Organic-inorganic multi-stage core-shell structure coloring agent with excellent water resistance and dispersion stability as well as preparation method and application of organic-inorganic multi-stage core-shell structure coloring agent
By using SiO2@cationic dye@SiO2 organic-inorganic multi-level core-shell microspheres as the colorant of the ink, the water solubility and weather resistance problems of the cationic dye in the ink are solved, and the excellent color saturation and water resistance of the ink are achieved. Expands its application scope and improves information preservation capabilities.
Patent Information
- Application Number
- CN202410779029.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-06-17
AI Technical Summary
Existing cationic dyes in ink have strong water solubility and poor weather resistance, causing written or painting information to be easily lost when exposed to water and sunlight. There is a lack of cationic colorants with excellent color saturation, weather resistance and water resistance.
Using SiO2@cationic dye@SiO2 organic-inorganic multi-level core-shell microspheres as the colorant, the core-shell structure is formed through the combination of the surface charge of the SiO2 microspheres and the cationic dye, and the SiO2 coating layer is used to prepare a product with high color saturation and Ink with excellent water resistance.
It significantly improves the environmental adaptability of cationic dyes and expands its application scope. The ink writes smoothly and the writing is not easy to fade in water. It has excellent water resistance and is suitable for long-term preservation of markers and high-end paintings.
Smart Images

Figure CN118791886A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of water-resistant materials, in particular to a water-resistant pen ink and a preparation method thereof, and belongs to the field of new material research. Background Art
[0002] Ink plays a role in human production and life and covers many fields, and is closely related to people, such as pen ink for writing, pigment ink used in paintings or other works of art, and high-brightness printing ink used in the printing field. Therefore, it is particularly important to further optimize the performance of ink.
[0003] There are many types of ink formulas. The existing colorants are mainly divided into two types: pigment type and dye type. The pigments used in pigment type colorants are divided into inorganic pigments and organic pigments. Inorganic pigments mainly include oxides, hydroxides, sulfides, metals and various colored non-metallic salts. Organic pigments mainly include azo pigments, acidic and alkaline dye lake pigments, polycyclic ketone pigments, etc.
[0004] Dye-type colorants are composed of soluble molecules and can be stably dispersed in the ink system. They have the advantages of bright colors and low cost. Cationic dyes are widely used in various marker inks because of their heat resistance, sun resistance, acid and alkali resistance, etc. However, cationic dyes have defects such as strong water solubility and poor weather resistance. When used as ink colorants, written or drawn information is often lost due to water and sunlight exposure. Therefore, it is urgent to develop a cationic colorant with excellent color saturation, weather resistance and water resistance to solve this problem. Summary of the invention
[0005] The present invention aims to provide a water-resistant pen ink and a preparation method thereof. 2 @Cationic dyes@SiO 2 Organic-inorganic multi-level core-shell microspheres are used as colorants to prepare pen inks, giving the inks excellent weather resistance and water resistance. The preparation process of the organic-inorganic multi-level core-shell structure colorant is simple, safe and environmentally friendly. The marker ink prepared with it has the characteristics of color saturation, not easy to fade in water, and excellent weather resistance, which greatly improves the environmental adaptability of cationic dyes and expands the application range of cationic dyes.
[0006] In order to achieve the above-mentioned invention object, the main technical scheme of the present invention is:
[0007] The present invention provides an organic-inorganic multi-level core-shell structure colorant with excellent water resistance and dispersion stability. The colorant structure is SiO 2 @Cationic dyes@SiO 2, SiO 2The surface charge of the microspheres is -20mV to -50mV, the particle size is 80nm to 800nm, and the SiO 2 The surface of the microspheres is SiO2 with a core-shell structure formed by cationic dyes. 2 @Cationic dye; SiO 2 @Cationic dye outer layer coated with SiO 2 ; Coating layer SiO 2 The thickness is 5nm-60nm, and the cationic dye is one or more of the colors such as yellow, orange, brilliant red, red, brilliant purple, blue, turquoise blue, etc. Colorant SiO 2 @Cationic dyes@SiO 2 The particle size is 90nm~1000nm, and the surface charge is -25mV~-45mV. It has excellent dispersion stability, high color saturation and water resistance. It can be used as a colorant to prepare marker ink, which can write smoothly and the writing is water-resistant.
[0008] Furthermore, in the above technical solution, the yellow cationic dye is one or more of X-8GL, X-8GLN, E-3RD, X-2RL, 7GLL, 7GL, X-3RL, and X-GL.
[0009] Furthermore, in the above technical solution, the red cationic dye is one or more of GTL, GTLN, 2BL, 2GL, and X-GRL.
