Method for preparing metal composite nanomaterial by coupling laser with plasma, metal composite nanomaterial and electronic component coating
The preparation of metal composite nanomaterial coatings through laser-coupled plasma technology solves the problems of insufficient conductivity and anti-corrosion performance of metal coatings in the existing technology, and realizes electronic component coatings with high conductivity and corrosion resistance, forming a Excellent chromium oxide protective film.
Patent Information
- Application Number
- CN202410848322.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-22
AI Technical Summary
Existing metal coatings in electronic components have insufficient electrical conductivity and anti-corrosion properties due to large powder particles, and cannot meet the high conductivity and protection needs.
Laser-coupled plasma technology is used to prepare metal composite nanomaterials. By adding copper powder, rare earth oxides, chromium alloys and conductive additives to water, laser coupling processing and low-temperature cold trap powder deposition are performed to form conductive and corrosion-resistant metals. Composite nanomaterial coating, and coat it on the surface of electronic components through vacuum plating technology.
Significantly improves the conductivity and anti-corrosion performance of electronic component coatings, and the uniformity of nano-scale particle size forms an excellent chromium oxide protective film, enhancing the overall performance of the coating.
Smart Images

Figure CN118808637A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano material coatings, and in particular relates to a method for preparing a metal composite nano material coating using laser coupled plasma and an electronic component coating. Background Art
[0002] Metal coatings are widely used in electronic components and related connectors due to their conductivity. In integrated circuits during semiconductor manufacturing, metal coatings are applied to the outside of electronic components to provide conductivity and protection.
[0003] When used in electronic components and other fields, metal coatings are required to have good electrical conductivity and corrosion resistance. In the prior art, metal coatings are generally formed by electroplating metal powders. The particles of metal powders are relatively large, resulting in gaps in the metal coatings, which affects the electrical conductivity and corrosion resistance of the metal coatings. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a metal composite nano material coating by laser coupled plasma. The prepared metal composite nano material coating has good electrical conductivity and corrosion resistance.
[0005] Another object of the present invention is to provide an electronic component coating.
[0006] In order to achieve the above purpose, the technical solution adopted by the present invention is:
[0007] The method for preparing metal composite nanomaterials by laser coupled plasma comprises the following steps:
[0008] 1) adding a dispersant to water, and then sequentially adding copper powder, rare earth oxide, conductive additive and chromium alloy, and mixing them evenly to obtain a metal dispersion system, wherein the mass ratio of the copper powder to the rare earth oxide is 10:0.2-0.5; the mass ratio of the copper powder to the conductive additive is 10:1-1.5; the mass ratio of the copper powder to the chromium alloy is 10:0.8-1.2;
[0009] 2) subjecting the metal dispersion system in step 1) to laser coupled plasma treatment, and simultaneously using a low temperature cold trap for powder deposition to obtain a metal composite nanomaterial.
[0010] Furthermore, the copper powder has a particle size of 1 to 30 μm.
[0011] Furthermore, the rare earth oxide is Y2O3 or CeO2, and the chromium alloy is Cr 13 Al4.
[0012] Furthermore, the conductive additive is a mixture of graphene and graphite-phase carbon nitride, and the mass ratio of the graphene to the graphite-phase carbon nitride is 2 to 5:1.
[0013] Furthermore, the temperature of the low temperature cold trap is -10 to 0°C.
[0014] Furthermore, the mass ratio of the copper powder to water is 10:30-50, and the mass ratio of the copper powder to dispersant is 10:0.5-0.8.
[0015] Furthermore, the dispersant is a mixture of one or more of sodium hexametaphosphate, sodium tripolyphosphate and sodium pyrophosphate.
[0016] The metal composite nano material is prepared by adopting the method for preparing the metal composite nano material by laser coupled plasma.
[0017] Electronic component coating, the above metal composite nano material is mixed with water and coating dispersant to form metal slurry, and then the metal slurry is coated on the surface of the electronic component by vacuum plating to form a metal composite nano material coating.
[0018] Furthermore, the mass ratio of the metal composite nanomaterial to water is 1:3-5; the mass ratio of the metal composite nanomaterial to the coating dispersant is 1:0.2-0.4.
