Ultrahigh-sensitivity colloidal gold nanoparticle as well as preparation method and application thereof

By growing Au nanoparticles in situ on dendritic mesoporous silica nanoparticles, ultra-highly sensitive gold colloidal nanospheres are prepared, which solves the problems of low stability and sensitivity of traditional colloidal gold and achieves higher detection sensitivity and Stable and suitable for immunochromatographic diagnosis.

CN118808666APending Publication Date: 2024-10-22CHINA PHARM UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410847857.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-22

Smart Images

  • Figure CN118808666A_ABST
    Figure CN118808666A_ABST
Patent Text Reader

Abstract

The invention discloses an ultrahigh-sensitivity colloidal gold nanoparticle as well as a preparation method and application thereof, and belongs to the technical field of colloidal gold labeling, the method comprises the following steps: synthesizing dendritic mesoporous silica nanoparticles DMSNs with a central radial aperture; carrying out surface amination treatment on the synthesized dendritic mesoporous silica nanoparticles DMSNs with the central radial aperture to obtain aminated mesoporous silica microspheres; the preparation method comprises the following steps: depositing Au (OH) 3 nanoparticles as nucleation sites by using aminated mesoporous silica microspheres to obtain gold dendritic mesoporous silica nanoparticles DMSNs; au nanoparticles grow in situ by using nucleation sites on the surfaces of gold dendritic mesoporous silica nanoparticles DMSNs, and the ultra-high-sensitivity colloidal gold nanoparticles are synthesized; according to the invention, the AuNPs composite nanomaterial can present deeper purple, the color signal intensity is amplified, and the visual detection effect is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of colloidal gold labeling, and specifically relates to an ultra-high-sensitivity gold colloidal nano-microsphere and a preparation method and application thereof. Background Art

[0002] The immunochromatography process uses antigen-antibody labeling reagents, which can achieve rapid diagnosis of diseases through specific recognition and binding of disease markers. Traditional immunochromatography technology uses colloidal gold as a marker. Colloidal gold has a high electron density, can adsorb biomacromolecules without affecting the activity of biomolecules, and has bright colors. It can be used to qualitatively detect or semi-quantitatively analyze the target through strip color development. However, the stability of colloidal gold is easily affected by the pH value of the environment. If the pH value deviates from the optimal range, it may cause colloidal gold aggregation. At the same time, the sensitivity of antigen detection using colloidal gold as a marker is relatively low, which is a typical limitation in the application of immunochromatography. This has brought continuous obstacles to detection and highlighted the need for further research to improve its sensitivity and accuracy. In order to improve the sensing performance, researchers have studied methods including silver enhancement, double gold binding, and gold aggregation to increase the size of colloidal gold and improve the absorbance of colloidal gold to obtain higher colorimetric contrast. However, these methods have disadvantages such as the instability of chemical reagents and the inevitable additional steps of chemical enhancement of the signal of the test line, which limits their widespread application. At the same time, various colloidal gold assembly techniques have been reported to improve light absorption, including nanoaggregates, nanoclusters, and nanocarriers. These nanocomposites have different optical properties from single colloidal gold and can be used to establish sensitive, simple, and rapid detection systems. Dendritic mesoporous silica nanoparticles (DMSNs) have uniform particle size, rigid structure, large pore channels, and high available surface area, and can be enriched with a variety of labels for signal amplification and ultrasensitive detection.

[0003] Typically, the seeding of gold nanoparticles on silica is synthesized using a two-step process, i.e., gold nanoparticles are first formed by reduction of gold salts by strong reducing agents, followed by grafting of amino-terminated silane coupling agents onto the silica surface to give the silica a nucleophilic surface for coordination bonding with colloidal gold particles. These small colloids of gold are usually formed by reduction of gold salts by strong reducing agents, and may require several days of aging, up to 2 weeks for their size to stabilize, before being seeded onto the surface-functionalized silica core. While this common two-step seeding process (i.e., formation of small colloidal gold followed by attachment to the core) is effective, it is also laborious and expensive in terms of time and expense. A different surface seeding strategy has also been reported to prepare the surface - precipitation-deposition method, where the silica support is contacted with an aqueous solution of gold(III) chloride, the pH of which is raised by the addition of a base, thereby forming oxide precursor particles on the support upon heating. The size and density of the nanoparticle gold on the substrate are easily controlled by the concentration of gold(II) chloride, the type of supporting substrate, the reaction temperature and time, and the pH of the reaction. At the same time, the spatial limitation of the carrier improves the problem that the colloidal gold nanoparticles have a low melting point, high surface free energy and are easy to aggregate, which may lead to the colloidal gold nanoparticles being unable to contact the reactants during the reaction. Therefore, it is necessary to study an ultra-high sensitive gold colloidal nanosphere. Summary of the invention

