Inorganic slurry as well as preparation method and application thereof

By developing inorganic slurries suitable for the spot coating process and using specific ratios of dispersants and binders, the problems of nozzle clogging, solid-liquid separation and coverage control of the inorganic coating liquid in the lithium battery separator coating process have been solved, achieving A battery separator with high air permeability and low water content improves battery performance and safety.

CN118801042AActive Publication Date: 2024-10-18HEBEI GELLEC NEW ENERGY MATERIAL SCI&TECHNOLOY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410786790.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-18
Estimated Expiration
2044-06-18

AI Technical Summary

Technical Problem

The existing lithium battery separator coating process cannot effectively adapt to the characteristics of the inorganic coating fluid, resulting in nozzle clogging, solid-liquid separation, coating leakage and scratches. It is also unable to achieve controllable coverage and air permeability, affecting battery performance and safety. sex.

Method used

Develop an inorganic slurry that contains dispersant, wetting agent, ceramic powder, thickener and binder. The inorganic slurry is formulated according to a specific ratio and is coated on the lithium battery separator through a spot coating process. Utilize The selection and proportioning of the binder controls the tension and centrifugal force to form uniform, circular coating points, which solves the problem of particles in the coating liquid and the lack of air permeability.

Benefits of technology

It realizes the effective transfer and coating of inorganic slurry in the spot coating process, forming a battery separator with high air permeability and low water content, avoiding coating leakage and scratches, reducing costs, and improving the appearance and performance of the battery separator. , extending the cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118801042A_ABST
    Figure CN118801042A_ABST
Patent Text Reader

Abstract

The invention discloses inorganic slurry and a preparation method and application thereof.The inorganic slurry is prepared from a dispersing agent, a wetting agent, ceramic powder, a thickening agent and a bond.The inorganic slurry is prepared by selecting the bonder and adjusting the proportion of the bonder; the inorganic slurry can better meet the requirements for tension and centrifugal force when the dispensing plate roller transfers the slurry in the dispensing process, deformation is effectively controlled in the slurry transferring process, and when the inorganic slurry is coated to a base film, the wrapping effect of formed hemispherical liquid drops is better, and the shape of a coating point is closer to a circle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery separators, and in particular relates to an inorganic slurry and a preparation method and application thereof. Background Art

[0002] With the rapid update of electronic products and the rapid expansion of new energy electric vehicles in the market, lithium batteries, as an important energy storage device with high energy density and long life, are increasingly attracting the attention of producers and users. One of the core components of lithium batteries is the diaphragm, which can effectively isolate the positive and negative electrodes, prevent short circuits and electrolyte impregnation, thereby ensuring the safety and performance stability of lithium batteries. Compared with PP or PE base films, coating films have better high temperature stability, chemical stability, and higher mechanical strength and toughness. Therefore, the lithium battery diaphragm coating process is crucial to the performance and service life of lithium batteries.

[0003] The commonly used diaphragm coating processes at present include roller coating, spray coating, scraper coating and rotary spray coating. Due to process limitations, a single diaphragm coating process cannot meet the needs of all coating materials. Among them, roller coating can be applied to most coating materials because of its relatively simple process, stable coating effect and easy operation.

[0004] Taking inorganic coating liquid as an example, most inorganic coating liquids are made of inorganic compounds such as alumina and boehmite, which have large particles or impurities. Because of their large particles, high specific gravity, and high hardness, they are prone to scratches and coating leaks. There is no problem with the use of inorganic coating liquid in roller coating, but if it is used in spraying, it is easy to cause nozzle blockage due to the large particles of the inorganic coating liquid; if it is used in rotary spraying, it is easy to cause solid-liquid separation during the rotary spraying process due to its high specific gravity. When the inorganic coating liquid is coated 100% on the surface of the diaphragm, the coating thickness is too large or the coating liquid density is high, which will affect the air permeability of the finished membrane, and thus affect the ion penetration.

[0005] At present, a new contact partial coating method, spot coating, is emerging. It does not have the clogging and solid-liquid separation problems of spraying, nor does it have to worry about missing coating or scratches due to large particles in the coating liquid. In addition, because spot coating is planned to achieve controllable coverage on the diaphragm, the air permeability problem caused by its thickness and coating liquid density can also be solved. And its finished product has the same characteristics as roller coating products in testing and use, so it has more advantages.

