Transition metal modified carbon nanotube accelerant, preparation method and CO2 trapping application
Using transition metal-modified carbon nanotubes as accelerators solves the problems of slow generation process and poor separation effect in hydrate CO2 capture technology, achieves efficient CO2 separation and recycling, and supports the green and low-carbon transformation of the ammonia synthesis industry.
Patent Information
- Application Number
- CN202410944387.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing hydrate CO2 capture technology in the synthetic ammonia industry has problems such as slow generation process and poor separation effect. Traditional kinetic accelerators are prone to foaming during the stirring process and are difficult to recycle, resulting in low CO2 separation efficiency.
Transition metal-modified carbon nanotubes are used as accelerators, and the hydrophilicity and CO2 adsorption performance of the carbon nanotubes are improved through hydrophilic functional group modification and transition metal loading, and high-temperature calcination is used to prepare carbon nanotubes with excellent kinetic acceleration effects. Transition metal loaded hydrophilic functionalized carbon nanotubes.
It achieves rapid generation of hydrates under mild conditions, improves the hydration rate and separation efficiency of CO2, and the accelerator can be recycled, reducing the energy consumption and cost of the synthetic ammonia industry, and supporting the green and low-carbon transformation of the synthetic ammonia industry.
Smart Images

Figure CN118807744A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of using a nano material hydrate kinetic promoter for decarbonization of synthetic ammonia, and specifically relates to a transition metal modified carbon nanotube promoter, a preparation method and CO2 capture application. Background Art
[0002] Ammonia is one of the most important basic chemical products and the foundation of my country's fertilizer industry. At present, the global nitrogen fertilizer production is about 120 million tons, and my country's synthetic ammonia industry production accounts for about 1 / 3 of the world's total production. Under the background of my country's "dual carbon", the synthetic ammonia industry with high energy consumption and high carbon emissions urgently needs green transformation. To produce synthetic ammonia, we must first produce raw gas containing a mixture of nitrogen and hydrogen. The main raw materials for synthetic ammonia production in my country are coal, supplemented by natural gas. According to the production needs of low-energy consumption and clean production of synthetic ammonia industry, natural gas is the most ideal raw material for synthetic ammonia production. On the one hand, the main component of natural gas, CH4, has high efficiency in obtaining raw gas H2. On the other hand, CH4 is the cleanest fossil energy, and its CO2 emissions are greatly reduced compared to coal. Therefore, using methane as raw gas to produce synthetic ammonia is an important way to transform the green synthetic ammonia industry, and it plays an important role in promoting the development of low-carbon economy in our province. The production of synthetic ammonia from methane includes three links: raw gas preparation, raw gas purification and ammonia synthesis. Among them, raw gas decarbonization and purification is the key link in the production of synthetic ammonia. Since carbon dioxide in the raw gas can poison the iron or copper catalyst in the ammonia synthesis process, directly leading to catalyst deactivation and greatly reducing the conversion efficiency of ammonia synthesis, the removal and recovery of CO2 in the raw gas of ammonia synthesis is not only related to the carbon balance of the synthesis process and system, but also has important significance for saving energy and reducing production costs. At present, common methods for decarbonizing synthesis gas include chemical absorption, physical adsorption, low-temperature separation, metal oxide and membrane separation, but there are still several problems. For example, the chemical absorption method of methyldiethanolamine (MDEA) is the most mature CO2 separation technology and has mature experience in large-scale industrial applications, but it has the disadvantages of high energy consumption for absorbent regeneration, large solvent loss and long-term use of easily corrosive equipment. Therefore, the development of low-energy consumption and low-cost decarbonization process is a major challenge facing the development of the ammonia industry.