[0004] The purpose of the present invention is to provide an ultra-high sensitive gold colloid nanosphere and its preparation method and application in immunochromatographic diagnosis, which retains the color development characteristics of colloidal gold, enables AuNPs composite nanomaterials to present a deeper purple color, amplifies the color signal intensity, and enhances the visual detection effect without further modification to improve its stability.

[0005] The purpose of the present invention is to be achieved through the following technical solutions:

[0006] In a first aspect, the present invention provides a method for preparing ultra-high sensitive gold colloid nanoparticles, the method comprising the following steps:

[0007] Step S1: Synthesizing dendritic mesoporous silica nanoparticles (DMSNs) with central radial pores;

[0008] Step S2: performing surface amination treatment on the dendritic mesoporous silica nanoparticles DMSNs with central radial pores synthesized in step S1 to obtain amination mesoporous silica microspheres;

[0009] Step S3: Depositing Au(OH) using the amino-modified mesoporous silica microspheres obtained in step S2 3 Nanoparticles were used as nucleation sites to obtain gold-seeded dendritic mesoporous silica nanoparticles DMSNs;

[0010] Step S4: using the nucleation sites on the surface of the gold-seeded dendritic mesoporous silica nanoparticles DMSNs obtained in step S3 to in-situ grow Au nanoparticles to synthesize ultra-high sensitivity gold colloid nanospheres.

[0011] Furthermore, the method for synthesizing the dendritic mesoporous silica nanoparticles DMSNs with central radial pores in step S1 is: adding triethanolamine to deionized water, adding hexadecyltrimethylammonium bromide and sodium salicylate under heating and stirring conditions for reaction; then adding tetraethyl orthosilicate for further reaction, washing with ethanol to remove unreacted products after the reaction, and collecting by centrifugation; then dispersing in an acidic methanol mixed solution and heating for reaction to remove the template agent hexadecyltrimethylammonium bromide; and finally centrifuging to obtain the dendritic mesoporous silica nanoparticles DMSNs with central radial pores.

[0012] The molar ratio of triethanolamine, hexadecyltrimethylammonium bromide, sodium salicylate and ethyl orthosilicate is 1:2.3:2.3:39.2.

[0013] The acidic methanol mixed solution is methanol and hydrochloric acid, and the volume ratio thereof is: methanol:hydrochloric acid=9:1.

[0014] Furthermore, step S2 is specifically as follows: dispersing the dendritic mesoporous silica nanoparticles DMSNs with central radial pores synthesized in step 1) in 100 mL of ethanol solution, adding 1.8 mL of 3-aminopropyltriethoxysilane and 3 mL of ammonium hydroxide to the solution system, vigorously stirring the reaction at room temperature for 12 h, and finally collecting by centrifugation, washing and purifying with ethanol three times, and freeze-drying the precipitate after centrifugation to obtain amino-modified mesoporous silica microspheres.

[0015] Further, step S3 is specifically: preparing a solution of the amino-modified mesoporous silica microspheres obtained in step S2 and adding the solution to Au(OH) 3 The solution was heated to 70°C and kept under vigorous stirring for 1 h to induce Au(OH) 3 The gold-seeded dendritic mesoporous silica nanoparticles (DMSNs) were obtained by deposition on the surface of amino-treated mesoporous silica.