[0006] However, the principle of transferring slurry by spot coating and conventional roller coating is different. Most of the main materials of slurry currently used in spot coating are PVDF, because PVDF particles are lighter than ceramic particles in the same volume, the slurry has a smaller specific gravity, and it has good adhesion. When applied to the spot coating process, it can overcome the centrifugal force of the plate roller, so that the slurry does not undergo large deformation during the transfer process. However, compared with ceramic slurry, PVDF has a lower hardness, a higher price, and is not as environmentally friendly as ceramics. Therefore, the development of ceramic spot coating slurry is also very important to meet different needs. However, conventional ceramic slurry (inorganic slurry) cannot adapt to the spot coating process because of its high specific gravity and lack of adhesion between powders. Therefore, it is necessary to prepare an inorganic slurry that can meet the spot coating process. Summary of the invention

[0007] In view of the shortcomings of the prior art, the present invention aims to provide an inorganic slurry.

[0008] Another object of the present invention is to provide a method for preparing the above-mentioned inorganic slurry.

[0009] Another object of the present invention is to provide application of the above inorganic slurry in spot coating.

[0010] The purpose of the present invention is achieved through the following technical solutions.

[0011] An inorganic slurry comprises: a dispersant, a wetting agent, a ceramic powder, a thickener and a binder. Calculated by mass, the ratio of the dispersant, the wetting agent, the ceramic powder, the thickener and the binder is (0.5-1.0): (2.0-2.5): (15-20): (15-18): (15-25).

[0012] The above technical solution also includes: water, in which the ratio of the ceramic powder to water is (15-20): (45-55) by mass.

[0013] In the above technical solution, the binder is one or a mixture of methyl methacrylate copolymer, acrylate copolymer and styrene-butyl methacrylate.

[0014] In the above technical solution, the dispersant is ammonium polyacrylate.

[0015] In the above technical solution, the ceramic powder is an inorganic substance with thermal stability and chemical inertness.

[0016] In the above technical solution, the ceramic powder is a metal oxide, hydroxide, nitride, hydrated oxide or inorganic polymer.

[0017] In the above technical solution, the metal oxide is aluminum oxide, silicon oxide, zirconium oxide or titanium oxide; the hydroxide is magnesium hydroxide; the nitride is aluminum nitride; the hydrated oxide is boehmite; and the inorganic polymer is nano-silicon.

[0018] In the above technical solution, the wetting agent is an inorganic wetting agent.

[0019] In the above technical solution, the inorganic wetting agent is sodium tripolyphosphate.

[0020] In the above technical solution, the thickener is hydroxymethyl cellulose.

[0021] In the above technical solution, the viscosity of the inorganic slurry is 100-200 cp.

[0022] A method for preparing an inorganic slurry comprises: mixing ceramic powder, water and a dispersant until uniform, sand-milling to obtain a first solution, mixing the first solution, a thickener, a binder and a wetting agent, stirring until uniform, and obtaining an inorganic slurry, wherein the ratio of the dispersant, the wetting agent, the ceramic powder, the thickener, the binder and the water is (0.5-1.0): (2.0-2.5): (15-20): (15-18): (15-25): (45-55) by mass.

[0023] In the above technical solution, the method for mixing ceramic powder, water and dispersant until they are uniform is: stirring the ceramic powder, water and dispersant at a rotation speed of 1800-2200 r / min and a revolution speed of 30-50 r / min for 60-70 minutes.

[0024] In the above technical solution, the sanding time is 12 to 30 minutes.

[0025] Application of inorganic slurry in spot coating.

[0026] In the above technical solution, the inorganic slurry is coated on the base film by spot coating and dried to obtain a battery separator.

[0027] In the above technical solution, the drying time is 1 to 3 minutes, and the drying temperature is 45 to 60°C.

[0028] In the above technical solution, the coating speed is 50-150 m / min.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] 1. The inorganic slurry of the present invention can better meet the requirements of tension and centrifugal force when the dot coating roller transfers the slurry during the dot coating process by selecting the binder and adjusting the ratio of the binder, effectively control the deformation during the slurry transfer process, and can also make the hemispherical droplets formed when the inorganic slurry is coated on the base film have a better wrapping effect, and the shape of the coating point is closer to a circle;

[0031] 2. The inorganic slurry of the present invention is applied to the spot coating process to solve the problem that roller coating cannot achieve controllable coverage and spray coating cannot coat the inorganic slurry, and can improve the problem of high air permeability of roller coating inorganic slurry;

[0032] 3. The inorganic slurry of the present invention can be applied to the spot coating process to improve the appearance of the battery separator, and effectively avoid the defects of missing coating, scratches and large material spots caused by the presence of large particles in the slurry;