[0019] Beneficial effects of the present invention:
[0020] The laser coupled plasma method for preparing metal composite nanomaterials of the present invention can reduce the particle size of powders, fuse various substances together, and improve the conductivity and anti-corrosion performance of electronic component coatings.
[0021] The method for preparing metal composite nanomaterials by laser coupled plasma of the present invention is that the prepared metal composite material is in powder form with small and uniform particle size. The combination of rare earth oxide and copper improves the anti-corrosion performance of the electronic component coating. In addition, the addition of chromium alloy forms a chromium oxide protective film on the surface of the electronic component coating, thereby improving the anti-corrosion performance of the electronic component coating. At the same time, a conductive additive is added, the conductive additive contains graphene and graphite phase carbon nitride, and the addition of the conductive additive improves the conductive performance of the electronic component coating.
[0022] The laser coupled plasma method for preparing metal composite nanomaterials of the present invention uses a low temperature cold trap to deposit powders, which is conducive to adjusting the deposition rate and further regulating the size distribution of nano powders, and the obtained metal composite nanomaterial particles are relatively uniform. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The conductive properties of the electronic component coatings of Examples 1 to 3 and Comparative Examples 1 to 5;
[0024] Figure 2is the average particle size of the metal composite nanomaterials of Examples 1 to 3 and Comparative Examples 1 to 5;
[0025] Figure 3 This is an electron microscope image of the metal composite nanomaterial of Example 1;
[0026] Figure 4 This is an electron microscope image of the metal composite nanomaterial of Comparative Example 5;
[0027] Figure 5 This is an electron microscope image of the electronic component coating of Example 1;
[0028] Figure 6 This is an electron microscope image of the electronic component coating of Comparative Example 5. DETAILED DESCRIPTION
[0029] The present invention will be further described below in conjunction with the embodiments of the present invention.
[0030] Example 1
[0031] The method for preparing metal composite nanomaterials by laser coupled plasma of this embodiment comprises the following steps:
[0032] 1) Add 6g of dispersant to 400g of water, then add 100g of copper powder, 3g of rare earth oxide, 12g of conductive additive and 10g of chromium alloy in sequence, mix well to obtain a metal dispersion system. The particle size of the copper powder is 1 to 30μm. The rare earth oxide is Y2O3. The conductive additive is a mixture of graphene and graphite phase carbon nitride, and the mass ratio of graphene to graphite phase carbon nitride is 3:1. The chromium alloy is Cr 13 Al4. The dispersant is sodium hexametaphosphate.
[0033] 2) The metal dispersion system described in step 1) is moved to a laser coupling device, and the metal dispersion system is treated with a laser having a wavelength of 1064 nm, the laser power is set to 200 W, and the duration is 30 minutes to ensure that all materials are effectively coupled and activated. During the treatment process, a low-temperature cold trap technology is used to collect the generated nanoparticles. The cold trap temperature is set at -10°C to optimize the deposition effect of the nanoparticles to obtain a metal composite nanomaterial.
[0034] The metal composite nanomaterial of this embodiment is prepared by the above-mentioned method for preparing metal composite nanomaterial by laser coupled plasma.
[0035] The electronic component coating of this embodiment is to mix the above-mentioned metal composite nanomaterial with water and coating dispersant to form a metal slurry, put the metal slurry into a vacuum plating device, and spray it under a pressure of less than 5 Pa. The spraying time is controlled within 20 minutes to ensure that the surface of the electronic component is evenly covered with a thin and uniform layer of metal composite nanomaterial coating to form a metal composite nanomaterial coating. The mass ratio of the metal composite nanomaterial to water is 1:4; the mass ratio of the metal composite nanomaterial to the dispersant is 1:0.3, and the coating dispersant is sodium hexametaphosphate.
[0036] Example 2
[0037] The method for preparing metal composite nanomaterials by laser coupled plasma of this embodiment comprises the following steps:
[0038] 1) Add 8g of dispersant to 500g of water, then add 100g of copper powder, 5g of rare earth oxide, 15g of conductive additive and 8g of chromium alloy in sequence, mix well to obtain a metal dispersion system. The particle size of the copper powder is 1 to 30μm. The rare earth oxide is CeO2. The conductive additive is a mixture of graphene and graphite phase carbon nitride, and the mass ratio of graphene to graphite phase carbon nitride is 2:1. The chromium alloy is Cr 13 Al4. The dispersant is sodium tripolyphosphate.