[0016] Further, step S4 is specifically as follows: the gold-seeded dendritic mesoporous silica nanoparticles DMSNs obtained in step S3 are dispersed in water, 0.15 mL of the gold-seeded dendritic mesoporous silica nanoparticles DMSNs solution is added to 8 mL of K-gold solution, stirred at 25 ° C for 15 min, and 800 μL of 6.6 mM NaBH 4As a reducing agent, stir for 20 minutes; add 100 μL 10 mM trisodium citrate as a capping agent for every 2 ml K-gold and continue the reaction for 15 minutes. After the reaction, centrifuge and dilute and wash with deionized water to remove unreacted substances in the solution to synthesize ultra-high sensitive gold colloid nanospheres.

[0017] According to another aspect of the present invention, there is provided an ultra-high sensitive gold colloid nano-microsphere prepared by the above preparation method, comprising silica nanoparticles and gold nanoparticles in situ grown on amino-modified mesoporous silica.

[0018] According to another aspect of the present invention, the use of the ultra-high sensitive gold colloid nanoparticles in immunochromatographic detection of PSA samples is also provided; the prepared gold colloid nanoparticles present a deeper purple color, amplify the color signal intensity, and enhance the visual detection effect.

[0019] The present invention has the following beneficial effects: the method for preparing ultra-high-sensitivity gold colloid nano-microspheres provided by the present invention uses dendritic silica nano-particles with central radial pores as carriers, provides a large amount of internal space for gold nano-particle assembly, and deposits and grows in situ on the aminated mesoporous silica by amination treatment; in a one-step process, the gold nano-particles are inoculated onto the dendritic mesoporous silica core without the need to pre-synthesize colloidal gold. At the same time, the gold colloid nano-microspheres have a strong color signal intensity. Compared with the pure colloidal gold immunochromatography technology used on the market, the highly sensitive colloidal gold nano-microspheres of the present invention contain a large amount of AuNPs, which can significantly amplify the color signal intensity of AuNPs, and can be used for the development of diagnostic test paper products to obtain products with stronger stability and higher sensitivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a schematic diagram of the synthesis of ultra-high sensitive gold colloid nanoparticles of the present invention;

[0021] Figure 2 This is a transmission electron microscope image of the ultra-high sensitive gold colloid nanospheres prepared in Example 1;

[0022] Figure 3 The particle size diagram of the ultra-high sensitive gold colloid nanoparticles prepared in Example 1;

[0023] Figure 4 is the zeta potential of the ultra-high sensitive gold colloid nanospheres prepared in Example 1;

[0024] Figure 5 is the UV-visible absorption spectrum of the ultra-high sensitive gold colloid nanospheres prepared in Example 1;

[0025] Figure 6is the infrared spectrum of the ultra-high sensitive gold colloid nanospheres prepared in Example 1;

[0026] Figure 7 This is an example diagram of the ultra-high sensitive gold colloid nanoparticles prepared in Example 1 in an immunochromatographic test strip;

[0027] Figure 8 This is an example of traditional colloidal gold in immunochromatographic test strips. DETAILED DESCRIPTION

[0028] In order to help people in the relevant technical field better understand the content of the patent of the present invention, the embodiments of the present invention are described in detail below. This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and specific operation process are given, but the content of the present invention is not limited to the following examples.

[0029] Embodiment 1:

[0030] 1. Preparation of ultra-high sensitivity gold colloid nanoparticles

[0031] Figure 1 Schematic diagram of the synthesis process of ultra-high sensitive gold colloid nanoparticles. The specific preparation process is as follows:

[0032] 1) Synthesis of dendritic mesoporous silica nanoparticles DMSNs with central radial pores: Weigh 68 mg of triethanolamine and dissolve it in 25 mL of deionized water, stir at 80 ° C for 30 min, then add 380 mg of hexadecyltrimethylammonium bromide (CTAB) and 168 mg of sodium salicylate to continue the reaction for 1 h, then add 4 mL of tetraethyl orthosilicate (TEOS) to continue the reaction for 4 h, collect by centrifugation after the reaction is completed and wash with ethanol. Redisperse in an acidic methanol solution (a mixed solution of 45 mL of methanol and 5 mL of hydrochloric acid), heat and reflux at 60 ° C for 6 h, and repeat this step three times to remove the template CTAB. Finally, ethanol centrifugation purification is performed 3 times.

