Surface treatment method of metal film tube and reaction kettle

By forming a diamagnetic coating on the surface of the metal membrane tube, the problem of clogging of the filter holes of the membrane tube is solved, the cleaning frequency is reduced, the production capacity is increased, and a more efficient filtration flux is achieved.

CN118808093AActive Publication Date: 2024-10-22DONGMING RISUN CHEM CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410795071.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-22
Estimated Expiration
2044-06-19

AI Technical Summary

Technical Problem

The filter holes of metal membrane tubes are easily blocked, resulting in reduced flux and frequent cleaning, which affects caprolactam production.

Method used

A diamagnetic coating is formed on the surface of the metal film tube, and the magnetic adsorption of the chelating agent is inhibited through pretreatment, spraying of polytetrafluoroethylene powder and curing treatment.

Benefits of technology

It effectively avoids the adsorption of chelating agent on the surface of the membrane tube and the filter pores, reduces the cleaning frequency, and increases the flux of the metal membrane tube and the production capacity of caprolactam.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118808093A_ABST
    Figure CN118808093A_ABST
Patent Text Reader

Abstract

The invention provides a surface treatment method of a metal film tube and a reaction kettle, and the method comprises the following steps: pretreating the surface of the metal film tube to clean the surface of the metal film tube; the surface of the cleaned metal film pipe is sprayed, so that a coating is formed on the surface of the metal film pipe, and the coating is a diamagnetic coating; the diamagnetic coating is used for inhibiting magnetic adsorption of the chelating agent to the metal film tube; carrying out curing treatment on the coating on the metal film tube; and cooling the cured metal film tube to room temperature. The surface of the metal film tube is sprayed to form the diamagnetic coating, so that the surface of the metal film tube has the characteristic of inhibiting the magnetic adsorption effect of the chelating agent on the metal film tube, and the chelating agent is prevented from being adsorbed on the surface of the metal film tube and in the filtering holes of the metal film tube to influence the filtering effect of the metal film tube. When the metal film pipe is cleaned, the metal film pipe can be easily cleaned, the cleaning frequency of the metal film pipe is reduced, and the productivity of corresponding products is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of metal film tubes, and in particular to a surface treatment method and a reaction kettle for metal film tubes. Background Art

[0002] Caprolactam products are an important organic chemical raw material. Their main use is to produce polyamide slices through polymerization, which can be further processed into nylon fibers, engineering plastics, plastic films, etc. Cyclohexanone ammoximation reaction is a key process in the production of caprolactam. This process uses titanium silicon molecular sieve (TS-1) as a catalyst, tert-butyl alcohol as a solvent, cyclohexanone, hydrogen peroxide and gaseous ammonia as raw materials. Cyclohexanone oxime is generated in a kettle reactor with a stirrer, and TS-1 is filtered using a metal membrane tube. The filtered reaction clear liquid is sent to the subsequent process, and the turbid liquid containing the catalyst is recycled back to the reactor for reuse. The separation equipment of titanium silicon molecular sieve and reaction liquid is one of the core equipment of cyclohexanone ammoximation technology. At present, the widely used ones are built-in or external metal sintered membranes, that is, metal membrane tubes. The filtration pore size of the metal membrane tube is 5μm, and the filtration efficiency of TS-1 is greatly affected by the catalyst particle size and the oximation process. As the oximation reaction proceeds, the particle size of TS-1 decreases from the initial 90-100 μm to less than 5 μm due to collisions between TS-1 and the stirring paddle, which easily leads to clogging of the filter holes of the metal membrane tube. In addition, the raw hydrogen peroxide contains chelating stabilizers (also called chelating agents). After chelating metal ions, they are adsorbed into the filter holes due to magnetic adsorption. During backwashing, due to magnetic adsorption, it is difficult for the chelating agents to be washed off from the filter holes and the surface of the metal membrane tube, which also causes clogging of the filter holes. Due to the above two reasons, the flux of the metal membrane tube is reduced, and the metal membrane tube needs to be cleaned frequently, which affects the progress of the ammoximation reaction and reduces the yield of caprolactam. Summary of the invention

[0003] The purpose of the embodiments of the present application is to provide a surface treatment method for a metal membrane tube and a reactor, so as to solve the problem that the filter holes of the metal membrane tube are difficult to clean and the frequent cleaning of the metal membrane tube affects the production capacity.

