Mirror surface processing method for CVD reaction cavity for semiconductor and application of mirror surface processing method
Through the method of segmented forging and multi-process combination, the problem of material defects in CVD reaction chamber mirror processing is solved, the processing quality and corrosion resistance are improved, and the efficient production and long life of the CVD reaction chamber mirror structure are ensured.
Patent Information
- Application Number
- CN202410789114.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-06-19
AI Technical Summary
In CVD reaction chamber mirror processing, H62 brass materials are prone to material inclusions, cracks and other undesirable defects during the forging process, which affects the reliability and processing quality of later parts.
H62 brass ingots are forged using segmented forging and different forging speeds, combined with processes such as heat treatment, layered rough turning, contour winding fine turning, polishing and ultrasonic cleaning to ensure the internal grain refinement and surface finish of the material. , avoid defects and improve corrosion resistance through anodization.
The overall wall thickness of the mirror structure of the CVD reaction chamber is highly uniform and has no leakage points, which improves the processing quality and corrosion resistance and extends the service life.
Smart Images

Figure CN118809089A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of CVD reaction chamber processing, and in particular to a method for processing a mirror surface of a CVD reaction chamber for semiconductors and an application thereof. Background Art
[0002] CVD (Chemical Vapor Deposition) is a thin film deposition technology that converts gaseous reactants into solid substances through chemical reactions and deposits them on the surface of the wafer. It is an important process in semiconductor chip manufacturing. The uniformity of thin film deposition has a crucial impact on the yield of the final product. The CVD chamber is the place where the entire deposition reaction takes place. During the deposition process, there is multi-field coupling such as flow field, temperature field and plasma field.
[0003] According to the heating method of CVD, CVD can be divided into hot wall and cold wall. The common chemical vapor deposition system on the market is usually hot wall CVD, which directly relies on the temperature rise of the furnace to heat the growth area. The hot wall CVD process is relatively more mature, with lower preparation cost, and shows good reliability in material growth, so it is favored by many laboratories. The cold wall CVD system directly supplies power to heat the conductive substrate through a constant current source. There is no direct contact between the cavity wall and the sample. It is only slightly heated due to thermal radiation conduction, so it is called "cold wall". Its advantage is that its cooling rate can be controlled by the added constant current source, and the cooling rate can be controlled within a large range. At present, the manufacturers selling hot wall CVD equipment are mainly concentrated in China, the United States and some European countries, including well-known Applied Materials, Quantum Design, Oxford Instruments and firstnano, as well as Tianjin Zhonghuan, Xiamen Eleven Dimension, Hefei Kejing and other manufacturers. Cold wall CVD is mainly provided by foreign manufacturers such as Quantum Design.
[0004] The CVD chamber plays a great protective role in the process of atmospheric deposition. It is isolated from the outside atmosphere to ensure a stable deposition environment, which is critical to the cleanliness and purity of the materials deposited on the surface. The outer wall of this chamber has its own cooling water system, and the inner wall surface roughness requirements are very high. The inner wall needs to be gold-plated in the end. The raw material of the CVD chamber is brass H62, which is ordinary brass with good mechanical properties, good plasticity in hot state, good plasticity in cold state, good machinability, easy brazing and welding, corrosion resistance, but prone to corrosion cracking, and needs to be forged from small specifications to large diameter specifications, and the forging process must be hot forging. Hot forging is prone to material inclusions, cracks and other phenomena, all of which will cause certain risks to later parts. Summary of the invention
[0005] In view of the above-mentioned technical problems, the present invention provides a method for processing a mirror structure of a CVD reaction chamber for semiconductors and its application.
[0006] The technical solution of the present invention is: a method for processing a mirror structure of a CVD reaction chamber for a semiconductor, comprising the following steps:
[0007] S1, forging;
[0008] H62 brass ingots were selected as raw materials for heating and forging. The H62 brass ingots were placed in a vacuum furnace and heated to 700-1250°C. Then, they were forged 10 times to forge the H62 brass ingots from φ200mm to φ550mm part blanks.