[0033] 2) Surface amination treatment of dendritic mesoporous silica nanoparticles DMSNs with central radial pores: The mesoporous silica nanoparticles synthesized in step 1) were dispersed in 100 mL of ethanol solution, 1.8 mL of 3-aminopropyltriethoxysilane (APTES) and 3 mL of ammonium hydroxide were added to the solution system, and the reaction was vigorously stirred at room temperature for 12 h. Finally, the mixture was collected by centrifugation, purified by ethanol washing 3 times, and the precipitate after centrifugation was freeze-dried.

[0034] 3) Synthesis of ultra-high sensitive gold colloid nanoparticles:

[0035] a. Take 2mL 0.1M NaOH and 0.45mL 6.35mM HAuCl 4The solution was reacted in a glassware treated with aqua regia for 15 min at room temperature. 4 The hydrolysis of the gold hydroxide [Au(OH) 3 ] solution, add 0.4 mL of a 20 mg / mL solution made of freeze-dried amino-modified mesoporous silica microspheres, heat to 70 °C, and keep under vigorous stirring for 1 h to induce Au(OH) 3 The gold-seeded dendritic mesoporous silica nanoparticles DMSNs were deposited on the surface of amino-modified mesoporous silica. After centrifugation, the gold-seeded dendritic mesoporous silica nanoparticles DMSNs were diluted and washed twice with anhydrous ethanol and deionized water respectively, and dispersed in 1 mL of water.

[0036] b. Take 60 mg of anhydrous potassium carbonate K 2 CO 3 and 1.5 mL 25 mM HAuCl 4 Add 100 mL of water and age overnight in the dark to obtain a K-gold solution;

[0037] c. Add 0.15 mL of the above gold-seeded mesoporous silica solution to 8 mL of K-gold solution and stir at 25 °C for 15 min. Add 800 μL of freshly prepared 6.6 mM NaBH 4 As a reducing agent, stir for 20 minutes. Add 100 μL of 10 mM trisodium citrate as a capping agent for every 2 ml of K-gold and continue the reaction for 15 minutes. After the reaction is completed, centrifuge and dilute and wash with deionized water to remove the unreacted substances in the solution, and disperse in 1 mL of water.

[0038] Figure 2 This is a transmission electron microscope image of the prepared ultra-high sensitivity gold colloid nanospheres. Figure 2 The test results show that the pore size of the dendritic mesoporous silica nanoparticles DMSNs with central radial pores is about 20 mm, and a large amount of colloidal gold is loaded in them. Figure 3 The particle size diagram of the prepared ultra-high sensitive gold colloid nanospheres. According to the test results, the size of the dendritic mesoporous silica nanoparticles DMSNs with central radial pores is about 250nm. Figure 4 The zeta potential of the ultra-high sensitive gold colloid nanospheres prepared is shown in Figure 2. According to the test results, due to the presence of silanol groups, the zeta potential of the bare dendritic mesoporous silica nanoparticles DMSNs is negative, and the potential becomes positive after amination. After the Au nanoparticles are in situ deposited and grown on the surface of the amination-treated mesoporous silica microspheres, the positive charge on the surface is transferred to a negative charge. Figure 5 The UV-visible absorption spectrum and infrared absorption spectrum of the prepared ultra-high sensitive gold colloid nanospheres. According to the test results, after Au nanoparticles were in situ deposited and grown on the surface of amino-modified mesoporous silica microspheres, a characteristic absorption peak of Au appeared at 539nm. Figure 6 This is the infrared absorption spectrum of the prepared ultra-high sensitive gold colloid nanospheres. According to the test results, the absorption spectra at 797, 958 and 1067 cm -1 The peaks at 4 and 13 belong to the bending vibration of Si-O-Si, the stretching vibration of Si-OH and the stretching vibration of Si-O-Si respectively. The above results indicate that Au nanoparticles are successfully fixed on the dendritic mesoporous silica nanoparticles DMSNs.