[0003] As a new type of CO2 capture and separation technology, hydrate decarbonization technology realizes gas capture and separation through non-stoichiometric cage crystals formed by water molecules and small gas molecules. It has the advantages of simple process, high gas storage capacity, green environmental protection, low energy consumption and no by-products in the process. The cost of carbon capture (80-160 yuan / ton) is much lower than that of chemical absorption (190-250 yuan / ton). It has great commercial application prospects in the separation of low-concentration concentrated emission sources such as synthetic ammonia conversion gas. After desulfurization pretreatment, the synthesis gas of methane-to-synthetic ammonia conversion gas is mainly N2 and H2, and the volume fraction of impurity gas CO2 is about 18%-20%. Since the phase equilibrium conditions for CO2 to form hydrates are much lower than those for N2 and H2, CO2 in the mixed gas preferentially forms hydrates at a specific pressure and temperature, while N2 and H2 are difficult to form hydrates, thereby achieving CO2 separation and removal. The current hydrate decarbonization technology faces the problems of slow generation process and poor separation effect.
[0004] At present, traditional kinetic promoters such as sodium dodecyl sulfate (SDS) and sodium dodecylbenzene sulfonate (SDBS) promote the kinetic process of hydrate growth by enhancing gas-liquid contact to reduce interfacial surface tension. However, this type of surfactant is very easy to foam during the stirring process of the hydrate formation tower, which not only affects gas mass transfer, but also makes it difficult to recycle the promoter. Therefore, in order to realize the application of hydrate decarbonization technology in CO2 separation in synthetic ammonia conversion gas, it is urgent to develop green and environmentally friendly nano-kinetic promoters that are conducive to CO2 gas mass transfer, fast hydrate growth kinetics and recyclable, so as to carry out efficient synthetic ammonia decarbonization purification under mild conditions.
[0005] CN118016456A discloses a transition metal oxide quantum dot / carbon nanotube composite material, which belongs to the field of energy storage and conversion materials and their preparation technology. It is characterized in that the carbon nanotubes stably dispersed in water are obtained by two-step oxidation treatment combined with the Hummers method and hydrogen peroxide treatment, and the transition metal ions are precipitated into nuclei and loaded on the carbon nanotubes by the slow diffusion of ammonia gas, a decomposition product of ammonium bicarbonate, into the aqueous phase, and the obtained transition metal oxide quantum dot / carbon nanotube composite material has a high transition metal oxide loading. However, the two-step oxidation steps combined with the hydrogen peroxide treatment by the Hummers method are relatively cumbersome, which makes the preparation time too long, and the load is a transition metal oxide.
[0006] CN116247174A discloses a positive electrode material for lithium-sulfur batteries, comprising a carbon source and a metal salt solution, wherein the metal ions in the metal salt solution include at least one of nickel ions, cobalt ions or iron ions; characterized in that the carbon source is added to a solvent, heated and stirred to obtain a first dispersion; the first dispersion and the metal salt solution are mixed and heated to obtain a second dispersion; the second dispersion is dried to obtain a first precursor; the first precursor is kept at 800-1000°C for 3-5 hours in an inert gas to obtain a solid product, the fixed product is acid-washed to obtain a carbon nanotube composite material with metal particles loaded on the inner wall; sulfur is added to the composite material and heated to allow sulfur vapor to adhere to the outer wall of the carbon nanotube to obtain a positive electrode material for lithium-sulfur batteries. The patent does not perform hydrophilization treatment on carbon nanotubes, and the metal particles are mainly loaded on the inner wall of the carbon nanotubes.
[0007] CN117604559A discloses a conductive material for a catalytic electrode for preparing formic acid by electrocatalytic reduction of CO2, characterized in that it comprises a carbon nanotube solution and a precursor solution, which are first mixed to obtain a mixture I; the mixture I is secondly mixed with sodium hydroxide to obtain a supported bimetallic catalyst; the supported bimetallic catalyst is thirdly mixed with ethanol and Nafion solution to obtain a conductive material for a catalytic electrode. The conductive material is prepared by using metal elements Cu and In to prepare an indium copper bimetallic supported carbon nanotube catalyst, and the indium element is used to reduce the hydrogen evolution reaction, thereby improving the selectivity and catalytic stability of the product and increasing its adsorption capacity for CO2. However, the preparation method also has the problem of not being hydrophilized, and the active component on the surface of the carbon nanotube is a metal oxide.
