Composition, external cavity coating and preparation method and application of external cavity coating
By using a composite coating of silicone, anti-fingerprint additives and cross-linking additives on micro-baking equipment, the problem of insufficient anti-fingerprint and moisture-heat resistance of the outer cavity coating in the existing technology is solved, and high temperature, water and moisture resistance are achieved. Excellent performance in cooking and hot and humid environments, extending the service life of the equipment.
Patent Information
- Application Number
- CN202310386565.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-18
AI Technical Summary
The outer cavity coating of existing micro-baked products cannot effectively resist fingerprints and oil stains, and has poor resistance to moisture and heat, resulting in a short service life. It is also difficult for the existing technology to have high temperature resistance, water boiling resistance and fingerprint resistance at the same time.
A composition is used to prepare the outer cavity coating, including 14-73 parts by weight of silicone resin, 5-53 parts by weight of anti-fingerprint additives and 0.5-24 parts by weight of cross-linking assistants, and is formed by heat treatment coating to enhance the coating’s high temperature resistance, water boiling resistance and fingerprint resistance.
The outer cavity coating formed has excellent high temperature resistance, water boiling resistance and moisture and heat resistance. It can effectively prevent high-temperature oxidation and corrosion of the substrate. It also has excellent anti-fingerprint properties. It does not leave fingerprints when touched by fingers, and oil stains are easy to clean. Extended equipment service life.
Smart Images

Figure BDA0004174272510000091 
Figure BDA0004174272510000101 
Figure HDA0004174272530000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of kitchen appliance materials, and in particular relates to a composition, an outer cavity coating, and a preparation method and application thereof. Background Art
[0002] With the improvement of living standards, people's attention to kitchen appliances is not only on the function of the inner cavity of the product, but also on the appearance of the product. Excellent appearance is not only good-looking but also stain-resistant, among which anti-fingerprint becomes an important feature. At present, the outer covers of microwave ovens, ovens and other microwave ovens are mainly metal outer covers + decorative coatings. Although they look good, they are not resistant to fingerprints and oil stains. During use, fingerprints and oil stains will seriously affect the appearance. Therefore, the outer cavity coating formed by the existing outer cavity material is difficult to meet the consumer's requirements for anti-fingerprint performance, which brings great troubles to product users.
[0003] In addition, the bonding force between the existing outer cavity coating and the substrate is weak. After long-term use, the outer cavity coating is easy to fall off from the substrate, resulting in failure of the outer cavity coating, which makes it difficult for the existing outer cavity coating to resist the erosion of the humid and hot environment for a long time. In the prior art, there is no outer cavity coating material that can simultaneously have high temperature resistance, boiling resistance, humid and hot environment resistance and excellent anti-fingerprint performance. Summary of the invention
[0004] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, the purpose of the present invention is to provide a composition, an outer cavity coating, and a preparation method and application thereof. The outer cavity coating formed by the composition system of the present invention not only has relatively excellent high temperature resistance, water boiling resistance and wet heat resistance, but also can effectively prevent the substrate from high temperature oxidation and corrosion; at the same time, the outer cavity coating formed by the composition system also has excellent anti-fingerprint performance.
[0005] In one aspect of the present invention, the present invention provides a composition. According to an embodiment of the present invention, the composition is used to prepare an outer cavity coating, and the composition comprises: 14-73 parts by weight of silicone resin, 5-53 parts by weight of anti-fingerprint auxiliary agent, 0.5-24 parts by weight of cross-linking auxiliary agent and 20-63 parts by weight of solvent.
[0006] According to the composition of the embodiment of the present invention, the outer cavity coating formed by the composition system not only has relatively excellent high temperature resistance, boiling water resistance and moisture and heat resistance, but also can effectively prevent high temperature oxidation and corrosion of the substrate; at the same time, the outer cavity coating formed by the composition system also has excellent anti-fingerprint performance.
[0007] In addition, the composition according to the above embodiment of the present invention may also have the following additional technical features:
[0008] In some embodiments of the present invention, the composition comprises: 20-60 parts by weight of the silicone resin, 6-32 parts by weight of the anti-fingerprint agent, 0.5-18 parts by weight of the cross-linking agent and 32-60 parts by weight of the solvent.
[0009] In some embodiments of the present invention, the anti-fingerprint auxiliary agent includes at least one of methyltriethoxysilane, tetraethoxysilane, polyether-modified silicone, isocyanate-modified silicone, acrylic copolymer and siloxane-modified polyurethane.