[0039] Example 2: Experimental process of ultra-high sensitivity gold colloid nanospheres in immunochromatographic detection of PSA samples

[0040] Take 100 μL of the 10 mg / mL gold colloid nanospheres prepared in Example 1, add 500 μL of 10 mM pH 8.0 Tris buffer to dissolve, ultrasonically disperse, centrifuge at 15000 rpm, 4°C for 5 min, and remove the supernatant. Add 500 μL of 10 mM pH 8.0 Tris buffer and 0.01% Tween 20 to the washed microspheres and ultrasonically disperse. Add 7.5 μg of prostate-specific antigen (PSA) antibody and chicken IgY antibody to the dispersed microsphere solution, respectively, and vortex quickly. Incubate at room temperature for 1 to 3 hours. Ultrasonic disperse the coupling solution, add 40 μL of bovine serum albumin (BSA) and 1.6 μL of blocking agent to the coupling solution, and vortex. Block at 37°C for 30 minutes to 1 hour. Wash 4 times with reconstitution solution (0.1mM pH 7.4PBS, 1% (w / v) BSA, 10% (w / v) sucrose, 0.01% casein), and dilute to 20μL with reconstitution solution and store at 4℃. Coat the conjugate pad after blocking and drying with conjugate pad pretreatment solution (10mM pH 7.4PBS, 1% (w / v) BSA, 0.5% (w / v) PVP, 5% (w / v) trehalose, 0.5% (w / v) skim milk, 0.1% Tween 20). Vacuum dry the coated strip. Block the sample pad with sample pad pretreatment solution (10mM pH7.4PBS, 1% (w / v) BSA, 0.5% (w / v) PVP, 0.9% (w / v) NaCl, 0.01% (w / v) sodium casein) and dry. Prepare the traditional colloidal gold test strip in the same way as above. Prepare the test strips: sample pad, conjugate pad, buffer pad, NC membrane, absorbent pad. Use human serum albumin to gradient dilute the PSA antigen standard to prepare 200, 100, 50, 10, 5, 4, 2, 1, 0.5, 0.1, 0.05, 0.01 ng / mL PSA antigen concentration standards, as well as a set of blank controls. Add 80 μL of the test solution at 18.5°C, incubate for 8 minutes, and observe. The test results are as follows: Figure 5As shown (the concentrations in the figure from left to right are 200, 100, 50, 10, 5, 4, 2, 1, 0.5, 0.1, 0.05, and 0.01 ng / mL).

[0041] When the sample contains antigen, the antigen first forms a complex with the PSA antibody labeled with the ultra-high sensitive gold colloid nano-microspheres on the binding pad. The complex is chromatographed toward the end of the absorbent pad due to capillary action. When flowing through the T line (quality inspection line), the complex can be captured and enriched by the PSA secondary antibody on the T line, and a purple strip visible to the naked eye may appear on the T line. The excess ultra-high sensitive gold colloid nano-microspheres are enriched by binding to the sheep anti-chicken IgY on the C line, and a purple strip visible to the naked eye may appear on the C line. When there is no antigen in the sample, the T line has no color strip, while the C line has a purple strip visible to the naked eye.

[0042] like Figure 7 , 8 As shown, it is an ultra-high sensitive gold colloid nanoparticle ( Figure 7 ) and the traditional quantum dot fluorescent microspheres prepared by electrostatic adsorption ( Figure 8 ) Test results of PSA antigen detection. The T-line band of the traditional colloidal gold was clearly visible at an antigen concentration of 4ng / mL (the T line is above the band and the C line is below the band), and the T-line band of the ultra-high sensitive gold colloidal nanospheres was clearly visible at an antigen concentration of 0.1ng / mL. The test results show that the ultra-high sensitive gold colloidal nanospheres have a lower detection limit than the traditional colloidal gold detection method.

[0043] The above description is only a preferred embodiment of the present invention and is not limited to the above implementation mode. Any equivalent modifications, equivalent substitutions and improvements made by ordinary technicians in this field based on the contents disclosed by the present invention should be included in the protection scope recorded in the claims.