[0008] CN115888699A discloses a method for preparing a composite material of precious metal loaded on carbon nanotubes, characterized in that the functional groups such as carbonyl, hydroxyl, carboxyl, etc. on the functional carbon nanotubes are used to reduce the salt containing precious metals. The preparation steps are as follows: add the raw material functionalized carbon nanotubes, the salt containing precious metals and deionized water into a three-necked flask, reflux reaction for 6 to 8 hours under stirring conditions, cool, centrifuge and dry to obtain the composite material of precious metal loaded carbon nanotubes. Advantages: (1) The raw materials are cheap and easy to obtain, and no additional reducing agent is required, which greatly reduces the preparation cost; (2) It is green and the reaction conditions are mild, the operation is safe, and it is suitable for industrial production; (3) The metal particles on the obtained precious metal loaded carbon nanotubes have a small particle size of only 2-3nm, and the catalytic effect is good. However, the preparation method uses precious metals as raw materials, which is relatively expensive, and the carbon nanotubes are functionalized carbon nanotubes, and the carbon nanotubes are not modified with hydrophilic functional groups. Summary of the invention
[0009] In order to overcome the shortcomings of the prior art, the present invention provides a method for preparing a transition metal modified carbon nanotube promoter, comprising the following steps:
[0010] S1: adding concentrated sulfuric acid to the hydrophobic multi-walled carbon nanotube powder, stirring and shaking, then adding concentrated nitric acid, reflux at high temperature in an oil bath, then adding a solvent, and filtering to obtain a hydrophilic functionalized carbon nanotube powder;
[0011] S2: dissolving the hydrophilic functionalized carbon nanotube powder obtained in S1 in a solvent, then mixing and stirring with a transition metal salt solution, evaporating, grinding and calcining to obtain transition metal-loaded hydrophilic functionalized carbon nanotubes.
[0012] Furthermore, the volume ratio of concentrated sulfuric acid to concentrated nitric acid described in S1 is 3:1.
[0013] Furthermore, the stirring time described in S1 is 6 hours, the stirring rate is 400-600 rpm, and the oscillation time is 4 hours.
[0014] Furthermore, the oil bath temperature described in S1 is 140° C., and the oil bath high temperature reflux time is 1 h.
[0015] Furthermore, the mass ratio of the transition metal to the hydrophilic functionalized carbon nanotube powder described in S2 is 0.2:1.
[0016] Furthermore, the evaporation temperature described in S2 is 50° C., the grinding time is 30 min, the heating rate during the calcination process is 10° C. / min, the calcination temperature is 550° C., and the calcination time is 1 h.
[0017] A transition metal modified carbon nanotube promoter. The transition metal modified carbon nanotube is a structure in which transition metal particles are distributed on the outer wall of the carbon nanotube.
[0018] The invention discloses an application of a transition metal-modified carbon nanotube promoter, wherein the transition metal-modified carbon nanotube is applied in the preparation of a carbon dioxide hydrate promoter for decarbonization of synthetic ammonia.
[0019] Technical Effects
[0020] (1) Preparation method: The preparation method of a transition metal-modified carbon nanotube promoter provided by the present invention adopts a variety of methods such as hydrophilic functional group modification, transition metal impregnation, and high-temperature calcination, which can control the transition metal-loaded hydrophilic functionalized carbon nanotube kinetic promoter with excellent kinetic promotion effect. In addition, the preparation process of the present invention is simple, the energy consumption of the decarbonization step of synthetic ammonia is low, and it has obvious cost advantages.
[0021] (2) Transition metal modified FMWCNTs: The present invention provides a transition metal modified carbon nanotube promoter, which can improve its interaction with water and CO2 through the innovative use of multi-walled carbon nanotubes (FMWCNTs) modified with hydrophilic functional groups, thereby improving the formation and decomposition efficiency of hydrates, and loading transition metals with good thermal conductivity and strong CO2 adsorption capacity such as copper Cu, silver Ag, praseodymium Pr, etc., to successfully prepare a highly efficient kinetic promoter, which can achieve CO2 removal "hydration" under mild conditions and "decomposition" of hydrates at room temperature, realize the effective recycling of the promoter solution, and reduce resource waste; and the promoter can be used to efficiently separate CO2 from the synthetic ammonia raw gas, and has a very high CO2 hydration rate and a one-time hydrated CO2 recovery rate, the CO2 hydration rate is greater than 75%, and the one-time hydrated CO2 recovery rate is 80%.