[0010] In some embodiments of the present invention, the silicone resin includes at least one of methylphenyl silicone resin, methyl silicone resin, low phenylmethyl silicone resin, epoxy-modified silicone resin, silicone polyester-modified resin, benzyl transparent silicone resin, methyl transparent silicone resin, mica bonding silicone resin, polymethyl silicone resin, amino silicone resin, fluorosilicone resin, silicone resin solution, silicone-epoxy resin, and silicone polyester resin.
[0011] In some embodiments of the present invention, the crosslinking aid includes at least one of a polycarbodiimide crosslinking aid, an acrylate crosslinking aid, an organic peroxide crosslinking aid, a polyamine crosslinking aid, a polyol crosslinking aid, a glycidyl ether crosslinking aid, a silicone crosslinking aid, a benzenesulfonic acid crosslinking aid, an aziridine crosslinking aid, an olefin monomer crosslinking aid and an inorganic crosslinking aid.
[0012] In some embodiments of the present invention, the polyamine crosslinking aid includes at least one of propylene diamine and MOCA; and / or, the polyol crosslinking aid includes at least one of polyethylene glycol, polypropylene glycol, trimethylolpropane, and trimethylolethane; and / or, the inorganic crosslinking aid includes at least one of zinc oxide, aluminum chloride, and aluminum sulfate; and / or, the silicone crosslinking aid includes at least one of tetraethyl orthosilicate, methyl orthosilicate, and trimethoxysilane; and / or, the benzenesulfonic acid crosslinking aid includes at least one of p-toluenesulfonic acid and p-toluenesulfonyl chloride; and / or, the acrylate The crosslinking aid of the type includes at least one of 1,4-butylene glycol diacrylate, ethylene glycol dimethacrylate, TAC, butyl acrylate, HEA, HPA, HEMA, HPMA and MMA; and / or, the organic peroxide crosslinking aid includes at least one of dicumyl peroxide and bis-2,4-dichlorobenzoyl peroxide; and / or, the olefin monomer crosslinking aid includes at least one of acrylic acid, hydroxyethyl acrylate, hydroxypropyl acrylate, methacrylic acid, hydroxyethyl methacrylate, hydroxypropyl methacrylate, divinylbenzene, N-hydroxymethyl acrylamide and diacetone acrylamide.
[0013] In some embodiments of the present invention, the solvent includes at least one of an alkane solvent, an ether solvent, a ketone solvent, and a benzene-derived biosolvent.
[0014] In another aspect of the present invention, the present invention provides an outer cavity coating. According to an embodiment of the present invention, the outer cavity coating is prepared by using the composition described in the above embodiment. As a result, the outer cavity coating has relatively excellent high temperature resistance, boiling resistance and moisture and heat resistance, and can also effectively prevent the substrate from high temperature oxidation and corrosion; at the same time, the outer cavity coating also has excellent anti-fingerprint performance, no fingerprints are left when touched by fingers, and oil stains are easy to clean.
[0015] In a third aspect of the present invention, the present invention provides a method for preparing the above-mentioned outer cavity coating. According to an embodiment of the present invention, the method comprises:
[0016] (1) mixing a silicone resin, an anti-fingerprint additive, a cross-linking additive, and a solvent to form a coating solution;
[0017] (2) The coating liquid is formed on a substrate and heat-treated to form the outer cavity coating on the substrate.
[0018] According to the method for preparing the above-mentioned outer cavity coating of the embodiment of the present invention, the outer cavity coating prepared by the method has relatively excellent high temperature resistance, boiling resistance and moisture and heat resistance, and can also effectively prevent the substrate from high temperature oxidation and corrosion; at the same time, it also has excellent anti-fingerprint performance, no fingerprints are left when touched by fingers, and oil stains are easy to clean. The preparation method is simple in steps and easy to operate.
[0019] In addition, the method for preparing the outer cavity coating according to the above embodiment of the present invention may also have the following additional technical features:
[0020] In some embodiments of the present invention, step (1) includes: (1-1) mixing the silicone resin with the solvent to form a first mixed liquid; (1-2) mixing the first mixed liquid with the cross-linking agent to form a second mixed liquid; (1-3) mixing the second mixed liquid with the anti-fingerprint agent to form the coating liquid.
[0021] In some embodiments of the present invention, the temperature of the heat treatment is 25°C-450°C.