[0004] The embodiment of the present application adopts the following technical solution: a surface treatment method of a metal film tube, comprising:

[0005] Pre-treating the surface of the metal film tube to clean the surface of the metal film tube;

[0006] Spraying the cleaned surface of the metal film tube to form a coating on the surface of the metal film tube, wherein the coating is an anti-magnetic coating; the anti-magnetic coating is used to inhibit the magnetic adsorption of the chelating agent to the metal film tube;

[0007] Performing a curing treatment on the coating on the metal film tube;

[0008] The metal film tube after curing is cooled to room temperature.

[0009] In some embodiments, the surface of the metal film tube is pretreated, including:

[0010] A solvent or alkaline cleaning agent is used to at least remove grease, dust and pollutants soluble in the solvent on the surface of the metal membrane tube.

[0011] In some embodiments, spraying the surface of the cleaned metal film tube comprises:

[0012] The polytetrafluoroethylene powder is electrostatically sprayed onto the outer surface of the metal film tube, wherein the particle size of the polytetrafluoroethylene powder is 20 microns to 30 microns.

[0013] In some embodiments, spraying the surface of the cleaned metal film tube further comprises:

[0014] A positively charged spray gun is used, 15 cm to 30 cm away from the outer surface of the metal film tube, and stainless steel is used as the cathode to spray polytetrafluoroethylene powder onto the outer surface of the metal film tube; wherein the spraying pressure of the spray gun is 2Pa to 10Pa, and the spraying voltage of the spray gun is 60KV to 100KV.

[0015] In some embodiments, curing the coating on the metal film tube comprises:

[0016] The metal film tube is placed in a curing furnace for heating, the curing temperature is 370° C. to 400° C., and the curing time is 10 minutes to 60 minutes.

[0017] In some embodiments, cooling the cured metal film tube to room temperature comprises:

[0018] The metal film tube after curing is naturally cooled to room temperature to reduce the generation of thermal stress during the cooling process.

[0019] An embodiment of the present application also provides a reaction kettle, comprising a metal film tube treated by the surface treatment method of the metal film tube as described in any of the above embodiments, wherein the antimagnetic coating on the metal film tube is used to inhibit the magnetic adsorption of the chelating agent to the metal film tube.

[0020] In some embodiments, the reactor comprises:

[0021] A reactor body having a closed space;

[0022] A stirring device, located in the enclosed space of the reactor body, for stirring the reaction turbid liquid in the reactor body;

[0023] A base, which is arranged on the inner wall of the closed space of the reactor body;

[0024] The metal film tube is arranged on the base and is used to filter the reaction turbid liquid in the reactor body to obtain a reaction clear liquid, wherein the reaction clear liquid is located in the metal film tube;

[0025] A decoupling tube has one end connected to the metal film tube and the other end penetrating the wall of the reactor body and extending to the outside of the reactor to discharge the reaction clear liquid in the metal film tube.

[0026] In some embodiments, one end of the metal film tube is detachably disposed on the base, and the other end of the metal film tube is connected to one end of the outlet tube.

[0027] In some embodiments, at least two bases are provided on the inner wall of the enclosed space of the reactor body, each base is provided with at least two slots, the number of the metal film tubes corresponds to the number of the slots, and one end of the metal film tube is fixed to the corresponding slot.