[0022] (3) Application: The transition metal-modified carbon nanotube carbon dioxide hydrate promoter provided by the present invention contributes to the development of industrial circular economy, provides a new approach for the green and low-carbon transformation of the synthetic ammonia industry, and can be used for CO2 capture. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and should not be regarded as limiting the scope. For those of ordinary skill in the art, other relevant drawings can be obtained based on these drawings without creative work. In the drawings:
[0024] Figure 1 is a transmission electron microscope morphology image of the transition metal-loaded FMWCNTs of the present invention;
[0025] Figure 2 This is a result diagram of CO2 adsorption selectivity of transition metal-loaded FMWCNTs prepared in Example 1 of the present invention under hydration reaction pressure conditions;
[0026] Figure 3 is a graph of the CO2 hydration rate of transition metal-loaded FMWCNTs prepared in Example 1 of the present invention under hydration reaction conditions;
[0027] Figure 4 This is a graph of CO2 separation efficiency and gas storage capacity of transition metal-loaded FMWCNTs prepared in Example 1 of the present invention under hydration reaction conditions. DETAILED DESCRIPTION
[0028] The following will be combined with Examples 1 to 3 of the present invention and the attached Figures 1 to 4, the technical solution of the present invention is clearly and completely described. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] The present invention provides a method for preparing a transition metal-modified carbon nanotube promoter, comprising the following steps:
[0030] S1: First, hydrophobic multi-walled carbon nanotubes (MWCNTs) are modified with hydrophilic functional groups (-OH / -COOH / -NH2) to obtain hydrophilic functionalized carbon nanotubes (FMWCNTs). Hydrophilic functional groups on the surface of carbon nanotubes are used to form hydrogen bonds with water, thereby improving the hydrophilicity and dispersibility of CNTs in solution. In addition, the hydrophilic functional groups of CNTs can enhance the adsorption performance of CO2 molecules, which is beneficial to gas mass transfer.
[0031] S2: Then, transition metals are further loaded on the basis of FMWCNTs. On the one hand, transition metal particles are introduced as active sites for adsorbing CO2 on the surface of FMWCNTs to enhance gas mass transfer. On the other hand, transition metal particles, as heterogeneous nucleation sites, can accelerate the induced nucleation of hydrates and facilitate heat transfer during the massive growth of hydrates, thereby promoting the rapid and massive generation of hydrates. Then, the transition metal-loaded FMWCNTs are added to deionized water, and thermodynamic promoters such as tetrahydrofuran are added to form a nanofluid promoter solution. The solution is ultrasonically dispersed to make the transition metal-loaded FMWCNTs evenly dispersed in the solution to obtain a transition metal-modified carbon nanotube promoter.
[0032] Example 1
[0033] S1: Add concentrated sulfuric acid (concentration of 95% to 98%) to the MWCNTs powder, and then perform magnetic stirring for 6 hours, ultrasonic oscillation for 4 hours, and then add concentrated nitric acid (concentration of 65% to 70%), and perform magnetic stirring for 30 minutes to obtain a mixed solution. Then, place the solution in an oil bath pot and reflux at 140°C for 1 hour, add deionized water to dilute, and place it at room temperature for 24 hours. Repeat the filtration several times until the pH of the filtrate becomes neutral to obtain FMWCNTs.
[0034] S2: The FMWCNTs obtained in S1 were then dissolved in an ethanol solution, and then Cu(NO3)2·3H2O and FMWCNTs in a mass ratio of 0.2:1 were dissolved in another ethanol solution, and then the two were mixed and stirred for 2 h to obtain a mixed solution, and then the solution was evaporated to dryness at 50 °C in an evaporating table, ground for 30 min, and then heated at 10 °C / min in a tubular furnace and calcined at 550 °C for 1 h to obtain Cu-loaded FMWCNTs.