[0022] In a fourth aspect of the present invention, the present invention provides a micro-baking device. According to an embodiment of the present invention, the micro-baking device has an outer cavity coating of the above embodiment or an outer cavity coating prepared by the method described in the above embodiment. Therefore, the micro-baking device has all the advantages of the outer cavity coating of the above embodiment. Specifically, the outer cavity of the micro-baking device has excellent high temperature resistance, boiling resistance and moisture and heat resistance, thereby extending the service life of the micro-baking device. At the same time, it also has excellent anti-fingerprint performance, further meeting the needs of consumers.
[0023] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0025] Figure 1 The figure is a schematic flow chart of a method for preparing an outer cavity coating according to an embodiment of the present invention. DETAILED DESCRIPTION
[0026] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.
[0027] In one aspect of the present invention, the present invention provides a composition. According to an embodiment of the present invention, the composition is used to prepare an outer cavity coating, and the composition includes: 14-73 parts by weight of silicone resin (e.g., 15 / 20 / 30 / 40 / 50 / 60 / 70 parts by weight), 5-53 parts by weight of anti-fingerprint auxiliary agent (e.g., 5 / 10 / 15 / 20 / 25 / 30 / 35 / 40 / 45 / 50 parts by weight), 0.5-24 parts by weight of cross-linking auxiliary agent (e.g., 0.5 / 1 / 5 / 10 / 15 / 20 / 24 parts by weight), and 20-63 parts by weight of solvent (e.g., 20 / 25 / 30 / 35 / 40 / 45 / 50 / 55 / 60 parts by weight). Therefore, the outer cavity coating formed by the composite system not only has excellent high temperature resistance, boiling water resistance and moisture and heat resistance, but also can effectively prevent high temperature oxidation and corrosion of the substrate; at the same time, the outer cavity coating formed by the composite system also has excellent anti-fingerprint performance.
[0028] The principle by which the outer cavity coating proposed by the present invention can achieve the above beneficial effects is described in detail below:
[0029] In the prior art, the outer cavity coating of microwave ovens, ovens and other micro-baking products has the following disadvantages: 1) poor anti-fingerprint performance, oil stains attached to its surface cannot be removed; 2) poor moisture and heat resistance, rust and discoloration occur in an environment with a temperature of 60°C and a humidity of 93% within 5 hours; 3) poor water boiling resistance, whitening or even falling off in a short period of time (30 minutes or more); 4) poor high temperature resistance, yellowing and cracking occur after baking in a 300°C environment for 1 hour. In order to solve the above problems, the present invention provides a composition for preparing an outer cavity coating, the composition comprising 14-73 parts by weight of silicone resin, 5-53 parts by weight of anti-fingerprint additive, 0.5-24 parts by weight of cross-linking additive and 20-63 parts by weight of solvent. Silicone resin is a thermosetting polysiloxane polymer with a highly cross-linked structure, which has excellent electrical insulation, heat resistance and water resistance, and silicone resin has good adhesion to iron, aluminum, silver, tin, glass and ceramics. The inventors added a crosslinking agent and an anti-fingerprint agent to the silicone resin to make the whole system undergo a crosslinking reaction, which not only makes the outer cavity coating formed by the composition system have excellent high temperature resistance, water boiling resistance and moisture and heat resistance, but also effectively prevents the substrate from high temperature oxidation and corrosion; at the same time, the outer cavity coating formed by the composition system has excellent anti-fingerprint performance, no fingerprints left when touched by fingers, and easy to clean oil stains. Specifically, the outer cavity coating formed by the composition system is resistant to high temperatures ≥300°C, resistant to water boiling ≥30 hours, and resistant to moisture and heat ≥18 hours.
[0030] The inventors found that if the content of the anti-fingerprint auxiliary agent is too low, it is not possible to effectively ensure that the outer cavity coating formed by the composition system has excellent anti-fingerprint performance. If the content of the anti-fingerprint auxiliary agent is too high, the boiling resistance and moisture and heat resistance of the outer cavity coating formed by the composition system will decrease. If the content of the cross-linking auxiliary agent is too low, it will not be possible to ensure the cross-linking effect of the entire system, thereby causing the anti-fingerprint performance, moisture and heat resistance, and boiling resistance of the outer cavity coating formed by the composition system to decrease. If the content of the cross-linking auxiliary agent is too high, the leveling of the outer cavity coating formed by the composition system will deteriorate (for example, problems such as pinholes and orange peels will occur).