Claims

1. A method for preparing ultra-high sensitive gold colloid nanoparticles, characterized in that: The method comprises the following steps: Step S1: Synthesizing dendritic mesoporous silica nanoparticles (DMSNs) with central radial pores; Step S2: performing surface amination treatment on the dendritic mesoporous silica nanoparticles DMSNs with central radial pores synthesized in step S1 to obtain amination mesoporous silica microspheres; Step S3: using the amino-modified mesoporous silica microspheres obtained in step S2 to deposit Au(OH)3 nanoparticles as nucleation sites to obtain gold-seeded dendritic mesoporous silica nanoparticles DMSNs; Step S4: using the nucleation sites on the surface of the gold-seeded dendritic mesoporous silica nanoparticles DMSNs obtained in step S3 to in-situ grow Au nanoparticles to synthesize ultra-high sensitivity gold colloid nanospheres.

2. The method for preparing ultra-high sensitive gold colloid nanoparticles according to claim 1, characterized in that: The method for synthesizing the dendritic mesoporous silica nanoparticles DMSNs with central radial pores in step S1 is as follows: adding triethanolamine to deionized water, adding hexadecyltrimethylammonium bromide and sodium salicylate under heating and stirring conditions to react; then adding tetraethyl orthosilicate for further reaction, washing with ethanol to remove unreacted products after the reaction is completed, and collecting by centrifugation; then dispersing in an acidic methanol mixed solution and heating to react to remove the template agent hexadecyltrimethylammonium bromide; and finally centrifuging to obtain the dendritic mesoporous silica nanoparticles DMSNs with central radial pores.

3. The method for preparing ultra-high sensitive gold colloid nanoparticles according to claim 2, characterized in that: The molar ratio of triethanolamine, hexadecyltrimethylammonium bromide, sodium salicylate and ethyl orthosilicate is 1:2.3:2.3:39.

2.

4. The method for preparing ultra-high sensitive gold colloid nanoparticles according to claim 2, characterized in that: The acidic methanol mixed solution is methanol and hydrochloric acid, and the volume ratio thereof is: Methanol: hydrochloric acid = 9:

1.

5. The method for preparing ultra-high sensitive gold colloid nanoparticles according to claim 1, characterized in that: Step S2 is specifically as follows: the dendritic mesoporous silica nanoparticles DMSNs with central radial pores synthesized in step 1) are dispersed in 100 mL of ethanol solution, 1.8 mL of 3-aminopropyltriethoxysilane and 3 mL of ammonium hydroxide are added to the solution system, the reaction is vigorously stirred at room temperature for 12 h, and finally centrifuged and collected, washed and purified with ethanol three times, and the precipitate after centrifugation is freeze-dried to obtain amino-modified mesoporous silica microspheres.

6. The method for preparing ultra-high sensitive gold colloid nanoparticles according to claim 1, characterized in that: Step S3 is specifically as follows: the aminated mesoporous silica microspheres obtained in step S2 are made into a solution and added to the Au(OH)3 solution, heated to 70°C, and maintained for 1 hour under vigorous stirring to induce Au(OH)3 to deposit on the surface of the aminated mesoporous silica to obtain gold-seeded dendritic mesoporous silica nanoparticles DMSNs.

7. The method for preparing ultra-high sensitive gold colloid nanoparticles according to claim 1, characterized in that: Step S4 is specifically as follows: the gold-seeded dendritic mesoporous silica nanoparticles DMSNs obtained in step S3 are dispersed in water, 0.15 mL of the gold-seeded dendritic mesoporous silica nanoparticles DMSNs solution is added to 8 mL of K-gold solution, stirred at 25°C for 15 min, 800 μL of 6.6 mM NaBH4 is added as a reducing agent, and stirred for 20 min; 100 μL of 10 mM trisodium citrate is added as a capping agent per 2 mL of K-gold and the reaction is continued for 15 min. After the reaction is completed, the solution is centrifuged and diluted and washed with deionized water to remove unreacted substances, thereby synthesizing ultra-high sensitive gold colloid nanospheres.

8. An ultra-high sensitive gold colloid nanoparticle, characterized in that: The gold colloid nanoparticles are obtained by the preparation method described in any one of claims 1 to 7.

9. Use of the ultra-high sensitive gold colloid nanoparticles according to claim 8 in immunochromatographic detection of PSA samples.