[0033] 4. Spot coating is non-whole-surface coating, which can save slurry and reduce costs compared to roller coating. Compared with roller coating, spot coating leaves much less slurry on the base film, making the water content of the diaphragm relatively low, reducing the amount of water and lithium reacting, reducing the gas generated, and reducing the risk of explosion due to high internal gas pressure in the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 is a cross-sectional view of a battery separator obtained by spot coating;

[0035] Figure 2 This is a photo of the battery separator obtained by spot coating in Example 2;

[0036] Figure 3 This is a photo of the battery separator obtained by roller coating in Example 2;

[0037] Figure 4 This is a photo of the battery separator obtained by roller coating in Example 2;

[0038] Figure 5 A schematic diagram of a method for measuring coverage;

[0039] Figure 6 This is the OM appearance of the battery separator in Example 5. DETAILED DESCRIPTION

[0040] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0041] The raw material information involved in the following examples is as follows:

[0042] Sodium tripolyphosphate: It is an amorphous water-soluble linear polyphosphate with the chemical formula of Na5P3O 10, belongs to inorganic compounds. It is a white powdery crystal with good fluidity, easily soluble in water, and its aqueous solution is alkaline.

[0043] Alumina: It is an inorganic substance with the chemical formula of AL2O3, and has the characteristics of high melting point, high thermal conductivity and high corrosion resistance. Its melting point is 2054℃, boiling point is 2980℃, it can be ionized at high temperature, it is an ionic crystal, and it is a white amorphous powder. It is insoluble in water, but easily soluble in strong alkali and strong acid.

[0044] Acrylate copolymer: a general term for polymers produced by copolymerization reaction of acrylate (mainly methyl acrylate, ethyl acrylate, butyl acrylate and methyl methacrylate) as raw materials. Acrylate has active double bonds and is easy to self-polymerize and copolymerize. The copolymerization monomer can be one or more; it can be another acrylic compound or other unsaturated compound with double bonds (mainly styrene, acrylonitrile, vinyl acetate, vinyl chloride, etc.).

[0045] Friction powder loss: Take a battery separator with a size of 30*250mm, weigh it and record it as a (mg), place the battery separator in a powder loss rate tester, use the pressure measurement method, the test time is 30s, after the test, weigh it and record it as b (mg), the friction powder loss c = (ab).

[0046] Air permeability value added: battery separator air permeability value - base membrane air permeability value.

[0047] Ionic conductivity: The test temperature is 25±5℃ and the relative humidity is 60%RH.

[0048] In the following examples, the base film has a thickness of 9 μm and a width of 1000 mm.

[0049] Example 1

[0050] A method for preparing an inorganic slurry comprises: mixing ceramic powder, pure water and a dispersant, stirring the mixture in a planetary stirring device at a rotation speed of 2000 r / min and a revolution speed of 35 r / min for 60 min until the mixture is uniform, sand-milling the mixture for 15 min to obtain a first solution, mixing the first solution, a thickener, a binder and a wetting agent, stirring the mixture in a planetary stirring device at a rotation speed of 1500 r / min and a revolution speed of 20 r / min for 10 min until the mixture is uniform, to obtain an inorganic slurry, wherein the viscosity of the inorganic slurry is 100 cp, and the ratio of the dispersant, the wetting agent, the ceramic powder, the thickener, the binder and the pure water is 0.7:2.3:15:15:21:46 in terms of mass fractions, the binder is an acrylate copolymer, the dispersant is polyacrylate ammonium salt, the ceramic powder is alumina, the wetting agent is sodium tripolyphosphate, and the thickener is hydroxymethyl cellulose.

[0051] Example 2

[0052] The inorganic slurry in Example 1 was coated on one side of a base film with a length of 3000 m at a speed of 120 m / min, and the inorganic slurry formed a coating on the base film, which was dried at 50° C. for 2 min to obtain a battery separator, wherein the coating method was one of spot coating and roller coating, the coating thickness was 2 μm, and the effective coating width was 800 mm. The coverage of the spot coating was controlled at 20±5%.

[0053] Before coating, two barrels (200 kg per barrel) of the inorganic slurry in Example 1 were prepared, one barrel each for roller coating and spot coating. After roller coating, 55.6 kg of inorganic slurry remained, and after spot coating, 171.2 kg of inorganic slurry remained.