[0028] The beneficial effects of the embodiments of the present application are:

[0029] The anti-magnetic coating is sprayed on the surface of the metal film tube so that the surface of the metal film tube can have the characteristic of inhibiting the magnetic adsorption of the chelating agent on the metal film tube, avoiding the chelating agent adsorbing on the surface of the metal film tube and the filter holes of the metal film tube to affect the filtering effect of the metal film tube. When cleaning the metal film tube, the metal film tube can be cleaned more easily, reducing the cleaning frequency of the metal film tube and improving the production capacity of the corresponding product. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the related technologies, the drawings required for use in the embodiments or the related technical descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0031] Figure 1 This is a schematic diagram of the structure of the reactor of this application;

[0032] Figure 2 This is a schematic diagram of the cross-sectional structure of the reactor of this application;

[0033] Figure 3 This is a schematic diagram of the structure of the metal film tube of this application.

[0034] Figure numerals: 1. Reactor; 2. Metal membrane tube; 3. Stirring device; 4. Base; 5. Coating. DETAILED DESCRIPTION

[0035] Various aspects and features of the present application are described herein with reference to the accompanying drawings.

[0036] It should be understood that various modifications may be made to the embodiments of the present application. Therefore, the above description should not be considered as limiting, but only as an example of an embodiment. Other modifications within the scope and spirit of the present application will occur to those skilled in the art.

[0037] The accompanying drawings, which are incorporated in and constitute a part of the specification, illustrate embodiments of the present application and, together with the general description of the present application given above and the detailed description of the embodiments given below, serve to explain the principles of the present application.

[0038] These and other characteristics of the present application will become apparent from the following description of a preferred form of embodiment given as a non-limiting example with reference to the accompanying drawings.

[0039] It should also be understood that although the present application has been described with reference to some specific examples, those skilled in the art will be able to readily implement many other equivalent forms of the present application.

[0040] The above and other aspects, features and advantages of the present application will become more apparent in view of the following detailed description when taken in conjunction with the accompanying drawings.

[0041] Specific embodiments of the present application are described hereinafter with reference to the accompanying drawings; however, it should be understood that the embodiments applied for are merely examples of the present application, which may be implemented in a variety of ways. Well-known and / or repeated functions and structures are not described in detail to avoid unnecessary or redundant details that obscure the present application. Therefore, the specific structural and functional details applied for herein are not intended to be limiting, but merely serve as a basis and representative basis for the claims to teach those skilled in the art to use the present application in a variety of ways with substantially any suitable detailed structure.

[0042] This specification may use the phrases "in one embodiment," "in another embodiment," "in yet another embodiment," or "in other embodiments," all of which may refer to one or more of the same or different embodiments according to the present application.

[0043] In order to solve the problems in the background technology, the present application provides a surface treatment method of a metal film tube, the method comprising the following steps:

[0044] The surface of the metal film tube is pretreated to clean the surface of the metal film tube.

[0045] For example, the surface of the metal film tube is first pretreated. The pretreatment mainly involves cleaning the surface of the metal film tube to prevent grease, dust and other pollutants on the surface of the metal film tube from affecting the subsequent surface treatment effect of the metal film tube. During the pretreatment, grease, dust and other pollutants on the surface of the metal film tube can be cleaned to maintain the cleanliness of the surface of the metal film tube, so as to better achieve the subsequent treatment of the metal film tube.

[0046] It is understandable that both the inner and outer surfaces of the metal film tube can be cleaned, or only the outer surface of the metal film tube can be cleaned. It is understandable that the cleaning of the surface of the metal film tube described here includes simultaneously cleaning the filter holes of the metal film tube.

[0047] The cleaned surface of the metal film tube is sprayed to form a coating on the surface of the metal film tube, wherein the coating is an anti-magnetic coating; the anti-magnetic coating is used to inhibit the magnetic adsorption of the chelating agent to the metal film tube.