[0010] Furthermore, in the above technical solution, the blue cationic dye is one or more of X-GRRL, X-GRL, FRL, X-BL, M-RL, and X-GBL.
[0011] The main steps of preparing the organic-inorganic multi-level core-shell structure colorant are as follows:
[0012] ① Preparation of monodispersed SiO 2 Nanoparticles, and prepare them into a dispersion of a certain concentration;
[0013] ② The SiO prepared in ① 2 The nanoparticles are electrostatically adsorbed with a certain proportion of cationic dyes to obtain SiO 2 @Cationic dye core-shell microspheres;
[0014] ③Prepare a certain concentration of SiO 2 @Cationic dye dispersion, using The core-shell microspheres are coated with SiO 2 , and obtain SiO with high color saturation and excellent water resistance 2 @Cationic dyes@SiO 2 Organic-inorganic multi-level core-shell structure colorant.
[0015] Furthermore, in the above technical solution, the SiO 2 The particle size of the microspheres is 80nm to 800nm.
[0016] Furthermore, in the above technical solution, the monodispersed SiO 2 The concentration of the dispersion is 0.1 wt% to 40 wt%.
[0017] Furthermore, the SiO 2 The molar ratio with the cationic dye is 1:7 to 1:1, the electrostatic adsorption time is 0.3h to 48h, and the temperature is 20℃ to 60℃.
[0018] Furthermore, in the above technical solution, the core-shell microsphere SiO 2 @The mass concentration of cationic dye core-shell microspheres is 3wt% to 50wt%. The present invention provides a method for preparing marker ink, using the prepared SiO 2 @Cationic dyes@SiO 2 An organic-inorganic multi-level core-shell structure colorant is mixed with other moisturizers, bactericides, surfactants, and viscosity regulators in solvent water and stirred evenly to prepare an ink with excellent water resistance and weather resistance.
[0019] The weight percentage of each component in the formula of the marker pen ink is 3% to 15% of the colorant, 10% to 40% of the moisturizer, 0.1% to 0.4% of the bactericide, 0.1% to 0.5% of the surfactant, 0.1% to 1% of the viscosity regulator, and the rest is the solvent, which is water.
[0020] Furthermore, in the above process of preparing the ink, the humectant used may be one or more of ethylene glycol, propylene glycol, glycerol, polyethylene glycol, and glycerol.
[0021] Furthermore, in the above-mentioned process of preparing the ink, the bactericide used may be one or more of sodium benzoate, methyl benzoate, sodium benzoate, phenol, and 1,2-benzothiazoline-3-one.
[0022] Furthermore, in the above process of preparing the ink, the surfactant used may be one of colloidal silica, sodium fatty alcohol sulfate, and sodium fatty alcohol polyoxyethylene ether sulfate.
[0023] Furthermore, in the above process of preparing the ink, the viscosity modifier used may be one of xanthan gum, natural rubber, PVP (polyvinyl pyrrolidone), and polyacrylic acid.
[0024] Furthermore, in the above ink preparation process, the stirring process is carried out in a constant temperature water bath for 0.5h to 3h.
[0025] Advantageous Effects of the Invention
[0026] The present invention discloses a water-resistant pen ink and a preparation method thereof, wherein SiO 2 @Cationic dyes@SiO 2 Organic-inorganic multi-level core-shell microspheres are used as colorants to prepare marker ink, which has excellent writing performance, bright color saturation and water resistance. The present invention solves the problem of poor water resistance of writing in the existing marker ink technology, greatly improves its environmental adaptability, and is conducive to expanding the application range of markers and the long-term preservation of high-end paintings or important information. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0028] Figure 1 (a), (c), and (e) represent the SiO 2 Microspheres, SiO 2 @X-GL、SiO 2 @X-GL@SiO 2 SEM images of (b), (d) and (f) represent SiO 2 Microspheres, SiO 2 @X-GL、SiO 2 @X-GL@SiO 2 Particle size distribution diagram.
[0029] Figure 2 The SiO 2 @X-GRL@SiO 2 , digital photos of marker ink with X-GRL as colorant, immersed in water for 24 hours;
[0030] Figure 3 In Example 3, SiO 2 @X-GRL@SiO 2 Digital photograph of a marker writing performance test configured for colorant. DETAILED DESCRIPTION
[0031] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings so that the present invention can be better understood by technical researchers in the field, thereby clearly defining the protection scope of the present invention.