[0009] During the forging process, the oxide scale on the surface of the H62 brass ingot is cleaned after each forging.
[0010] S2, parts processing;
[0011] S2-1, rough turning the blank obtained in step S1, and after the rough turning, heat treating the blank at a temperature of 500-800° C.;
[0012] S2-2, finishing turning the part blank after rough turning in step S1-1, the finishing turning process is divided into 3 to 5 feeds, and the cutting amount of each time is controlled to be 0.4 to 0.6 mm; after finishing turning, the left chamber of the CVD reaction chamber and the right chamber of the CVD reaction chamber are obtained;
[0013] S3. Welding
[0014] The left chamber of the CVD reaction chamber and the right chamber of the CVD reaction chamber obtained in step S2-2 are welded to obtain a CVD reaction chamber primary body, and then the CVD reaction chamber primary body is orthopedic to make the inner and outer diameter errors of the CVD reaction chamber primary body ≤ 0.2 mm;
[0015] S4, surface treatment;
[0016] The CVD reaction chamber precursor after the correction treatment in step S3 is polished, and then ground with grinding paste until the surface roughness of the inner wall of the CVD reaction chamber precursor reaches Ra0.5-0.8, and finally the CVD reaction chamber precursor is cleaned to obtain a finished CVD reaction chamber mirror structure.
[0017] Further, in step S1, during the 1st to 4th forging processes, the forging speed is controlled to be 50-70 m / min; during the 4th to 7th forging processes, the forging speed is controlled to be maintained at 150-200 m / min; during the 7th to 10th forging processes, the forging speed is controlled to be maintained at 220-300 m / min;
[0018] Description: By forging the H62 brass ingot in sections and controlling the forging speed in each stage, the internal grain refinement of the H62 brass ingot is made more uniform.
[0019] Furthermore, in step S2-1, the rough turning is performed on the part blank in layers, and the processing depth of each layer is controlled to be 5 to 10 mm; in step S2-2, the tool is processed layer by layer around the contour loop composed of all points at the same height along the axial direction of the part blank during fine turning, and the layer spacing and cutting width of each layer are controlled to be 2 to 4 mm;
[0020] Note: By rough turning the part blank in layers, the wear rate of the tool can be effectively reduced and the processing efficiency of the part blank can be improved; by using the contour line winding finishing method, the problem of extended processing cycle caused by excess interference or excessive excess affecting the processing quality during the finishing of the next layer of excess material can be avoided.
[0021] Furthermore, in step S4, during the polishing process, sandpaper from coarse to fine is used for polishing, and the roughness of the CVD reaction chamber primary body is tested after each polishing;
[0022] Note: By gradually polishing the CVD reaction chamber primary body, it is beneficial to improve the surface finish of the CVD reaction chamber primary body, thereby improving the use effect.
[0023] Furthermore, after step S1 is completed, the part blank is sealed and placed in an ammonia water container for 12 to 19 hours, and the part blank is controlled not to contact with the ammonia water;
[0024] Note: By sealing the blank part in an ammonia container, it is easy to detect defects such as cracks inside the blank part, avoiding the effect of the CVD reaction chamber mirror surface structure being affected after processing.
[0025] Furthermore, before step S1 is performed, the H62 brass ingot is preheated to 350-550° C.;
[0026] Note: Preheating the H62 brass ingot is beneficial to improving the forgeability of the H62 brass ingot and making the internal structure more uniform.
[0027] Further, after step S4 is completed, the CVD reaction cavity mirror structure is anodized, and the anodization is performed at a temperature of 15 to 40° C. using a mixed solution containing 100 to 250 g / l sulfuric acid, 10 to 30 g / l oxalic acid, and 5 to 30 g / l propylene glycol; after the anodization is completed, the CVD reaction cavity mirror structure is exposed to neutral salt spray for 12 to 20 hours;
[0028] Description: By anodizing the mirror surface structure of the CVD reaction chamber, the corrosion resistance of the mirror surface structure of the CVD reaction chamber is improved and its service life is increased.