[0054] 10 points were randomly selected on each of the battery separators obtained by spot coating and the battery separators obtained by roller coating, and the thickness, air permeability, coating amount, adhesion, ionic conductivity and friction powder loss of the battery separators at each point were measured. The thickness increment was obtained by calculating the thickness of the battery separator. The thickness increment and coating amount are shown in Table 1. The average values ​​of the thickness, thickness increment, air permeability increment, coating amount, adhesion, ionic conductivity and friction powder loss of the battery separators at 10 points of the battery separators obtained by spot coating / roller coating are shown in Table 2.

[0055] Table 1

[0056]

[0057] It can be seen from Table 1 that in terms of coating thickness and uniformity, spot coating is slightly better than roller coating, and in terms of coating amount, spot coating is much less than roller coating.

[0058] Table 2

[0059]

[0060]

[0061] It can be seen from Table 2 that for the same coating thickness, the coating amount of spot coating is much smaller than that of roller coating, which saves a lot of inorganic slurry and thus reduces costs; and the battery separator obtained by spot coating has better air permeability, adhesion and friction powder loss than the battery separator obtained by roller coating.

[0062] Observe the appearance of the battery separator obtained by spot coating and the battery separator obtained by roller coating: it is found that there are two places where the battery separator obtained by roller coating has missed coating: one is that the bottom film is uneven (such as Figure 3 As shown), one is the large particles in the inorganic slurry (such as Figure 4There is also a spot of material (caused by impurities in the coating liquid). The battery separator obtained by spot coating does not have such defects, which shows that spot coating has relatively low requirements for the coating bottom film (base film), and it avoids the large particles that may exist in the inorganic slurry and will not affect the coating.

[0063] Example 3

[0064] The inorganic slurry in Example 1 was coated on one side of a base film with a length of 3000 m at a speed of 120 m / min, and the inorganic slurry formed a coating on the base film, which was dried at 50° C. for 2 min to obtain a battery separator, wherein the coating method was one of spot coating and roller coating, the coating thickness was 4 μm, and the effective coating width was 800 mm. The coverage of the spot coating was controlled at 20±5%.

[0065] 10 points were randomly selected on the battery separator obtained by spot coating and the battery separator obtained by roller coating, and the thickness and permeability of the battery separator at each point were measured. The thickness value-added was obtained by calculating the thickness of the battery separator, and the permeability value-added was obtained by calculating the permeability value of the battery separator. The thickness value-added and the permeability value-added are shown in Table 3.

[0066] Table 3

[0067]

[0068] It can be seen from Table 3 that when the thickness increment is about 4 μm, the air permeability increment of the battery separator coated by point coating is much smaller than that by roller coating, which is more conducive to ion penetration.

[0069] The present invention adopts a dot coating method to apply inorganic slurry to form a cylindrical inorganic support (such as Figure 1 ), the material of the contact electrode is a ceramic powder with high hardness, and the base film in the area not coated with inorganic slurry has no contact with the electrode, so that it can effectively prevent the lithium dendrites formed by long-term battery cycling from piercing the diaphragm and causing a short circuit (the same effect as ceramic roller coating). Because there is a large area of ​​gap between the base film and the electrode, the liquid retention and wettability of the battery diaphragm are greatly increased, thereby extending the cycle life of the lithium battery.

[0070] The inorganic slurry of the present invention can meet the requirement of transferring the slurry to the surface of the base film by the spot coating process, replacing the roller coating (roller coating is applied to the surface of the base film), and forming a Figure 2 The dot shape is neatly arranged in a matrix, and the dot area is controllable, that is, the coverage of the inorganic slurry on the base film is controllable. The coverage is measured as follows: Figure 5As shown, under low magnification microscope observation (such as 50X), the rectangular area a1 in the microscope field of view and the areas of 9 coating points in the rectangle are measured by "area mode", the sum of the areas of the 9 coating points is a2, and the coverage is a2 / a1. The inorganic slurry combined with the spot coating coating process of the present invention solves the problem that the inorganic slurry cannot be coated due to the equipment and coating method of spray coating, and solves the problem that the roller coating cannot achieve non-full coating.

[0071] Example 4 (for comparison)

[0072] A conventional ceramic slurry, which uses alumina as the main material, has the following preparation process: ceramic powder, pure water and a dispersant are mixed, stirred for 60 minutes at a rotation speed of 2000 r / min and a revolution speed of 40 r / min in a planetary stirring device until uniform, sand milled for 15 minutes to obtain a first solution, the first solution, a thickener and a binder are mixed, stirred for 10 minutes at a rotation speed of 1200 r / min and a revolution speed of 20 r / min in a planetary stirring device until uniform, to obtain an inorganic slurry, the viscosity of the inorganic slurry is 60 cp, the ratio of the dispersant, ceramic powder, thickener, binder and pure water is 3.0:17:13:20:47 by mass, the binder is methyl methacrylate copolymer, the dispersant is polyacrylate ammonium salt, the ceramic powder is alumina, and the thickener is hydroxymethyl cellulose.