[0031] According to some specific embodiments of the present invention, the composition includes: 20-60 parts by weight of silicone resin, 6-32 parts by weight of anti-fingerprint additive, 0.5-18 parts by weight of cross-linking additive and 32-60 parts by weight of solvent. By limiting the content of each component within the above range, the high temperature resistance, boiling resistance and moisture and heat resistance of the outer cavity coating formed by the composition system are further improved, and high temperature oxidation and corrosion of the substrate are further effectively prevented; at the same time, the anti-fingerprint performance of the outer cavity coating formed by the composition system is further improved.
[0032] In the embodiments of the present invention, the specific types of the above-mentioned silicone resins are not particularly limited, and those skilled in the art can flexibly select according to actual needs. As some specific examples, the silicone resin includes at least one of methylphenyl silicone resin, methyl silicone resin, epoxy-modified silicone resin, silicone polyester-modified resin, benzyl transparent silicone resin, mica bonding silicone resin, amino silicone resin, fluorosilicone resin, silicone-epoxy resin, and silicone polyester resin. It should be noted that the performance of silicone resin is also closely related to the type of organic group R on the silicone resin. When the organic group is -CH3, the thermal stability, hydrophobicity, demolding property and arc resistance of the silicone resin can be improved; when the organic group is -C6H5, the oxidative stability and thermal stability of the silicone resin can be improved; when the organic group is -CH=CH2, the curing performance of the silicone resin can be improved and the coupling property can be imparted; when the organic group is phenyl or ethyl, the miscibility of the silicone resin with organic matter can be improved; when the organic group is -NH2(CH2), the water solubility of the polymer can be improved and the coupling property can be imparted at the same time; when the organic group is a long-chain alkyl group, the hydrophobicity of the silicone resin can be improved.
[0033] In the embodiments of the present invention, the specific types of the anti-fingerprint auxiliary agent are not particularly limited, and those skilled in the art can flexibly select according to actual needs. As some specific examples, the anti-fingerprint auxiliary agent includes at least one of methyltriethoxysilane, tetraethoxysilane, polyether-modified silicone, isocyanate-modified silicone, acrylic copolymer and siloxane-modified polyurethane. The anti-fingerprint auxiliary agent of the above type is added to the silicone resin system, so that the outer cavity coating formed by the system has excellent anti-fingerprint performance, does not leave fingerprints when touched by fingers, and is easy to clean oil stains.
[0034] In the embodiments of the present invention, the specific types of the above cross-linking aids are not particularly limited, and those skilled in the art can flexibly select according to actual needs. As some specific examples, the cross-linking aids include at least one of polycarbodiimide cross-linking aids, acrylate cross-linking aids, organic peroxide cross-linking aids, polyamine cross-linking aids, polyol cross-linking aids, glycidyl ether cross-linking aids, silicone cross-linking aids, benzenesulfonic acid cross-linking aids, aziridine cross-linking aids, olefin monomer cross-linking aids and inorganic cross-linking aids. Among them, the specific types of polyamine cross-linking aids are not particularly limited, for example, the polyamine cross-linking aids include at least one of propylene diamine and MOCA. The specific types of polyol cross-linking aids are not particularly limited, for example, the polyol cross-linking aids include at least one of polyethylene glycol, polypropylene glycol, trimethylol propane, and trimethylol ethane. The specific types of inorganic cross-linking aids are not particularly limited, for example, the inorganic cross-linking aids include at least one of zinc oxide, aluminum chloride and aluminum sulfate. The specific types of organosilicon crosslinking aids are not particularly limited. For example, organosilicon crosslinking aids include at least one of ethyl orthosilicate, methyl orthosilicate and trimethoxysilane. The specific types of benzenesulfonic acid crosslinking aids are not particularly limited. For example, benzenesulfonic acid crosslinking aids include at least one of p-toluenesulfonic acid and p-toluenesulfonyl chloride. The specific types of acrylate crosslinking aids are not particularly limited. For example, acrylate crosslinking aids include at least one of dibutylene glycol diacrylate, ethylene glycol dimethacrylate, TAC, butyl acrylate, HEA, HPA, HEMA, HPMA and MMA. The specific types of organic peroxide crosslinking aids are not particularly limited. For example, organic peroxide crosslinking aids include at least one of diisopropylbenzene peroxide and di-2,4-dichlorobenzoyl peroxide. The specific types of vinyl monomer crosslinking aids are not particularly limited. For example, the vinyl monomer crosslinking aids include at least one of acrylic acid, hydroxyethyl acrylate, hydroxypropyl acrylate, methacrylic acid, hydroxyethyl methacrylate, hydroxypropyl methacrylate, divinylbenzene, N-hydroxymethyl acrylamide, and diacetone acrylamide.