[0029] Further, in step S4, when the CVD reaction chamber primary body is cleaned, the CVD reaction chamber primary body is first placed in kerosene for ultrasonic cleaning, and the ultrasonic frequency is controlled to be 20-30kHz, the time is 20-30min, and the temperature is 8-12°C; then the CVD reaction chamber primary body is placed in an isopropanol solution for ultrasonic cleaning, and the ultrasonic frequency is controlled to be 35-45kHz, the time is 20-30min, and the temperature is 13-16°C; finally, the CVD reaction chamber primary body is dried at a temperature of 110-125°C for 45-55min;
[0030] Description: By ultrasonically cleaning the CVD reaction chamber pre-body with different solvents and ultrasonic frequencies, it is beneficial to improve the comprehensiveness and thoroughness of the cleaning of the CVD reaction chamber pre-body.
[0031] The present invention also provides an application of a method for processing a mirror surface structure of a CVD reaction chamber for semiconductors, based on the above-mentioned method for processing a mirror surface structure of a CVD reaction chamber for semiconductors, in the application of processing a mirror surface structure of a CVD reaction chamber.
[0032] Compared with the prior art, the beneficial effects of the present invention are embodied in the following aspects:
[0033] First, the processing method of the present invention is reasonably designed, the overall wall thickness uniformity of the CVD reaction cavity mirror structure is high, and there is no leakage point, which effectively improves the processing quality of the CVD reaction cavity mirror structure; the CVD reaction cavity mirror structure of the present invention is processed by a natural diamond blade before polishing, which ensures the polishing amount and polishing accuracy in the later stage;
[0034] Second, the present invention utilizes different forging speeds to perform segmented forging on the H62 brass ingot, so that the internal grain refinement of the H62 brass ingot is more uniform, and ensures that there are no defects such as inclusions and cracks inside the material;
[0035] Third, the present invention can effectively reduce the wear rate of the tool and improve the processing efficiency of the part blank by performing layered rough turning on the part blank; at the same time, the use of the contour line winding finishing method can avoid the problem of extended processing cycle or excessive excess affecting the processing quality due to interference from excess material when finishing the next layer of excess material. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a schematic diagram of the mirror structure of the CVD reaction chamber of the present invention. DETAILED DESCRIPTION
[0037] Example 1
[0038] A method for processing a semiconductor CVD reaction chamber mirror structure comprises the following steps:
[0039] S1, forging;
[0040] H62 brass ingots were selected as raw materials for heating and forging. The H62 brass ingots were placed in a vacuum furnace and heated to 700°C. Then, they were forged 10 times to forge the H62 brass ingots from φ200mm to φ550mm part blanks.
[0041] During the forging process, the oxide scale on the surface of the H62 brass ingot is cleaned after each forging.
[0042] S2, parts processing;
[0043] S2-1, rough turning the blank obtained in step S1, and after the rough turning, heat treating the blank at 500° C.;
[0044] S2-2, finishing turning the part blank after rough turning in step S1-1, the finishing turning process is divided into 3 feeds, and the cutting amount of each time is controlled to be 0.4 mm; after finishing turning, the left chamber of the CVD reaction chamber and the right chamber of the CVD reaction chamber are obtained;
[0045] S3. Welding
[0046] The left chamber of the CVD reaction chamber and the right chamber of the CVD reaction chamber obtained in step S2-2 are welded to obtain a CVD reaction chamber primary body, and then the CVD reaction chamber primary body is corrected to make the inner and outer diameter errors of the CVD reaction chamber primary body 0.2 mm;
[0047] S4, surface treatment;
[0048] The CVD reaction chamber precursor after the correction treatment in step S3 is polished, and then ground with a grinding paste until the surface roughness of the inner wall of the CVD reaction chamber precursor reaches Ra0.8. Finally, the CVD reaction chamber precursor is cleaned to obtain a finished CVD reaction chamber mirror structure.