[0035] The obtained Cu-loaded FMWCNTs were added to deionized water, and then THF (tetrahydrofuran) was added to prepare a nanofluid promoter solution, and the solution was ultrasonically dispersed for 10 minutes to uniformly disperse the Cu-loaded FMWCNTs in the solution to obtain a Cu-loaded carbon nanotube promoter.
[0036] After the air tightness test of the experimental device, the solution was loaded into the reactor, the mixed gas was introduced into the equilibrium reactor to 4.5MPa and balanced at above 16°C for 30 minutes, and then introduced into the reactor, and the stirring paddle was turned on for 30 minutes to allow the gas and liquid to fully contact and reach the dissolution equilibrium. Then the stirring was turned off, and the temperature setting of the circulating condenser was adjusted to allow the hydration reaction to occur at about 2°C. After cooling for 90 minutes, the stirring paddle was turned on again to allow the hydration reaction to proceed rapidly until the pressure in the reactor remained unchanged for 20 minutes, which was considered to be the end of the hydration reaction.
[0037] Combination Figure 1 The transmission electron microscopy morphology of transition metal-loaded FMWCNTs can be obtained; combined with Figure 2 , using the Cu-loaded FMWCNTs prepared in Example 1 to perform Monte Carlo theoretical calculation simulation, the CO2 adsorption selectivity result diagram was obtained. Figure 2 It can be seen that the CO2 selectivity of the Cu-loaded FMWCNTs prepared in Example 1 of the present invention under low temperature and high pressure reaction conditions reaches more than 900%.
[0038] Combination Figure 3 It can be obtained that the CO2 hydration rate of the Cu-loaded FMWCNTs prepared in Example 1 of the present invention under low temperature and high pressure reaction conditions is higher than 75%; combined Figure 4 It can be obtained that the Cu-loaded FMWCNTs prepared in Example 1 of the present invention have excellent decarburization effect under low temperature and high pressure reaction conditions, and also have good kinetic promotion effect, and the transition metal-modified carbon nanotube promoter provided by the present invention avoids the problems of foaming caused by traditional kinetic promoters that hinder the hydration reaction from continuing and are not easy to recycle. The Cu-loaded FMWCNTs used in the above Example 1 achieve hydration kinetic performance under low temperature and high pressure, combined with Figure 4 The CO2 separation efficiency shown in the figure shows that the decarbonization efficiency is as high as 80%.
[0039] Example 2
[0040] S1: Add concentrated sulfuric acid to the MWCNTs powder, and then perform magnetic stirring for 6 hours, ultrasonic oscillation for 4 hours, and then add concentrated nitric acid and perform magnetic stirring for 32 minutes to obtain a mixed solution. Then, place the solution in an oil bath at 142°C for 1 hour, add deionized water to dilute, and place at room temperature for 24 hours. Repeat the filtration several times until the pH of the filtrate becomes neutral to obtain FMWCNTs.
[0041] S2: The FMWCNTs obtained in S1 were then dissolved in an ethanol solution, and then AgNO3 and FMWCNTs in a mass ratio of 0.2:1 were dissolved in another ethanol solution, and then the two were mixed and stirred for 2 h to obtain a mixed solution, and then the solution was evaporated to dryness at 50 °C in an evaporating table, ground for 30 min, and then heated at 10 °C / min in a tubular furnace and calcined at 550 °C for 1 h to obtain Ag-loaded FMWCNTs.
[0042] The obtained Ag-loaded FMWCNTs were added to deionized water, and then tetrabutylammonium bromide was added to prepare a nanofluid promoter solution, and the solution was ultrasonically dispersed for 10 minutes to uniformly disperse the Ag-loaded FMWCNTs in the solution to obtain an Ag-loaded carbon nanotube promoter.
[0043] Example 3
[0044] S1: Add concentrated sulfuric acid to the MWCNTs powder, and then stir magnetically for 6 hours, ultrasonically vibrate for 4 hours, then add concentrated nitric acid, stir magnetically for 28 minutes to obtain a mixed solution, then reflux the solution in an oil bath at 138°C for 1 hour, add deionized water to dilute, and place at room temperature for 24 hours, and repeatedly filter until the pH of the filtrate becomes neutral to obtain FMWCNTs;
[0045] S2: The FMWCNTs obtained in S1 were then dissolved in an ethanol solution, and then Pr(NO3)3 and FMWCNTs in a mass ratio of 0.2:1 were dissolved in another ethanol solution, and then the two were mixed and stirred for 2 h to obtain a mixed solution, and then the solution was evaporated to dryness at 50 °C in an evaporating table, ground for 30 min, and then heated at 10 °C / min in a tubular furnace and calcined at 550 °C for 1 h to obtain Pr-loaded FMWCNTs.