[0039] 2) The metal dispersion system of step 1) is moved to a laser coupling device, and the metal dispersion system is treated with a laser with a wavelength of 1064nm, the laser power is set to 200W, and the duration is 30min, to ensure that all materials are effectively coupled and activated. During the treatment process, a low-temperature cold trap technology is used to collect the generated nanoparticles. The cold trap temperature is set at -10°C to optimize the deposition effect of the nanoparticles to obtain a metal composite nanomaterial.
[0040] The metal composite nanomaterial of this embodiment is prepared by the above-mentioned method for preparing metal composite nanomaterial by laser coupled plasma.
[0041] The electronic component coating of this embodiment is prepared by mixing the metal composite nanomaterial with water and a coating dispersant to form a metal slurry, placing the metal slurry in a vacuum plating device, and spraying it under a pressure of less than 5 Pa. The spraying time is controlled within 20 minutes to form a metal composite nanomaterial coating. The mass ratio of the metal composite nanomaterial to water is 1:3; the mass ratio of the metal composite nanomaterial to the coating dispersant is 1:0.4. The coating dispersant is sodium tripolyphosphate.
[0042] Example 3
[0043] The method for preparing metal composite nanomaterials by laser coupled plasma of this embodiment comprises the following steps:
[0044] 1) Add 5g of dispersant to 300g of water, then add 100g of copper powder, 2g of rare earth oxide, 10g of conductive additive and 12g of chromium alloy in sequence, and mix them evenly to obtain a metal dispersion system. The particle size of the copper powder is 1 to 30μm. The rare earth oxide is Y2O3. The conductive additive is a mixture of graphene and graphite phase carbon nitride, and the mass ratio of graphene to graphite phase carbon nitride is 5:1. The chromium alloy is C r13 Al4. The dispersant is sodium hexametaphosphate.
[0045] 2) The metal dispersion system is moved to a laser coupling device and treated with a laser having a wavelength of 1064 nm. The laser power is set to 200 W and the duration is 30 min to ensure that all materials are effectively coupled and activated. During the treatment process, a low-temperature cold trap technology is used to collect the generated nanoparticles. The cold trap temperature is set at -10°C to optimize the deposition effect of the nanoparticles to obtain a metal composite nanomaterial.
[0046] The metal composite nanomaterial of this embodiment is prepared by the above-mentioned method for preparing metal composite nanomaterial by laser coupled plasma.
[0047] The electronic component coating of this embodiment is prepared by mixing the metal composite nanomaterial with water and a coating dispersant to form a metal slurry, placing the metal slurry in a vacuum plating device, and spraying it under a pressure of less than 5 Pa. The spraying time is controlled within 20 minutes to form a metal composite nanomaterial coating. The mass ratio of the metal composite nanomaterial to water is 1:5; the mass ratio of the metal composite nanomaterial to the coating dispersant is 1:0.4. The coating dispersant is sodium hexametaphosphate.
[0048] Example 4
[0049] The method for preparing metal composite nanomaterials by laser coupled plasma of this embodiment comprises the following steps:
[0050] 1) Add 6g of dispersant to 400g of water, then add 100g of copper powder, 2g of rare earth oxide, 1.2g of conductive additive and 10g of chromium alloy in sequence, mix well to obtain a metal dispersion system. The particle size of the copper powder is 1 to 30μm. The rare earth oxide is CeO2. The conductive additive is a mixture of graphene and graphite phase carbon nitride, and the mass ratio of graphene to graphite phase carbon nitride is 3:1. The chromium alloy is Cr 13 Al4. The dispersant is sodium hexametaphosphate.
[0051] 2) The metal dispersion system is moved to a laser coupling device and treated with a laser having a wavelength of 1064 nm. The laser power is set to 200 W and the duration is 30 min to ensure that all materials are effectively coupled and activated. During the treatment process, a low-temperature cold trap technology is used to collect the generated nanoparticles. The cold trap temperature is set at -10°C to optimize the deposition effect of the nanoparticles to obtain a metal composite nanomaterial.