[0049] Example 2
[0050] A method for processing a semiconductor CVD reaction chamber mirror structure comprises the following steps:
[0051] S1, forging;
[0052] H62 brass ingots were selected as raw materials for heating and forging. The H62 brass ingots were placed in a vacuum furnace and heated to 950°C. Then, they were forged 10 times to forge the H62 brass ingots from φ200mm to φ550mm part blanks.
[0053] During the forging process, the oxide scale on the surface of the H62 brass ingot is cleaned every time it is forged; during the 1st to 4th forging process, the forging speed is controlled to be 50m / min; during the 4th to 7th forging process, the forging speed is controlled to be maintained at 150m / min; during the 7th to 10th forging process, the forging speed is controlled to be maintained at 220m / min;
[0054] S2, parts processing;
[0055] S2-1, rough turning the blank obtained in step S1, and after the rough turning, heat treating the blank at 700° C.;
[0056] S2-2, finishing turning the part blank after rough turning in step S1-1, the finishing turning process is divided into 4 feeds, and the cutting amount of each time is controlled to be 0.5 mm; after finishing turning, the left chamber of the CVD reaction chamber and the right chamber of the CVD reaction chamber are obtained;
[0057] S3. Welding
[0058] The left chamber of the CVD reaction chamber and the right chamber of the CVD reaction chamber obtained in step S2-2 are welded to obtain a CVD reaction chamber primary body, and then the CVD reaction chamber primary body is corrected to make the inner and outer diameter errors of the CVD reaction chamber primary body 0.1 mm;
[0059] S4, surface treatment;
[0060] The CVD reaction chamber precursor after the correction treatment in step S3 is polished, and then ground with a grinding paste until the surface roughness of the inner wall of the CVD reaction chamber precursor reaches Ra0.6. Finally, the CVD reaction chamber precursor is cleaned to obtain a finished CVD reaction chamber mirror structure.
[0061] Example 3
[0062] A method for processing a semiconductor CVD reaction chamber mirror structure comprises the following steps:
[0063] S1, forging;
[0064] H62 brass ingots were selected as raw materials for heating and forging. The H62 brass ingots were placed in a vacuum furnace and heated to 1250°C. Then, they were forged 10 times to forge the H62 brass ingots from φ200mm to φ550mm part blanks.
[0065] During the forging process, the oxide scale on the surface of the H62 brass ingot is cleaned after each forging.
[0066] S2, parts processing;
[0067] S2-1, rough turning the part blank obtained in step S1, and heat treating the part blank at 800° C. during rough turning; rough turning the part blank is layered, and the processing depth of each layer is controlled to be 10 mm;
[0068] S2-2, the part blank after rough turning in step S1-1 is fine turned, and the fine turning process is divided into 5 feeds, and the cutting amount of each time is controlled to be 0.6mm; after the fine turning is completed, the left chamber of the CVD reaction chamber and the right chamber of the CVD reaction chamber are obtained; during the fine turning, the tool is processed layer by layer along the contour loop composed of all points at the same height of the axial direction of the part blank, and the layer spacing and cutting width of each layer are controlled to be 4mm;
[0069] S3. Welding
[0070] The left chamber of the CVD reaction chamber and the right chamber of the CVD reaction chamber obtained in step S2-2 are welded to obtain a CVD reaction chamber primary body, and then the CVD reaction chamber primary body is corrected to make the inner and outer diameter errors of the CVD reaction chamber primary body 0.2 mm;
[0071] S4, surface treatment;
[0072] The CVD reaction chamber precursor after the correction treatment in step S3 is polished, and then ground with a grinding paste until the surface roughness of the inner wall of the CVD reaction chamber precursor reaches Ra0.5. Finally, the CVD reaction chamber precursor is cleaned to obtain a finished CVD reaction chamber mirror structure.