[0032] Example 1
[0033] SiO 2 @X-GL@SiO 2 Preparation
[0034] First, prepare monodispersed SiO 2 The microspheres are prepared as follows: 160 mL of ethanol is added to a 250 mL three-necked flask, 33 mL of deionized water and 3.3 mL of ammonia water are mixed, and ultrasonic dispersion is performed for 2 minutes, and then the mixture is added to the three-necked flask. The mixture is heated in a 60°C oil bath and mechanically stirred at a speed of 200 revolutions per minute. When the temperature reaches 60°C, 4.4 mL of tetraethyl orthosilicate (TEOS) is slowly added for 10 minutes. After the addition is complete, the reaction is stirred for 10 hours until a light blue transparent seed solution is obtained. In another 500 mL three-necked flask, 160 mL of ethanol, 40 mL of deionized water and 40 mL of ammonia water are added. At room temperature, magnetic stirring is performed at a speed of 300 revolutions per minute. 3.3 to 0.8 mL of the above seed solution is added thereto. Liquid A (containing 20 mL of LTEOS) and liquid B (consisting of 10 mL of ethanol, 8 mL of ammonia water, and 3 mL of deionized water) were added dropwise at a rate of 0.2 mL / min for 100 minutes using a syringe pump. After the addition was completed, the reaction was continued for 5 hours, and the mixture was washed three times by centrifugation with a mixed solution of ethanol and water and dried for use. A monodispersed SiO with a surface charge of -21.30 mV and a particle size of 216.93 nm was obtained. 2 Microspheres.
[0035] Weigh a certain amount of the monodisperse SiO 2 Microspheres were added with anhydrous ethanol to prepare 10wt% SiO 2 Microsphere dispersion.
[0036] Weigh a certain amount of X-GL cationic dye and make the SiO 2 SiO in microsphere dispersion 2 The molar ratio of the cationic dye was 1:1, and anhydrous ethanol and deionized water were added in a volume ratio of 1:1 to prepare a SiO 2 @X-GL solution was placed in an ultrasonic multi-frequency cleaning apparatus at 20°C and ultrasonicated for 30 minutes for use.
[0037] Take a certain amount of SiO 2 @X-GL solution, 200 mg PVP and 4.5 mL H2O were added to a test tube and ultrasonicated for 30 min, then 20 mL anhydrous ethanol was added and ultrasonicated for 30 min, and finally 0.03 mL LTEOS was added, stirred at 200 rpm for 12 h, centrifuged and washed three times with ethanol solution, and deionized water was added to prepare a SiO2 solution with a mass fraction of 20%. 2 @X-GL dispersion.
[0038] Take a certain amount of the SiO2@X-GL solution obtained above, add 200mgPVP and 4.5mLH2O into a test tube and ultrasonicate for 30min, then add 20mL anhydrous ethanol and ultrasonicate for 30min, finally add 0.03mL LTEOS, stir at 200 rpm for 12h, centrifuge and wash three times with ethanol solution, and dry to obtain SiO2@X-GL@SiO2, with a surface charge of -25.53mV and an average particle size of 276.52nm. Add deionized water to prepare a SiO2@X-GL@SiO2 dispersion with a mass fraction of 20%.
[0039] SiO 2 @X-GL@SiO 2 The composite core-shell microsphere structure is used as a colorant with a mass percentage of 10%, propylene glycol is used as a humectant with a content of 30%, sodium benzoate is used as a bactericide with a content of 0.2%, colloidal silicon is used as a surfactant with a content of 0.3%, and xanthan gum is used as a viscosity regulator with a content of 0.5%. Marker ink is prepared with water as a solvent, stirred in a constant temperature water bath for 1.5 hours, and after mixing evenly, a marker ink with water-resistant properties is obtained.
[0040] Example 2
[0041] The difference from Example 1 is that the moisturizer is replaced by polyethylene glycol, and the SiO 2 @X-GL@SiO 2 Water-resistant marker pen with colorant.
[0042] Embodiment 3-4
[0043] The difference from Example 1 is that the cationic dyes are replaced by X-GRL and X-GBL, respectively, and SiO 2 @Cationic dyes@SiO 2 Colorant, and use it to prepare marker ink, which allows smooth writing and water-resistant writing.
[0044] Comparative Example 1
[0045] The difference from Example 1 is that the colorant is replaced by X-GRL, and the marker ink is prepared therefrom.
[0046] Figure 1 It shows that SiO 2 Microspheres, SiO 2 @X-GL、SiO 2 @X-GL@SiO 2 The microspheres have uniform particle size, regular morphology and good monodispersity. 2 Microspheres, SiO 2 @X-GL、SiO 2@X-GL@SiO 2 The average particle size is 216nm, 229nm, and 276nm. From the results of the particle size distribution diagram, it can be seen that the particle size distribution of the prepared silica microspheres is narrow, indicating that the particle size of the prepared microspheres is relatively uniform and can be used for subsequent ink testing; Figure 3 It shows that SiO 2 @X-GRL@SiO 2 The marker ink prepared with the composite core-shell microsphere structure as the colorant has smooth writing and clear handwriting; Figure 2 The results show that the marker ink with SiO2@X-GRL@SiO2 as the colorant did not fade significantly after being soaked in water for 24 hours, while the marker ink with X-GRL as the colorant faded significantly after being soaked in water for 24 hours, and part of the ink dissolved in the water. This shows that the marker ink with SiO2@X-GRL@SiO2 as the colorant has better water resistance.