[0048] Exemplarily, the surface of the cleaned metal film tube is sprayed, that is, the material for forming the antimagnetic coating is sprayed onto the surface of the metal film tube. This allows the material to form a coating on the surface of the metal film tube that adheres to the surface of the metal film tube. The coating is an antimagnetic coating, that is, it does not have magnetic adsorption capacity, and the magnetic adsorption effect of the chelating agent on the metal film tube is suppressed by the antimagnetic coating. Of course, it is understandable that during the spraying process, the hole wall of the filter hole of the metal film tube can also be sprayed with an antimagnetic coating, and the antimagnetic coating plays a barrier role. When the chelating agent is close to the surface of the metal film tube, since the surface of the metal film tube and the filter hole both have a layer of antimagnetic coating that does not have magnetic adsorption capacity, the chelating agent will no longer be adsorbed on the surface of the metal film tube and the filter hole.

[0049] Even if the filter holes are not sprayed with anti-magnetic coating, since the filter holes are very small, after the surface of the metal film tube has the pit magnetic coating, the chelating agent can only contact the filter holes. Combined with the specific production scenario, the chelating agent in the reaction turbid liquid is constantly stirred. After the metal film tube surface has the anti-magnetic coating, it is difficult for the chelating agent to form an adhesion relationship with the very small filter hole, because the contact area between the two is very small, and the chelating agent can easily detach from the metal film tube under the action of stirring. In addition, since the magnetic adsorption area between the chelating agent and the filter hole becomes very small, the adsorption force between the two also becomes very small. Therefore, even if the chelating agent can be adsorbed at the filter hole, it is easy to wash off the chelating agent on the metal film tube when the metal film tube is cleaned.

[0050] Of course, it is understandable that the antimagnetic coating may be formed on the surface of the metal film tube by other methods besides spraying.

[0051] The coating on the metal film tube is cured.

[0052] For example, after the anti-magnetic coating is sprayed on the metal film tube, in order to ensure the firmness between the anti-magnetic coating and the metal film tube and prevent the anti-magnetic coating from falling off the metal film tube and affecting the use of the metal film tube, the anti-magnetic coating is cured. The curing treatment includes but is not limited to placing the metal film tube with the anti-magnetic coating in a curing furnace for curing heating, that is, performing a thermal curing treatment.

[0053] The metal film tube after curing is cooled to room temperature.

[0054] Exemplarily, the metal film tube after curing is cooled to room temperature. The cooling process may be natural cooling to avoid thermal stress affecting the performance of the coating, thereby ensuring the anti-magnetic properties of the metal film tube.

[0055] The embodiment of the present application sprays an anti-magnetic coating on the surface of the metal film tube, so that the surface of the metal film tube can have the characteristic of inhibiting the magnetic adsorption effect of the chelating agent on the metal film tube, and avoids the chelating agent adsorbing on the surface of the metal film tube and the filter holes of the metal film tube to affect the filtering effect of the metal film tube. When cleaning the metal film tube, the metal film tube can be cleaned more easily, reducing the cleaning frequency of the metal film tube and improving the production capacity of the corresponding product.

[0056] In some embodiments, the surface of the metal film tube is pretreated, including:

[0057] A solvent or alkaline cleaning agent is used to at least remove grease, dust and pollutants soluble in the solvent on the surface of the metal membrane tube.

[0058] For example, the grease on the surface of the metal film tube and pollutants soluble in the solvent can be dissolved by a solvent or an alkaline cleaning agent, and the dust and the dissolved grease and pollutants can be washed away by the solvent or the alkaline cleaning agent. Of course, the surface of the metal film tube can also be cleaned by other cleaning agents, which does not affect the subsequent coating spraying of the metal film tube.

[0059] In some embodiments, spraying the surface of the cleaned metal film tube comprises:

[0060] The polytetrafluoroethylene powder is electrostatically sprayed onto the outer surface of the metal film tube, wherein the particle size of the polytetrafluoroethylene powder is 20 microns to 30 microns.