[0073] Example 4
[0074] A method for processing a semiconductor CVD reaction chamber mirror structure comprises the following steps:
[0075] S1, forging;
[0076] H62 brass ingots were selected as raw materials for heating and forging. The H62 brass ingots were placed in a vacuum furnace and heated to 700°C. Then, they were forged 10 times to forge the H62 brass ingots from φ200mm to φ550mm part blanks.
[0077] During the forging process, the oxide scale on the surface of the H62 brass ingot is cleaned after each forging.
[0078] S2, parts processing;
[0079] S2-1, rough turning the blank obtained in step S1, and after the rough turning, heat treating the blank at 500° C.;
[0080] S2-2, finishing turning the part blank after rough turning in step S1-1, the finishing turning process is divided into 3 feeds, and the cutting amount of each time is controlled to be 0.4 mm; after finishing turning, the left chamber of the CVD reaction chamber and the right chamber of the CVD reaction chamber are obtained;
[0081] S3. Welding
[0082] The left chamber of the CVD reaction chamber and the right chamber of the CVD reaction chamber obtained in step S2-2 are welded to obtain a CVD reaction chamber primary body, and then the CVD reaction chamber primary body is corrected to make the inner and outer diameter errors of the CVD reaction chamber primary body 0.2 mm;
[0083] S4, surface treatment;
[0084] The CVD reaction chamber preliminary body after the orthopedic treatment in step S3 is polished. During the polishing process, sandpaper from coarse to fine is used for polishing. The roughness of the CVD reaction chamber preliminary body is tested after each polishing. Then, the CVD reaction chamber preliminary body is polished with abrasive paste until the surface roughness of the inner wall of the CVD reaction chamber preliminary body reaches Ra0.8. Finally, the CVD reaction chamber preliminary body is cleaned to obtain a finished CVD reaction chamber mirror structure.
[0085] Among them, when cleaning the CVD reaction chamber primary body, the CVD reaction chamber primary body is first placed in kerosene for ultrasonic cleaning, and the ultrasonic frequency is controlled to be 20kHz, the time is 20min, and the temperature is 8°C; then the CVD reaction chamber primary body is placed in isopropanol solution for ultrasonic cleaning, and the ultrasonic frequency is controlled to be 35kHz, the time is 20min, and the temperature is 13°C; finally, the CVD reaction chamber primary body is dried at 110°C for 45min.
[0086] Example 5
[0087] A method for processing a semiconductor CVD reaction chamber mirror structure comprises the following steps:
[0088] S1, forging;
[0089] H62 brass ingots were selected as raw materials for heating and forging. The H62 brass ingots were first preheated to 350°C, then placed in a vacuum furnace and heated to 950°C, and then forged 10 times to forge the H62 brass ingots from φ200mm to φ550mm part blanks; the part blanks were sealed and placed in an ammonia container for 12 hours, and the part blanks were controlled not to contact the ammonia;
[0090] During the forging process, the oxide scale on the surface of the H62 brass ingot is cleaned after each forging.
[0091] S2, parts processing;
[0092] S2-1, rough turning the blank obtained in step S1, and after the rough turning, heat treating the blank at 700° C.;
[0093] S2-2, finishing turning the part blank after rough turning in step S1-1, the finishing turning process is divided into 4 feeds, and the cutting amount of each time is controlled to be 0.5 mm; after finishing turning, the left chamber of the CVD reaction chamber and the right chamber of the CVD reaction chamber are obtained;
[0094] S3. Welding
[0095] The left chamber of the CVD reaction chamber and the right chamber of the CVD reaction chamber obtained in step S2-2 are welded to obtain a CVD reaction chamber primary body, and then the CVD reaction chamber primary body is corrected to make the inner and outer diameter errors of the CVD reaction chamber primary body 0.1 mm;
[0096] S4, surface treatment;
[0097] The CVD reaction chamber precursor after the correction treatment in step S3 is polished, and then ground with a grinding paste until the surface roughness of the inner wall of the CVD reaction chamber precursor reaches Ra0.6. Finally, the CVD reaction chamber precursor is cleaned to obtain a finished CVD reaction chamber mirror structure.