[0035] In the embodiments of the present invention, the specific types of the above-mentioned solvents are not particularly limited, and those skilled in the art can flexibly select according to actual needs. As some specific examples, the solvent includes at least one of an alkane solvent, an ether solvent, a ketone solvent, and a benzene-derived biological solvent. Among them, the specific types of hydrocarbon solvents are not particularly limited. For example, the alkane solvent includes at least one of n-hexane, n-octane, n-decane, chloroform, dichloromethane, dichloroethylene, and mineral oil. The specific types of ether solvents are not particularly limited. For example, the ether solvent includes at least one of ether, petroleum ether, and dibutyl ether. The specific types of ketone solvents are not particularly limited. For example, the ketone solvent includes at least one of acetone, methyl ethyl ketone, cyclohexanone, and isophorone. The specific types of benzene derivative solvents are not particularly limited. For example, the benzene derivative solvent includes at least one of toluene, m-xylene, p-xylene, o-xylene, and chlorobenzene.
[0036] In another aspect of the present invention, the present invention proposes an outer cavity coating. According to an embodiment of the present invention, the outer cavity coating is prepared using the composition of the above embodiment. As a result, the outer cavity coating has relatively excellent high temperature resistance, boiling resistance and moisture and heat resistance, and can also effectively prevent high temperature oxidation and corrosion of the substrate; at the same time, the outer cavity coating also has excellent anti-fingerprint performance, no fingerprints are left when touched by fingers, and oil stains are easy to clean. Specifically, the outer cavity coating is resistant to high temperatures ≥300°C, resistant to boiling water ≥30 hours, and resistant to moisture and heat ≥18 hours.
[0037] In the third aspect of the present invention, the present invention provides a method for preparing the above-mentioned outer cavity coating. Figure 1 , the method comprising:
[0038] S100: mixing silicone resin, anti-fingerprint auxiliary agent, cross-linking auxiliary agent and solvent to form a coating liquid.
[0039] According to some specific embodiments of the present invention, step S100 includes the following steps: first, fully mixing the silicone resin and the solvent to form a first mixed solution; then, fully mixing the cross-linking agent in the first mixed solution to form a second mixed solution; and finally, fully mixing the anti-fingerprint agent in the second mixed solution to finally form a coating solution. In this way, the components are mixed more fully, and the side reactions that may be caused by the silicone resin and the anti-fingerprint agent first contact are avoided.
[0040] S200: forming a coating liquid on a substrate and performing a heat treatment to form an outer cavity coating on the substrate.
[0041] During the heat treatment process, a cross-linking reaction occurs in the entire system, causing the coating liquid to solidify to form an outer cavity coating. The outer cavity coating formed not only has excellent high temperature resistance, water boiling resistance and moisture and heat resistance, but also can effectively prevent high temperature oxidation and corrosion of the substrate; at the same time, the outer cavity coating formed also has excellent anti-fingerprint properties, leaving no fingerprints when touched by fingers, and oil stains are easy to clean.
[0042] According to some specific embodiments of the present invention, the temperature of the heat treatment is 25°C-450°C, preferably 150°C-340°C; the time of the heat treatment is 5 min-30 min, preferably 10 min-20 min.
[0043] According to the method for preparing the above-mentioned outer cavity coating according to an embodiment of the present invention, the outer cavity coating prepared by the method has relatively excellent high temperature resistance, boiling resistance and moisture and heat resistance, and can also effectively prevent high temperature oxidation and corrosion of the substrate; at the same time, it also has excellent anti-fingerprint performance, no fingerprints left when touched by fingers, and easy to clean oil stains. Specifically, the outer cavity coating is resistant to high temperatures ≥300°C, resistant to boiling water ≥30 hours, and resistant to moisture and heat ≥18 hours. The preparation method is simple in steps and easy to operate.
[0044] In a fourth aspect of the present invention, the present invention provides a micro-baking device. According to an embodiment of the present invention, the micro-baking device has an outer cavity coating of the above embodiment or an outer cavity coating prepared by the method described in the above embodiment. Therefore, the micro-baking device has all the advantages of the outer cavity coating of the above embodiment. Specifically, the outer cavity of the micro-baking device has excellent high temperature resistance, boiling resistance and moisture and heat resistance, thereby extending the service life of the micro-baking device. At the same time, it also has excellent anti-fingerprint performance, further meeting the needs of consumers.
[0045] Specifically, the microwave oven device may be a microwave oven, an oven or other types of microwave oven kitchen appliances.