[0061] Exemplary, polytetrafluoroethylene (PTFE) material has the characteristics of acid and alkali resistance, resistance to various organic solvents, and is almost insoluble in all solvents. At the same time, polytetrafluoroethylene has the characteristics of high temperature resistance, and its friction coefficient is extremely low. Therefore, the coating formed by spraying PTFE material has good performance of acid and alkali resistance and resistance to various organic solvents. In addition, the coating formed by PTFE material has a low friction coefficient, so that the chelating agent and titanium silicon molecular sieve (TS-1) are not easy to adhere to and fix with the coating, avoiding the chelating agent and titanium silicon molecular sieve from being attached to the surface of the metal membrane tube to form a blockage on the filter hole.

[0062] When the metal membrane tube filters the reaction turbid liquid, the reaction turbid liquid is filtered from the outside of the metal membrane tube through the filter holes to form a reaction clear liquid that enters the metal membrane tube. Therefore, only the outer surface of the metal membrane tube can be sprayed to form an anti-magnetic coating on the outer surface of the metal membrane tube.

[0063] The particle size of PTFE powder is 20 microns to 30 microns to ensure good coating effect and uniformity.

[0064] In some embodiments, spraying the surface of the cleaned metal film tube further comprises:

[0065] A positively charged spray gun is used, 15 cm to 30 cm away from the outer surface of the metal film tube, and stainless steel is used as the cathode to spray polytetrafluoroethylene powder onto the outer surface of the metal film tube; wherein the spraying pressure of the spray gun is 2Pa to 10Pa, and the spraying voltage of the spray gun is 60KV to 100KV.

[0066] For example, a dedicated electrostatic spray gun is used, in which a stainless steel part is used as the cathode, the spray gun is positively charged, the distance between the spray gun and the outer surface of the metal film tube is 20 cm, and the spraying pressure and voltage are controlled, the spraying pressure is 6 Pa, and the voltage is 80 KV to ensure effective adhesion of the powder.

[0067] Of course, the distance between the spray gun and the outer surface of the metal film tube can also be 15 cm or 30 cm. The spraying pressure can also be 2 Pa or 10 Pa. The spraying voltage can be 60 KV or 100 KV. The effects corresponding to different treatment conditions can be seen in Table 1.

[0068] Table 1: Filtration flux and backwashing frequency of metal membrane tubes under different treatment conditions

[0069]

[0070]

[0071] Among them, comparative example 1 is: installing an untreated metal membrane tube into a caprolactam oximation reactor, the oximation reaction temperature is 85°C, the pressure is 0.25MPa, and the anti-clogging ability of the metal membrane tube.

[0072] In some embodiments, curing the coating on the metal film tube comprises:

[0073] The metal film tube is placed in a curing furnace for heating, the curing temperature is 370° C. to 400° C., and the curing time is 10 minutes to 60 minutes.

[0074] For example, the metal film tube is placed in a curing furnace for heating, and the curing temperature is 370°C, or 400°C. The curing time can be 10 minutes or 60 minutes. The effects corresponding to different treatment conditions can still be seen in Table 1.

[0075] It can be seen from Table 1 that under preferred conditions, the time for the filtration flux of the metal membrane tube improved by electrostatic spraying PTFE in Example 1 to drop to 60% of the initial flux is the longest, reaching 186 days, and the anti-clogging ability of the unimproved metal membrane tube is only 58 days, which is also higher than the anti-clogging ability of the metal membrane tube under non-preferred conditions.

[0076] In some embodiments, cooling the cured metal film tube to room temperature comprises:

[0077] The metal film tube after curing is naturally cooled to room temperature to reduce the generation of thermal stress during the cooling process and to ensure the performance of the coating as much as possible.

[0078] Based on the same inventive concept, the present application embodiment also provides a reaction kettle 1, combined with Figure 1 , Figure 2 and Figure 3 The reactor 1 includes a metal film tube 2 treated by the surface treatment method of the metal film tube 2 as described in any one of the above embodiments, and the coating 5 on the metal film tube 2 is an antimagnetic coating, which is used to inhibit the magnetic adsorption of the chelating agent to the metal film tube 2. The reactor 1 using the above metal film tube 2 does not need to frequently clean the metal film tube 2, thereby improving the production capacity of the reactor 1.