[0098] Example 6
[0099] A method for processing a semiconductor CVD reaction chamber mirror structure comprises the following steps:
[0100] S1, forging;
[0101] H62 brass ingots were selected as raw materials for heating and forging. The H62 brass ingots were placed in a vacuum furnace and heated to 1250°C. Then, they were forged 10 times to forge the H62 brass ingots from φ200mm to φ550mm part blanks.
[0102] During the forging process, the oxide scale on the surface of the H62 brass ingot is cleaned after each forging.
[0103] S2, parts processing;
[0104] S2-1, rough turning the blank part obtained in step S1, and after rough turning, heat treating the blank part at 800° C.;
[0105] S2-2, finishing turning the part blank after rough turning in step S1-1, the finishing turning process is divided into 5 feeds, and the cutting amount of each time is controlled to be 0.6mm; after finishing turning, the left chamber of the CVD reaction chamber and the right chamber of the CVD reaction chamber are obtained;
[0106] S3. Welding
[0107] The left chamber of the CVD reaction chamber and the right chamber of the CVD reaction chamber obtained in step S2-2 are welded to obtain a CVD reaction chamber primary body, and then the CVD reaction chamber primary body is corrected to make the inner and outer diameter errors of the CVD reaction chamber primary body 0.2 mm;
[0108] S4, surface treatment;
[0109] The CVD reaction chamber precursor after the orthopedic treatment in step S3 is polished, and then ground with a grinding paste until the surface roughness of the inner wall of the CVD reaction chamber precursor reaches Ra0.5. Finally, the CVD reaction chamber precursor is cleaned to obtain a finished CVD reaction chamber mirror structure; finally, the CVD reaction chamber mirror structure is anodized, and the anodization is carried out at a temperature of 15°C using a mixed solution containing 100g / l sulfuric acid, 10-30g / l oxalic acid and 5g / l propylene glycol; after the anodization is completed, the CVD reaction chamber mirror structure is exposed to neutral salt spray for 12h.
[0110] Example 7
[0111] A method for processing a semiconductor CVD reaction chamber mirror structure comprises the following steps:
[0112] S1, forging;
[0113] H62 brass ingots were selected as raw materials for heating and forging. The H62 brass ingots were preheated to 550°C, and then placed in a vacuum furnace and heated to 1250°C. Then, 10 forgings were performed to forge the H62 brass ingots from φ200mm to φ550mm part blanks. Finally, the part blanks were sealed and placed in an ammonia container for 19 hours, and the part blanks were controlled not to contact the ammonia.
[0114] During the forging process, the oxide scale on the surface of the H62 brass ingot is cleaned every time it is forged; during the 1st to 4th forging process, the forging speed is controlled to be 50m / min; during the 4th to 7th forging process, the forging speed is controlled to be maintained at 1500m / min; during the 7th to 10th forging process, the forging speed is controlled to be maintained at 220m / min;
[0115] S2, parts processing;
[0116] S2-1, rough turning the part blank obtained in step S1, and heat treating the part blank at 800° C. after rough turning; wherein, the part blank is rough turned in layers, and the processing depth of each layer is controlled to be 5 mm;
[0117] S2-2, the part blank after rough turning in step S1-1 is fine turned, and the fine turning process is divided into 5 feeds, and the cutting amount of each time is controlled to be 0.4mm; after the fine turning is completed, the left chamber of the CVD reaction chamber and the right chamber of the CVD reaction chamber are obtained; wherein, during the fine turning, the tool processes the contour loop composed of all points at the same height of the axial direction of the part blank layer by layer, and the layer spacing and cutting width of each layer are controlled to be 2mm;
[0118] S3. Welding
[0119] The left chamber of the CVD reaction chamber and the right chamber of the CVD reaction chamber obtained in step S2-2 are welded to obtain a CVD reaction chamber primary body, and then the CVD reaction chamber primary body is corrected to make the inner and outer diameter errors of the CVD reaction chamber primary body 0.1 mm;
[0120] S4, surface treatment;