[0073] The conventional ceramic slurry in Example 4 was coated on one side of a base film with a length of 3000 m at a speed of 120 m / min, and the coating method was spot coating, and the film was dried at 50°C for 2 min. The coating thickness was 2 μm, and the coverage of the spot coating was controlled at 20±5%. During the coating process, the anilox roller was normally loaded with liquid, but the conventional ceramic slurry could not be transferred to the plate roller normally, so it could not be coated on the base film.

[0074] Example 5

[0075] A method for preparing an inorganic slurry is basically the same as the “method for preparing an inorganic slurry” in Example 1, with the only difference being that “by mass, the ratio of dispersant, wetting agent, ceramic powder, thickener, binder and pure water is 0.7:2.3:15:15:21:46” is replaced by “by mass, the ratio of dispersant, wetting agent, ceramic powder, thickener, binder and pure water is 0.7:2.3:19:15:14:49”.

[0076] The inorganic slurry in Example 5 was coated on one side of a base film with a length of 3000 m at a speed of 120 m / min. The coating method was spot coating. The inorganic slurry formed a coating on the base film and dried at 50°C for 2 min to obtain a battery separator. The coating thickness was 2 μm and the coverage of the spot coating was controlled at 20±5%. The battery separator was observed under a microscope. The morphology was as follows: Figure 6 As shown, the coating points are irregular and do not meet the requirements of the diaphragm.

[0077] The present invention is described above by way of example. It should be noted that, without departing from the core of the present invention, any simple deformation, modification or other equivalent replacement that can be made by those skilled in the art without inventive effort falls within the protection scope of the present invention.

Claims

1. An inorganic slurry, characterized in that: include: The dispersant, wetting agent, ceramic powder, thickener and binder are present in a ratio of (0.5-1.0): (2.0-2.5): (15-20): (15-18): (15-25) by mass.

2. The inorganic slurry according to claim 1, characterized in that Also includes: Water, calculated by weight, the ratio of the ceramic powder to water is (15-20): (45-55).

3. The inorganic slurry according to claim 1 or 2, characterized in that: The binder is one or a mixture of methyl methacrylate copolymer, acrylate copolymer and styrene-butyl methacrylate.

4. The inorganic slurry according to claim 3, characterized in that: The dispersant is ammonium polyacrylate.

5. The inorganic slurry according to claim 3, characterized in that: The ceramic powder is metal oxide, hydroxide, nitride, hydrated oxide or inorganic polymer.

6. The inorganic slurry according to claim 3, characterized in that: The wetting agent is an inorganic wetting agent.

7. The inorganic slurry according to claim 6, characterized in that: The inorganic wetting agent is sodium tripolyphosphate, and the thickener is hydroxymethyl cellulose.

8. A method for preparing an inorganic slurry, characterized in that: include: Ceramic powder, water and dispersant are mixed until uniform, and sand-milled to obtain a first solution; the first solution, thickener, binder and wetting agent are mixed, and stirred until uniform to obtain an inorganic slurry; in terms of mass fractions, the ratio of the dispersant, wetting agent, ceramic powder, thickener, binder and water is (0.5-1.0): (2.0-2.5): (15-20): (15-18): (15-25): (45-55).

9. Use of the inorganic slurry as claimed in claim 1 or 2 in spot coating. 10 . A battery separator, comprising a base film and coating points covering the base film, each coating point comprising the inorganic slurry according to claim 1 .

Citation Information

Patent Citations

  • High-wettability long-circulation aluminum oxide ceramic slurry, preparation method and lithium battery diaphragm

    CN111019409A

  • Flame-retardant high-temperature-resistant slurry, preparation method and diaphragm coated with flame-retardant high-temperature-resistant slurry

    CN115939665A

  • Lithium ion battery ceramic coating slurry, coating diaphragm and preparation method thereof

    CN116283346A

  • Composite diaphragm as well as preparation method and application thereof

    CN116598708A

  • Inorganic coated polyolefin diaphragm capable of resisting wrinkling during liquid injection and preparation method of inorganic coated polyolefin diaphragm

    CN117039326A