[0079] Taking caprolactam oximation as an example, raw materials such as cyclohexanone, hydrogen peroxide, gaseous ammonia, tert-butyl alcohol and the like react in an oximation reactor 1 to generate cyclohexanone oxime. After the reaction turbid liquid containing the catalyst is filtered through the metal membrane tube 2, the catalyst is trapped in the reactor 1, and the reaction clear liquid without the catalyst can be sent to the tert-butyl alcohol recovery tower. The metal membrane tube 2 after electrostatic spraying of PTFE is installed in the caprolactam oximation reactor 1, and the time when the flux of the metal membrane tube 2 drops to 60% of the initial flux is used as the measure of the anti-blocking ability of the membrane tube. The reactor 1 effectively ensures the stable and long-term operation of the caprolactam oximation catalyst separation technology.

[0080] In some embodiments, the reactor 1 comprises:

[0081] The reactor body has a closed space. For example, the reactor body can be a tank body with a closed space, which can be used for the reaction of materials to produce corresponding products. For example, the reactor body can be used for cyclohexanone ammoximation reaction to produce caprolactam products. The closed space of the reactor body has a certain pressure, so that the reaction turbid liquid in the reactor body can be filtered through the filter holes of the metal membrane tube 2 under the action of pressure.

[0082] The stirring device 3 is located in the enclosed space of the reactor body and is used to stir the reaction turbid liquid in the reactor body. The stirring device 3 may include a stirring head, a stirring rod and a motor. One end of the stirring rod is located outside the reactor body and connected to the motor. The other end of the stirring rod is located inside the reactor body and connected to the stirring head. The motor drives the stirring rod and the stirring head to rotate to stir the material in the reactor body and improve the uniformity of the material and the reaction efficiency.

[0083] The base 4 is arranged on the inner wall of the closed space of the reactor body, and the base 4 is used to install the metal membrane tube 2.

[0084] The metal film tube 2 is arranged on the base 4 and is used to filter the reaction turbid liquid in the reactor body to obtain a reaction clear liquid, wherein the reaction clear liquid is located in the metal film tube 2. That is, the reaction turbid liquid passes through the filter holes on the metal film tube 2 from the outside of the metal film tube 2 to form a reaction clear liquid and enter the metal film tube 2.

[0085] The outlet pipe (not shown in the figure) has one end connected to the metal film tube 2 and the other end extending through the wall of the reactor body to the outside of the reactor 1 to discharge the reaction clear liquid in the metal film tube 2. A separate outlet pipe can be provided for each metal film tube 2, or a main outlet pipe can be used and a plurality of branch pipes can be provided on the main outlet pipe, each branch pipe being connected to a corresponding metal film tube 2.

[0086] In some embodiments, in combination Figure 1 and Figure 2 , one end of the metal film tube 2 is detachably arranged on the base 4, and the other end of the metal film tube 2 is connected to one end of the outlet tube. The metal film tube 2 is detachably installed on the base 4, which facilitates the installation and removal of the metal film tube 2 and improves the installation and removal efficiency of the reactor 1. For example, a card slot can be set on the base 4, and one end of the metal film tube 2 is fixed on the card slot. Of course, it can be understood that other structural methods can also be used to achieve the detachable connection between the metal film tube 2 and the base 4. This is only used as an example and does not constitute a limitation on the scope of protection of the claims.

[0087] In some embodiments, at least two bases 4 are provided on the inner wall of the closed space of the reactor body, each base 4 is provided with at least two slots, the number of the metal film tubes 2 corresponds to the number of the slots, and one end of the metal film tube 2 is fixed to the corresponding slot. One end of the base 4 can be fixed on the inner wall of the closed space of the reactor body, and the other end of the base 4 extends toward the center of the closed space of the reactor body. By providing a plurality of slots on the base 4, a plurality of metal film tubes 2 can be installed to improve the filtration efficiency of the reaction turbid liquid in the closed space of the reactor body.