[0052] The metal composite nanomaterial of this embodiment is prepared by the above-mentioned method for preparing metal composite nanomaterial by laser coupled plasma.
[0053] The electronic component coating of this embodiment is prepared by mixing the metal composite nanomaterial with water and a coating dispersant to form a metal slurry, placing the metal slurry in a vacuum plating device, and spraying it under a pressure of less than 5 Pa. The spraying time is controlled within 20 minutes to form a metal composite nanomaterial coating. The mass ratio of the metal composite nanomaterial to water is 1:3; the mass ratio of the metal composite nanomaterial to the coating dispersant is 1:0.2. The coating dispersant is sodium hexametaphosphate.
[0054] Example 5
[0055] The method for preparing metal composite nanomaterials by laser coupled plasma of this embodiment comprises the following steps:
[0056] 1) Add 7g of dispersant to 300g of water, then add 100g of copper powder, 5g of rare earth oxide, 15g of conductive additive and 8g of chromium alloy in sequence, mix well to obtain a metal dispersion system. The particle size of the copper powder is 1 to 30μm. The rare earth oxide is Y2O3. The conductive additive is a mixture of graphene and graphite phase carbon nitride, and the mass ratio of graphene to graphite phase carbon nitride is 4:1. The chromium alloy is Cr 13 Al4. The dispersant is sodium pyrophosphate.
[0057] 2) The metal dispersion system described in step 1) is moved to a laser coupling device, and the metal dispersion system is treated with a laser having a wavelength of 1064 nm, the laser power is set to 200 W, and the duration is 30 minutes to ensure that all materials are effectively coupled and activated. During the treatment process, a low-temperature cold trap technology is used to collect the generated nanoparticles. The cold trap temperature is set at -10°C to optimize the deposition effect of the nanoparticles to obtain a metal composite nanomaterial.
[0058] The metal composite nanomaterial of this embodiment is prepared by the above-mentioned method for preparing metal composite nanomaterial by laser coupled plasma.
[0059] The electronic component coating of this embodiment is to mix the above-mentioned metal composite nanomaterial with water and coating dispersant to form a metal slurry, put the metal slurry into a vacuum plating device, and spray it under a pressure of less than 5 Pa. The spraying time is controlled within 20 minutes to form a metal composite nanomaterial coating. The mass ratio of the metal composite nanomaterial to water is 1:5; the mass ratio of the metal composite nanomaterial to the coating dispersant is 1:0.4. The coating dispersant is sodium pyrophosphate.
[0060] Comparative Example 1
[0061] The method for preparing metal composite nanomaterials by laser coupled plasma in this comparative example comprises the following steps:
[0062] 1) Add 6 g of dispersant to 400 g of water, then add 100 g of copper powder, mix well to obtain a metal dispersion system, wherein the particle size of the copper powder is 1 to 30 μm. The dispersant is sodium hexametaphosphate.
[0063] 2) The metal dispersion system described in step 1) is moved to a laser coupling device, and the metal dispersion system is treated with a laser having a wavelength of 1064 nm, the laser power is set to 200 W, and the duration is 30 minutes to ensure that all materials are effectively coupled and activated. During the treatment process, a low-temperature cold trap technology is used to collect the generated nanoparticles. The cold trap temperature is set at -10°C to optimize the deposition effect of the nanoparticles to obtain a metal composite nanomaterial.
[0064] The metal composite nanomaterial of this comparative example is prepared by adopting the above-mentioned method for preparing metal composite nanomaterial by laser coupled plasma.
[0065] The electronic component coating of this embodiment is to mix the above-mentioned metal composite nanomaterial with water and coating dispersant to form a metal slurry, put the metal slurry into a vacuum plating device, and spray it under a pressure of less than 5 Pa. The spraying time is controlled within 20 minutes to ensure that the surface of the electronic component is evenly covered with a thin and uniform layer of metal composite nanomaterial coating to form a metal composite nanomaterial coating. The mass ratio of the metal composite nanomaterial to water is 1:4; the mass ratio of the metal composite nanomaterial to the dispersant is 1:0.3, and the coating dispersant is sodium hexametaphosphate.