[0047] According to GB / T 34851-217, various indicators of the ink of Example 3 and Comparative Example 1 were tested. The results were as follows: According to the water resistance test method in standard 6.4, the ink did not fade after being tested in water for 24 hours, proving that it has excellent water resistance and meets national standards.
Claims
1. An organic-inorganic multi-stage core-shell structure colorant with excellent water resistance and dispersion stability, characterized in that: The colorant structure is SiO2@cationic dye@SiO2; the surface charge of SiO2 microspheres is -20mV~-50mV, the particle size is 80nm~800nm, the surface of SiO2 microspheres is SiO2@cationic dye forming a core-shell structure; the outer layer of SiO2@cationic dye is coated with SiO2; the thickness of the coating layer SiO2 is 5nm-60nm, the particle size of the colorant SiO2@cationic dye@SiO2 is 90nm~1000nm, and the surface charge is -25mV~-45mV.
2. The colorant according to claim 1, characterized in that: The cationic dye is one or more of yellow, orange, brilliant red, red, brilliant purple, blue and turquoise blue.
3. The method for preparing the colorant according to claim 1 or 2, characterized in that: The process steps include: ①Prepare monodispersed SiO2 nanoparticles and prepare them into a dispersion of a certain concentration; ② The SiO2 nanoparticles prepared in ① are electrostatically adsorbed with a certain proportion of cationic dyes to obtain SiO2@cationic dye core-shell microspheres; ③Prepare a certain concentration of SiO2@cationic dye dispersion, using The method is to coat SiO2 on the surface of core-shell microspheres to obtain SiO2@cationic dye@SiO2 organic-inorganic multi-level core-shell structure colorant with high color saturation and excellent water resistance.
4. The preparation method according to claim 3, wherein the yellow cationic dye is one or more of X-8GL, X-8GLN, E-3RD, X-2RL, 7GLL, 7GL, X-3RL, and X-GL; The red cationic dye is one or more of GTL, GTLN, 2BL, 2GL, and X-GRL; The blue cationic dye is one or more of X-GRRL, X-GRL, FRL, X-BL, M-RL and X-GBL.
5. The preparation method according to claim 3, characterized in that: The concentration of the monodisperse SiO2 microsphere dispersion described in step ① is 0.1wt% to 40wt%.
6. The preparation method according to claim 3, characterized in that: The molar ratio of SiO2 to cationic dye described in step ② is 1:7 to 1:1, the electrostatic adsorption time is 0.3h to 48h, and the temperature is 20℃ to 60℃.
7. The preparation method according to claim 6, characterized in that: The concentration of the core-shell microspheres SiO2@cationic dye core-shell microspheres in step ③ is 3wt% to 50wt%.
8. A method for preparing marker pen ink, characterized in that: The weight percentage of each component in the formula of the marker ink is 3% to 15% of the colorant described in claim 1 or 2, 10% to 40% of the moisturizer, 0.1% to 0.4% of the bactericide, 0.1% to 0.5% of the surfactant, 0.1% to 1% of the viscosity regulator, and the rest is water as a solvent.
9. The preparation method according to claim 8, characterized in that: The moisturizing agent is one or more of ethylene glycol, propylene glycol, glycerin, polyethylene glycol, and glycerol; The bactericide may be one or more of sodium benzoate, methyl benzoate, sodium benzoate, phenol, and 1,2-benzothiazoline-3-one; The surfactant may be one of colloidal silicon, sodium fatty alcohol sulfate, and sodium fatty alcohol polyoxyethylene ether sulfate; The viscosity regulator can be one of xanthan gum, natural rubber, PVP (polyvinyl pyrrolidone), and polyacrylic acid.
10. The preparation method according to claim 8, characterized in that: Prepare the various components of the ink, put them into a constant temperature water bath and stir them for 0.5 h to 3 h, and obtain the marker ink after mixing them evenly.
Citation Information
Patent Citations
Preparation method of core-pigment layer-shell compound structural electrophoretic particles used for electronic ink
CN101200548A
Erasable ink and preparation method thereof
CN101993635A
Practical water-based white board pen ink and preparation method thereof
CN104893419A
Aqueous composite nanometer coloring agent preparation method
CN105001673A
Fluorescent quick-dry ink and preparation method thereof
CN106634219A