[0088] Multiple embodiments of the present application are described in detail above, but the present application is not limited to these specific embodiments. Those skilled in the art can make various variations and modifications to the embodiments based on the concept of the present application, and these variations and modifications should all fall within the scope of protection required by the present application.

Claims

1. A surface treatment method for a metal film tube, characterized in that: include: Pre-treating the surface of the metal film tube to clean the surface of the metal film tube; Spraying the cleaned surface of the metal film tube to form a coating on the surface of the metal film tube, wherein the coating is an anti-magnetic coating; the anti-magnetic coating is used to inhibit the magnetic adsorption of the chelating agent to the metal film tube; Performing a curing treatment on the coating on the metal film tube; The metal film tube after curing is cooled to room temperature.

2. The surface treatment method of the metal film tube according to claim 1, characterized in that: Pre-treat the surface of the metal film tube, including: A solvent or alkaline cleaning agent is used to at least remove grease, dust and pollutants soluble in the solvent on the surface of the metal membrane tube.

3. The surface treatment method of the metal film tube according to claim 1, characterized in that: The surface of the cleaned metal film tube is sprayed, including: The polytetrafluoroethylene powder is electrostatically sprayed onto the outer surface of the metal film tube, wherein the particle size of the polytetrafluoroethylene powder is 20 microns to 30 microns.

4. The surface treatment method of the metal film tube according to claim 3, characterized in that: The surface of the cleaned metal film tube is sprayed, and also includes: A positively charged spray gun is used, 15 cm to 30 cm away from the outer surface of the metal film tube, and stainless steel is used as the cathode to spray polytetrafluoroethylene powder onto the outer surface of the metal film tube; wherein the spraying pressure of the spray gun is 2Pa to 10Pa, and the spraying voltage of the spray gun is 60KV to 100KV.

5. The surface treatment method of the metal film tube according to claim 1, characterized in that: The coating on the metal film tube is cured, comprising: The metal film tube is placed in a curing furnace for heating, the curing temperature is 370° C. to 400° C., and the curing time is 10 minutes to 60 minutes.

6. The surface treatment method of the metal film tube according to claim 1, characterized in that: The metal film tube after curing is cooled to room temperature, comprising: The metal film tube after curing is naturally cooled to room temperature to reduce the generation of thermal stress during the cooling process.

7. A reaction kettle, characterized in that: It comprises a metal film tube treated by the surface treatment method of a metal film tube as described in any one of claims 1 to 6, wherein the antimagnetic coating on the metal film tube is used to inhibit the magnetic adsorption of the chelating agent to the metal film tube.

8. The reactor according to claim 7, characterized in that: The reactor comprises: A reactor body having a closed space; A stirring device, located in the enclosed space of the reactor body, for stirring the reaction turbid liquid in the reactor body; A base, which is arranged on the inner wall of the closed space of the reactor body; The metal film tube is arranged on the base and is used to filter the reaction turbid liquid in the reactor body to obtain a reaction clear liquid, wherein the reaction clear liquid is located in the metal film tube; A decoupling tube has one end connected to the metal film tube and the other end penetrating the wall of the reactor body and extending to the outside of the reactor to discharge the reaction clear liquid in the metal film tube.

9. The reactor according to claim 8, characterized in that: One end of the metal film tube is detachably arranged on the base, and the other end of the metal film tube is connected to one end of the outlet tube.

10. The reactor according to claim 8, characterized in that: At least two bases are arranged on the inner wall of the enclosed space of the reactor body, each base is provided with at least two slots, the number of the metal film tubes corresponds to the same number of the slots, and one end of the metal film tube is fixed to the corresponding slot.

Citation Information

Patent Citations

  • Insulation coating for cathode of metal shaped tube electrochemical machining and preparation method of insulation coating

    CN109722109A

  • Mine explosion-proof diesel engine tail gas purification device and method

    CN112081645A

  • A cyclohexanone ammonium oxime reactor

    CN201596496U

  • Magnetism reation kettle

    CN208465848U

  • Ammoximation reaction device

    CN210065604U