[0046] The embodiments of the present invention are described in detail below. It should be noted that the embodiments described below are exemplary and are only used to explain the present invention, and cannot be interpreted as limiting the present invention. In addition, if not explicitly stated, all reagents used in the following embodiments are commercially available, or can be synthesized according to this article or known methods, and the reaction conditions not listed are also easily available to those skilled in the art.
[0047] Example 1
[0048] At room temperature, 46 parts by weight of toluene solvent was added to 40 parts by weight of methylphenyl silicone resin, and the mixture was stirred for 30 minutes to obtain a first solution.
[0049] 9 parts by weight of a cross-linking aid, dicumyl peroxide, was added to the first solution and stirred evenly to obtain a second solution.
[0050] 19 parts by weight of anti-fingerprint auxiliary agent methyltriethoxysilane were added to the second solution and mixed evenly to obtain a coating solution.
[0051] The coating liquid was evenly sprayed on the surface of the substrate, and heat-treated at 210° C. for 10 min to obtain an anti-fingerprint coating.
[0052] Example 2
[0053] The weight proportion of the anti-fingerprint auxiliary agent in this embodiment is 6 parts, and the other contents are the same as those in Embodiment 1.
[0054] Example 3
[0055] The weight proportion of the anti-fingerprint auxiliary agent in this embodiment is 10 parts, and the other contents are the same as those in Embodiment 1.
[0056] Example 4
[0057] The weight proportion of the anti-fingerprint auxiliary agent in this embodiment is 15 parts, and the other contents are the same as those in Embodiment 1.
[0058] Example 5
[0059] The weight proportion of the anti-fingerprint auxiliary agent in this embodiment is 25 parts, and the other contents are the same as those in Embodiment 1.
[0060] Example 6
[0061] The weight proportion of the anti-fingerprint auxiliary agent in this embodiment is 40 parts, and the other contents are the same as those in Embodiment 1.
[0062] Example 7
[0063] The weight proportion of the anti-fingerprint auxiliary agent in this embodiment is 50 parts, and the other contents are the same as those in Embodiment 1.
[0064] Example 8
[0065] The weight portion of the cross-linking aid in this embodiment is 1 part, and the other contents are the same as those in Embodiment 1.
[0066] Example 9
[0067] The weight proportion of the crosslinking aid in this embodiment is 5 parts, and the other contents are the same as those in Embodiment 1.
[0068] Example 10
[0069] The weight proportion of the crosslinking aid in this embodiment is 15 parts, and the other contents are the same as those in Embodiment 1.
[0070] Embodiment 11
[0071] The weight proportion of the crosslinking aid in this embodiment is 18 parts, and the other contents are the same as those in Embodiment 1.
[0072] Example 12
[0073] The silicone resin used in this embodiment is methyl silicone resin, the weight portion of which is 20 parts, the cross-linking agent used is propylene diamine, the weight portion of the solvent is 20 parts, the anti-fingerprint agent used is polyether modified silicone, and the heat treatment is performed at 190° C. for 20 minutes. Other contents are the same as in Example 1.
[0074] Example 13
[0075] The silicone resin used in this embodiment is fluorosilicone resin, which has a weight portion of 30 parts, the weight portion of the solvent is 30 parts, the cross-linking agent used is polyethylene glycol, the anti-fingerprint agent used is isocyanate-modified silicone, and the heat treatment is performed at 150° C. for 20 minutes. Other contents are the same as in Example 1.
[0076] Embodiment 14
[0077] The silicone resin used in this embodiment is amino silicone resin, which has a weight portion of 50 parts, the weight portion of the solvent is 50 parts, the cross-linking agent used is zinc oxide, the anti-fingerprint agent used is acrylic copolymer, and the heat treatment is performed at 340°C for 10 minutes. Other contents are the same as those in Example 1.
[0078] Embodiment 15
[0079] The silicone resin used in this embodiment is an organosilicon-epoxy resin, and its weight proportion is 60 parts. The weight proportion of the solvent is 60 parts. The cross-linking agent used is 1,4-butylene glycol diacrylate. The anti-fingerprint agent used is siloxane-modified polyurethane. Other contents are the same as those in Example 1.
[0080] Comparative Example 1
[0081] In this comparative example, no anti-fingerprint additive is added, and other contents are the same as those in Example 1.
[0082] Comparative Example 2
[0083] The weight portion of the anti-fingerprint auxiliary agent added in this comparative example is 2 parts, and the other contents are the same as those in Example 1.