[0066] Comparative Example 2
[0067] The method for preparing metal composite nanomaterials by laser coupled plasma in this comparative example comprises the following steps:
[0068] 1) Add 6g of dispersant to 400g of water, then add 100g of copper powder, 3g of rare earth oxide, 12g of conductive additive and 10g of chromium alloy in sequence, and mix them evenly to obtain a metal dispersion system. The particle size of the copper powder is 1 to 30μm. The rare earth oxide is Y2O3. The conductive additive is graphene. The chromium alloy is Cr 13 Al4. The dispersant is sodium hexametaphosphate.
[0069] 2) The metal dispersion system described in step 1) is moved to a laser coupling device, and the metal dispersion system is treated with a laser having a wavelength of 1064 nm, the laser power is set to 200 W, and the duration is 30 minutes to ensure that all materials are effectively coupled and activated. During the treatment process, a low-temperature cold trap technology is used to collect the generated nanoparticles. The cold trap temperature is set at -10°C to optimize the deposition effect of the nanoparticles to obtain a metal composite nanomaterial.
[0070] The metal composite nanomaterial of this comparative example is prepared by adopting the above-mentioned method for preparing metal composite nanomaterial by laser coupled plasma.
[0071] The electronic component coating of this embodiment is to mix the above-mentioned metal composite nanomaterial with water and coating dispersant to form a metal slurry, put the metal slurry into a vacuum plating device, and spray it under a pressure of less than 5 Pa. The spraying time is controlled within 20 minutes to ensure that the surface of the electronic component is evenly covered with a thin and uniform layer of metal composite nanomaterial coating to form a metal composite nanomaterial coating. The mass ratio of the metal composite nanomaterial to water is 1:4; the mass ratio of the metal composite nanomaterial to the dispersant is 1:0.3, and the coating dispersant is sodium hexametaphosphate.
[0072] Comparative Example 3
[0073] The method for preparing metal composite nanomaterials by laser coupled plasma in this comparative example comprises the following steps:
[0074] 1) Add 6g of dispersant to 400g of water, then add 100g of copper powder, 12g of conductive additive and 10g of chromium alloy in sequence, mix well to obtain a metal dispersion system. The particle size of the copper powder is 1 to 30μm. The conductive additive is a mixture of graphene and graphite phase carbon nitride, and the mass ratio of graphene to graphite phase carbon nitride is 3:1. The chromium alloy is Cr 13 Al4. The dispersant is sodium hexametaphosphate.
[0075] 2) The metal dispersion system described in step 1) is moved to a laser coupling device, and the metal dispersion system is treated with a laser having a wavelength of 1064 nm, the laser power is set to 200 W, and the duration is 30 minutes to ensure that all materials are effectively coupled and activated. During the treatment process, a low-temperature cold trap technology is used to collect the generated nanoparticles. The cold trap temperature is set at -10°C to optimize the deposition effect of the nanoparticles to obtain a metal composite nanomaterial.
[0076] The metal composite nanomaterial of this comparative example is prepared by adopting the above-mentioned method for preparing metal composite nanomaterial by laser coupled plasma.
[0077] The electronic component coating of this embodiment is to mix the above-mentioned metal composite nanomaterial with water and coating dispersant to form a metal slurry, put the metal slurry into a vacuum plating device, and spray it under a pressure of less than 5 Pa. The spraying time is controlled within 20 minutes to ensure that the surface of the electronic component is evenly covered with a thin and uniform layer of metal composite nanomaterial coating to form a metal composite nanomaterial coating. The mass ratio of the metal composite nanomaterial to water is 1:4; the mass ratio of the metal composite nanomaterial to the dispersant is 1:0.3, and the coating dispersant is sodium hexametaphosphate.
[0078] Comparative Example 4
[0079] The method for preparing metal composite nanomaterials by laser coupled plasma in this comparative example comprises the following steps:
[0080] 1) Add 6g of dispersant to 400g of water, then add 100g of copper powder, 3g of rare earth oxide, and 12g of conductive additive in sequence, and mix them evenly to obtain a metal dispersion system; the particle size of the copper powder is 1 to 30μm. The rare earth oxide is Y2O3. The conductive additive is a mixture of graphene and graphite phase carbon nitride, and the mass ratio of graphene to graphite phase carbon nitride is 3:1. The chromium alloy is Cr 13 Al4. The dispersant is sodium hexametaphosphate.
