[0056] The nano plant fiber is sourced from bamboo fiber, has a particle size between 40-100 nm, and an aspect ratio between 20-80.

[0057] The polyvinyl alcohol exists mainly in the form of crystals in the gel, and the proportion of polyvinyl alcohol involved in crystallization accounts for about 34% of the total amount of polyvinyl alcohol.

[0058] The properties of the prepared gels are shown in Table 1.

[0059] Table 1. Properties of gels prepared in Examples Example 1 Example 2 Example 3 Example 4 Example 5 Tensile strength (MPa) 4.2 5.7 8.4 3.9 3.7 Elongation at break (%) 1460 1237 986 1524 1348 <![CDATA[Tear energy (J / m 2 )]]> 896 1023 1365 842 789 Peel force (N / m) Glass: 486 Titanium alloy: 364 PET: 288 Glass: 389 Titanium alloy: 289 PET: 136 Glass: 402 Titanium alloy: 307 PET: 105 Glass: 521 Titanium alloy: 449 PET: 147 Glass: 498 Titanium alloy: 418 PET: 161 <![CDATA[Adhesive interface toughness (J / m 2 ).]]> Glass: 427 Titanium alloy: 314 PET: 186 Glass: 362 Titanium alloy: 217 PET: 115 Glass: 383 Titanium alloy: 248 PET: 92 Glass: 475 Titanium alloy: 417 PET: 115 Glass: 423 Titanium alloy: 349 PET: 124 <![CDATA[Fatigue threshold G 0 (J / m 2 )]]> 164 176 207 149 183 Conductivity (S / m) 0.42 0.46 0.37 0.44 0.53

Claims

1. An ultra-high-toughness, fatigue-resistant and high-adhesion eutectic gel, composed of polyvinyl alcohol, nano-plant fibers and eutectic solvent, with the specific component ratio being: The mass concentration of polyvinyl alcohol in the eutectic solvent is between 5-20%; the mass of the nano-plant fiber is between 8-30% of the polyvinyl alcohol; Its preparation process is: I: PVA is added into water, heated to the temperature at which PVA can be dissolved, and then stirred to prepare an aqueous solution with a mass concentration of 15%-25%. The aqueous solution is added into the eutectic solvent, and then the nanocellulose is added after rapid continuous stirring. The mixture is stirred at 300-600 rpm for 10-20 minutes, and then ultrasonically vibrated for 30-60 minutes, during which the temperature is kept constant, to obtain a semi-fluid colloid with a concentration of 200-600 cp; II: After the semi-fluid colloid is cooled to room temperature, it is placed in a freezer at -30°C to -50°C for 8-12 hours, then taken out and placed in a 70-90°C oven, and heated until the water content of the gel is reduced by 15-25%; III: After taking out the gel, repeat the freezing-heat treatment steps of II for 3-5 times, and heat treat each time until the water mass in the gel is reduced by 15-25%, until the water in the gel is completely evaporated to obtain the final gel material.

2. The ultra-high-toughness, fatigue-resistant and high-adhesion eutectic gel according to claim 1, characterized in that: The molecular weight of the polyvinyl alcohol is between 20,000 and 80,000, and the alcoholysis degree is between 75 and 100%.

3. The ultra-high-toughness, fatigue-resistant and high-adhesion eutectic gel according to claim 1, characterized in that: The eutectic solvents include synthetic eutectic solvents and natural eutectic solvents.

4. The ultra-high-toughness, fatigue-resistant and high-adhesion eutectic gel according to claim 1, characterized in that: The particle size of the nano-plant fiber is between 20-100 nm, and the aspect ratio is between 10-100.

5. The ultra-high-toughness, fatigue-resistant and high-adhesion eutectic gel according to claim 1, characterized in that: The polyvinyl alcohol exists in the gel mainly in a crystalline form, and the crystallinity of the polyvinyl alcohol in the gel is between 25-40%.

6. The ultra-high-toughness, fatigue-resistant and high-adhesion eutectic gel according to claim 1, characterized in that: In the gel, both the polyvinyl alcohol phase and the eutectic phase exist as continuous phases.