[0084] Comparative Example 3
[0085] The weight portion of the anti-fingerprint auxiliary agent added in this comparative example is 57 parts, and the other contents are the same as those in Example 1.
[0086] The anti-fingerprint performance, boiling water resistance, moisture and heat resistance, and temperature resistance of the anti-fingerprint coatings prepared in Examples 1-15 and Comparative Examples 1-3 were tested respectively, and the specific testing methods are as follows:
[0087] Anti-fingerprint performance: The coating liquids prepared in Examples 1-15 and Comparative Examples 1-3 were sprayed on the same substrate respectively. After curing, the surface was pressed with a thumb. The thumb was removed after staying for 10 seconds each time to observe whether there were fingerprints. This was repeated 10 times. If there were no fingerprints on the coating surface, the anti-fingerprint performance was excellent; if there were slight fingerprints that could be wiped off with a tissue, the anti-fingerprint performance was good; if there were partial fingerprints that could be wiped off, the anti-fingerprint performance was qualified; if there were many fingerprints or the fingerprints could not be wiped off, the anti-fingerprint performance was unqualified.
[0088] Water boiling resistance: The coating liquids prepared in Examples 1-15 and Comparative Examples 1-3 were sprayed on the same substrate respectively, and the samples were placed in water boiling vessels after curing. After continuous boiling for 30 hours, if the coating did not fall off and the color difference ⊿E before and after boiling was in the range of 0 to 0.25, the water boiling resistance was excellent; if the coating did not fall off and the color difference ⊿E before and after boiling was in the range of 0.25 to 0.5, the water boiling resistance was good; if the coating did not fall off and the color difference ⊿E before and after boiling was in the range of 0.5 to 1.0, the water boiling resistance was qualified; if the coating fell off, or the coating did not fall off and the color difference ⊿E before and after boiling was in the range of 1.0 to 1.5, the water boiling resistance was unqualified.
[0089] Moisture and heat resistance: The coating solutions prepared in Examples 1-15 and Comparative Examples 1-3 were sprayed on the same substrate respectively. After curing, the samples were placed in an environment with a temperature of 60°C and a humidity of 93% for 18 hours. If the coating did not fall off and the color difference ⊿E before and after the test was in the range of 0 to 0.25, the moisture and heat resistance was excellent; if the coating did not fall off and the color difference ⊿E before and after the test was in the range of 0.25 to 0.5, the moisture and heat resistance was good; if the coating did not fall off and the color difference ⊿E before and after the test was in the range of 0.5 to 1.0, the moisture and heat resistance was qualified; if the coating fell off, or the coating did not fall off and the color difference ⊿E before and after the test was in the range of 1.0 to 1.5, the moisture and heat resistance was unqualified.
[0090] Heat resistance: Spray the coating liquids prepared in Examples 1-15 and Comparative Examples 1-3 on the same substrate, respectively. After curing, place the samples in a high-temperature oven, set the temperature to 300°C, keep warm for 6 hours, take out and cool to room temperature, and observe whether there is cracking or discoloration. If the coating has no cracks and the color difference ⊿E before and after the high-temperature test is within the range of 0 to 0.25, the heat resistance is excellent; if the coating has no cracks and the color difference ⊿E before and after the high-temperature test is within the range of 0.25 to 0.5, the heat resistance is good; if the coating has no cracks and the color difference ⊿E before and after the high-temperature test is within the range of 0.5 to 1.0, the heat resistance is qualified; if the coating cracks, or if the coating has no cracks and the color difference ⊿E before and after the high-temperature test is within the range of 1.0 to 1.5, the heat resistance is unqualified.
[0091] The test results are shown in Table 1.
[0092] Table 1
[0093]
[0094]
[0095] It can be seen from Table 1 that Examples 1-15 all have excellent anti-fingerprint performance, water boiling resistance, moisture and heat resistance, and temperature resistance.
[0096] It can also be seen from Table 1 that the anti-fingerprint performance of Comparative Example 1 is poor, while Example 1 has excellent anti-fingerprint performance.
[0097] It can also be seen from Table 1 that, compared with Example 1, the anti-fingerprint performance of Comparative Example 2 is relatively poor.
[0098] It can also be seen from Table 1 that, compared with Example 1, the boiling water resistance and moisture heat resistance of Comparative Example 3 are relatively poor.
[0099] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0100] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A composition for preparing an outer cavity coating, characterized in that: The composition comprises: 14-73 parts by weight of silicone resin, 5-53 parts by weight of anti-fingerprint auxiliary agent, 0.5-24 parts by weight of cross-linking auxiliary agent and 20-63 parts by weight of solvent.