[0046] The obtained Pr-loaded FMWCNTs were added into deionized water, and then tetrabutylammonium fluoride was added to prepare a nanofluid promoter solution, and the solution was ultrasonically dispersed for 10 minutes to make the Pr-loaded FMWCNTs uniformly dispersed in the solution, thereby obtaining a Pr-loaded carbon nanotube promoter.
[0047] The present invention provides a method for preparing a transition metal-modified carbon nanotube promoter. The preparation method has a simple preparation process and low cost. The hydrate method is used for the decarbonization step of synthetic ammonia, which has low energy consumption and obvious cost advantages. It is also conducive to the development of industrial circular economy and provides a new path for the green and low-carbon transformation of the synthetic ammonia industry.
Claims
1. A method for preparing a transition metal modified carbon nanotube promoter, characterized in that: The following steps are involved: S1: adding concentrated sulfuric acid to the hydrophobic multi-walled carbon nanotube powder, stirring and shaking, then adding concentrated nitric acid, reflux at high temperature in an oil bath, then adding a solvent, and filtering to obtain a hydrophilic functionalized carbon nanotube powder; S2: dissolving the hydrophilic functionalized carbon nanotube powder obtained in S1 in a solvent, then mixing and stirring with a transition metal salt solution, evaporating, grinding and calcining to obtain transition metal-loaded hydrophilic functionalized carbon nanotubes.
2. The method for preparing a transition metal modified carbon nanotube promoter according to claim 1, characterized in that: The mass ratio of the hydrophobic multi-walled carbon nanotubes to the concentrated sulfuric acid in S1 is 1:18.4, and the volume ratio of the concentrated sulfuric acid to the concentrated nitric acid is 3:
1.
3. The method for preparing a transition metal modified carbon nanotube promoter according to claim 1, characterized in that: The stirring time described in S1 is 6 h, the stirring rate is 400-600 rpm, and the shaking time is 4 h.
4. The method for preparing a transition metal modified carbon nanotube promoter according to claim 1, characterized in that: The oil bath temperature described in S1 is 140° C., and the oil bath high temperature reflux time is 1 h.
5. The method for preparing a transition metal modified carbon nanotube promoter according to claim 1, characterized in that: The mass ratio of the transition metal to the hydrophilic functionalized carbon nanotube powder described in S2 is 0.2:
1.
6. The method for preparing a transition metal modified carbon nanotube promoter according to claim 1, characterized in that: The evaporation temperature described in S2 is 50°C, the grinding time is 30 min, the heating rate during the calcination process is 10°C / min, the calcination temperature is 550°C, and the calcination time is 1 h.
7. A transition metal-modified carbon nanotube promoter obtained by the preparation method according to any one of claims 1 to 6, characterized in that: The transition metal modified carbon nanotubes have a structure in which transition metal particles are distributed on the outer wall of the carbon nanotubes.
8. The use of a transition metal-modified carbon nanotube promoter according to claim 7, characterized in that: The transition metal-modified carbon nanotube is used in the preparation of a carbon dioxide hydrate promoter for decarbonization of synthetic ammonia.
Citation Information
Patent Citations
Preparation method of noble metal-loaded carbon nanotube composite material
CN115888699A
Preparation method of positive electrode material, positive electrode material and lithium-sulfur battery
CN116247174A
Preparation method of conductive material, catalytic electrode and application thereof, and method for preparing formic acid by electrocatalytic reduction of CO2
CN117604559A
Preparation method of transition metal oxide quantum dot / carbon nanotube composite material
CN118016456A
Carbon nanotube-contained composite decarbonization solution for recovering carbon dioxide in mixed gas
CN109603425A