[0081] 2) The metal dispersion system described in step 1) is moved to a laser coupling device, and the metal dispersion system is treated with a laser having a wavelength of 1064 nm, the laser power is set to 200 W, and the duration is 30 minutes to ensure that all materials are effectively coupled and activated. During the treatment process, a low-temperature cold trap technology is used to collect the generated nanoparticles. The cold trap temperature is set at -10°C to optimize the deposition effect of the nanoparticles to obtain a metal composite nanomaterial.
[0082] The metal composite nanomaterial of this comparative example is prepared by adopting the above-mentioned method for preparing metal composite nanomaterial by laser coupled plasma.
[0083] The electronic component coating of this embodiment is to mix the above-mentioned metal composite nanomaterial with water and coating dispersant to form a metal slurry, put the metal slurry into a vacuum plating device, and spray it under a pressure of less than 5 Pa. The spraying time is controlled within 20 minutes to ensure that the surface of the electronic component is evenly covered with a thin and uniform layer of metal composite nanomaterial coating to form a metal composite nanomaterial coating. The mass ratio of the metal composite nanomaterial to water is 1:4; the mass ratio of the metal composite nanomaterial to the dispersant is 1:0.3, and the coating dispersant is sodium hexametaphosphate.
[0084] Comparative Example 5
[0085] The method for preparing metal composite nanomaterials by laser coupled plasma in this comparative example comprises the following steps:
[0086] 1) Add 6g of dispersant to 400g of water, then add 100g of copper powder, 3g of rare earth oxide, 12g of conductive additive and 10g of chromium alloy in sequence, mix well to obtain a metal dispersion system. The particle size of the copper powder is 1 to 30μm. The rare earth oxide is Y2O3. The conductive additive is a mixture of graphene and graphite phase carbon nitride, and the mass ratio of graphene to graphite phase carbon nitride is 3:1. The chromium alloy is Cr 13 Al4. The dispersant is sodium hexametaphosphate.
[0087] 2) The metal dispersion system in step 1) is moved to a laser coupling device, and the metal dispersion system is treated with a laser having a wavelength of 1064 nm, the laser power is set to 200 W, and the duration is 30 minutes to ensure that all materials are effectively coupled and activated, thereby obtaining a metal composite nanomaterial.
[0088] The metal composite nanomaterial of this comparative example is prepared by adopting the above-mentioned method for preparing metal composite nanomaterial by laser coupled plasma.
[0089] The electronic component coating of this embodiment is to mix the above-mentioned metal composite nanomaterial with water and coating dispersant to form a metal slurry, put the metal slurry into a vacuum plating device, and spray it under a pressure of less than 5 Pa. The spraying time is controlled within 20 minutes to ensure that the surface of the electronic component is evenly covered with a thin and uniform layer of metal composite nanomaterial coating to form a metal composite nanomaterial coating. The mass ratio of the metal composite nanomaterial to water is 1:4; the mass ratio of the metal composite nanomaterial to the dispersant is 1:0.3, and the coating dispersant is sodium hexametaphosphate.
[0090] Test Example 1
[0091] The conductivity of the electronic component coatings of Examples 1 to 3 and Comparative Examples 1 to 5 was tested using a Sigma 2008B1 digital conductivity meter. The results are as follows: Figure 1 shown.
[0092] Test Example 2
[0093] The average particle size of the metal composite nanomaterials of Examples 1 to 3 and Comparative Examples 1 to 5 was measured. The results are as follows: Figure 2 shown.
[0094] Test Example 3
[0095] The corrosion resistance of the electronic component coatings of Examples 1 to 3 and Comparative Examples 1 to 5 was measured, and the results are shown in Table 1.
[0096] Table 1 Corrosion resistance of electronic component coatings of Examples 1 to 3 and Comparative Examples 1 to 5
[0097]
[0098] The particle sizes of the metal composite nanomaterials in Table 1 are all the particle sizes of the particles treated by laser coupled plasma.