2. The composition according to claim 1, characterized in that The composition comprises: 20-60 parts by weight of the silicone resin, 6-32 parts by weight of the anti-fingerprint auxiliary agent, 0.5-18 parts by weight of the cross-linking auxiliary agent and 32-60 parts by weight of the solvent.
3. The composition according to claim 1 or 2, characterized in that The anti-fingerprint auxiliary agent includes at least one of methyltriethoxysilane, tetraethoxysilane, polyether-modified silicone, isocyanate-modified silicone, acrylic copolymer and siloxane-modified polyurethane.
4. The composition according to claim 1 or 2, characterized in that The silicone resin includes at least one of methylphenyl silicone resin, methyl silicone resin, epoxy-modified silicone resin, silicone polyester-modified resin, benzyl transparent silicone resin, mica bonding silicone resin, amino silicone resin, fluorosilicone resin, silicone-epoxy resin, and silicone polyester resin.
5. The composition according to claim 1 or 2, characterized in that The crosslinking aid includes at least one of a polycarbodiimide crosslinking aid, an acrylate crosslinking aid, an organic peroxide crosslinking aid, a polyamine crosslinking aid, a polyol crosslinking aid, a glycidyl ether crosslinking aid, a silicone crosslinking aid, a benzenesulfonic acid crosslinking aid, an aziridine crosslinking aid, an olefin monomer crosslinking aid and an inorganic crosslinking aid.
6. The composition according to claim 5, characterized in that The polyamine cross-linking aid includes at least one of propylene diamine and MOCA; And / or, the polyol cross-linking aid includes at least one of polyethylene glycol, polypropylene glycol, trimethylolpropane and trimethylolethane; And / or, the inorganic cross-linking aid includes at least one of zinc oxide, aluminum chloride and aluminum sulfate; And / or, the organosilicon cross-linking aid includes at least one of ethyl orthosilicate, methyl orthosilicate and trimethoxysilane; And / or, the benzenesulfonic acid cross-linking aid includes at least one of p-toluenesulfonic acid and p-toluenesulfonyl chloride; and / or, the acrylate crosslinking aid comprises at least one of 1,4-butylene glycol diacrylate, ethylene glycol dimethacrylate, TAC, butyl acrylate, HEA, HPA, HEMA, HPMA and MMA; And / or, the organic peroxide cross-linking aid includes at least one of dicumyl peroxide and bis-2,4-dichlorobenzoyl peroxide; And / or, the vinyl monomer crosslinking aid includes at least one of acrylic acid, hydroxyethyl acrylate, hydroxypropyl acrylate, methacrylic acid, hydroxyethyl methacrylate, hydroxypropyl methacrylate, divinylbenzene, N-hydroxymethyl acrylamide, and diacetone acrylamide.
7. The composition according to claim 1 or 2, characterized in that The solvent includes at least one of an alkane solvent, an ether solvent, a ketone solvent and a benzene-derived biosolvent.
8. An outer cavity coating, characterized in that: The composition is prepared by using the composition described in any one of claims 1 to 7.
9. A method for preparing the outer cavity coating according to claim 8, characterized in that: include: (1) mixing a silicone resin, an anti-fingerprint additive, a cross-linking additive, and a solvent to form a coating solution; (2) The coating liquid is formed on a substrate and heat-treated to form the outer cavity coating on the substrate.
10. The method according to claim 9, characterized in that Step (1) comprises: (1-1) mixing the silicone resin and the solvent to form a first mixed liquid; (1-2) mixing the first mixed solution with the cross-linking auxiliary agent to form a second mixed solution; (1-3) The second mixed liquid is mixed with the anti-fingerprint auxiliary agent to form the coating liquid.
11. The method according to claim 9, characterized in that The temperature of the heat treatment is 25°C-450°C.
12. A microwave oven, characterized in that: An outer cavity coating according to claim 8 or an outer cavity coating prepared by the method of any one of claims 9 to 11.
Citation Information
Patent Citations
Coating composition
CN101338158A
Anti-fingerprint finish varnish
CN107245278A
Self-cleaning paint composition, paint, coating of paint and kitchen electric appliances
CN110373107A
High-shielding fingerprint-resistant backlight module reflecting film and preparation process thereof
CN111694080A
High-temperature-resistant paint composition, high-temperature-resistant paint, preparation method and application of high-temperature-resistant paint, and high-temperature-resistant coating
CN113174198A