[0099] From Table 1, Figure 1 and Figure 2 It can be seen that the electronic component coating of the present invention has good conductivity. After adding rare earth oxides, chromium alloys and conductive additives in Example 1, the corrosion resistance is good and does not affect the conductivity. Comparative Example 1 uses copper powder alone, and the corrosion resistance is poor. In Comparative Example 2, the conductive additive is graphene, and the conductivity is poor, which shows that graphene and graphite phase carbon nitride cooperate with each other to improve the conductivity. No rare earth oxides were added in Comparative Example 3, and no chromium alloy was added in Comparative Example 4, and the corrosion resistance was poor. In Comparative Example 5, no low-temperature cold trap was used for powder deposition, and the average particle size of the metal composite nanomaterial was large, and the conductivity and corrosion resistance were poor. Figure 3 and Figure 4 It can be seen that when a low-temperature cold trap is used for powder deposition, the particles of the metal composite nanomaterial are smaller and the particle size is more uniform. When a low-temperature cold trap is not used for powder deposition, the particles of the metal composite nanomaterial are larger. Figure 5 and Figure 6 It can be seen that the surface of the electronic component coating formed by using the metal composite nanomaterial formed by low-temperature cold trap deposition of powder is uniform and flat, without large clustered accumulation structures; since the electronic component coating is formed by the accumulation of nano-scale metal composite nanomaterials, the agglomeration of metal composite nanomaterials with larger particles can be effectively avoided, thereby forming an electronic component coating with an uneven surface.
Claims
1. A method for preparing metal composite nanomaterials by laser coupled plasma, characterized in that: The following steps are involved: 1) adding a dispersant to water, and then sequentially adding copper powder, rare earth oxide, conductive additive and chromium alloy, and mixing them evenly to obtain a metal dispersion system, wherein the mass ratio of the copper powder to the rare earth oxide is 10:0.2-0.5; the mass ratio of the copper powder to the conductive additive is 10:1-1.5; the mass ratio of the copper powder to the chromium alloy is 10:0.8-1.2; 2) subjecting the metal dispersion system in step 1) to laser coupled plasma treatment, and simultaneously using a low temperature cold trap for powder deposition to obtain a metal composite nanomaterial.
2. The method for preparing metal composite nanomaterials by laser coupled plasma according to claim 1, characterized in that: The copper powder has a particle size of 1 to 30 μm.
3. The method for preparing metal composite nanomaterials by laser coupled plasma according to claim 1, characterized in that: The rare earth oxide is Y2O3 or CeO2, and the chromium alloy is Cr 13 Al4.
4. The method for preparing metal composite nanomaterials by laser coupled plasma according to claim 1, characterized in that: The conductive additive is a mixture of graphene and graphite-phase carbon nitride, and the mass ratio of the graphene to the graphite-phase carbon nitride is 2 to 5:
1.
5. The method for preparing metal composite nanomaterials by laser coupled plasma according to claim 1, characterized in that: The temperature of the low temperature cold trap is -10 to 0°C.
6. The method for preparing metal composite nanomaterials by laser coupled plasma according to claim 1, characterized in that: The mass ratio of the copper powder to water is 10:30-50, and the mass ratio of the copper powder to dispersant is 10:0.5-0.
8.
7. The method for preparing metal composite nanomaterials by laser coupled plasma according to claim 1, characterized in that: The dispersant is a mixture of one or more of sodium hexametaphosphate, sodium tripolyphosphate and sodium pyrophosphate.
8. A metal composite nanomaterial, characterized in that: The metal composite nanomaterial is prepared by the method for preparing metal composite nanomaterials by laser coupled plasma in claim 1.
9. Electronic component coating, characterized in that The metal composite nanomaterial according to claim 8 is mixed with water and a coating dispersant to form a metal slurry, and then the metal slurry is coated on the surface of the electronic component by vacuum plating to form a metal composite nanomaterial coating.
10. The electronic component coating according to claim 9, characterized in that: The mass ratio of the metal composite nano material to water is 1:3-5; the mass ratio of the metal composite nano material to the coating dispersant is 1:0.2-0.4.