[0121] The CVD reaction chamber preliminary body after the orthopedic treatment in step S3 is polished by using sandpaper from coarse to fine, and the roughness of the CVD reaction chamber preliminary body is tested after each polishing; then the CVD reaction chamber preliminary body is polished by using abrasive paste until the surface roughness of the inner wall of the CVD reaction chamber preliminary body reaches Ra0.5, and finally the CVD reaction chamber preliminary body is cleaned to obtain a finished CVD reaction chamber mirror structure; finally, the CVD reaction chamber mirror structure is anodized, and the anodization is performed at a temperature of 40°C using a mixed solution containing 250g / l sulfuric acid, 30g / l oxalic acid and 30g / l propylene glycol; after the anodization is completed, the CVD reaction chamber mirror structure is exposed to neutral salt spray for 20h;
[0122] Among them, when cleaning the CVD reaction chamber primary body, the CVD reaction chamber primary body is first placed in kerosene for ultrasonic cleaning, and the ultrasonic frequency is controlled to be 30kHz, the time is 30min, and the temperature is 12°C; then the CVD reaction chamber primary body is placed in an isopropanol solution for ultrasonic cleaning, and the ultrasonic frequency is controlled to be 45kHz, the time is 30min, and the temperature is 16°C; finally, the CVD reaction chamber primary body is dried at 125°C for 55min.
[0123] Example 8
[0124] This embodiment records the application of a method for processing the mirror surface structure of a CVD reaction chamber for semiconductors, which is based on any one of the methods for processing the mirror surface structure of a CVD reaction chamber for semiconductors in embodiments 1-7 and is applied to the processing of the mirror surface structure of a CVD reaction chamber.
[0125] Test example
[0126] The performance of the finished product of the CVD reaction chamber mirror structure processed by the embodiments 1-7 of the present invention and the prior art was tested respectively, and the test results are shown in Table 1:
[0127] Table 1 Effects of the methods of various embodiments on the performance of the finished product of the CVD reaction chamber mirror structure
[0128]
[0129]
[0130] It can be seen from the data in Table 1 that compared with the prior art, the performance of the finished product of the CVD reaction chamber mirror structure processed by the present invention is better than that of the prior art;
[0131] Compared with Example 1, Example 2 performs segmented forging on the H62 brass ingot and controls the forging speed in each stage, so that the grain refinement inside the H62 brass ingot is more uniform;
[0132] Compared with Example 1, Example 3 can effectively reduce the wear rate of the tool and improve the processing efficiency of the part blank by rough turning the part blank in layers; the fine turning method of contour line winding can avoid the problem of extended processing cycle caused by excess interference or excessive excess affecting processing quality when fine turning the next layer of excess material;
[0133] Compared with Example 1, Example 4 performs step-by-step polishing on the CVD reaction chamber primary body, which is beneficial to improving the surface finish of the CVD reaction chamber primary body, thereby improving the use effect; ultrasonic cleaning of the CVD reaction chamber primary body with different solvents and ultrasonic frequencies is beneficial to improving the comprehensiveness and thoroughness of cleaning the CVD reaction chamber primary body, and improving the corrosion resistance of the CVD reaction chamber mirror structure;
[0134] Compared with Example 1, by sealing the blank in an ammonia container, it is convenient to detect defects such as cracks inside the blank, and avoid affecting the use effect after the mirror structure of the CVD reaction chamber is processed; by preheating the H62 brass ingot, it is beneficial to improve the forgeability of the H62 brass ingot and make the internal structure more uniform;
[0135] Compared with Example 1, Example 6 improves the corrosion resistance of the CVD reaction cavity mirror structure by performing anodizing treatment on the CVD reaction cavity mirror structure, thereby increasing its service life;
[0136] Compared with Examples 1 to 6, in the process of machining the mirror structure of the CVD reaction chamber, the process parameters are optimized so that all performances of the mirror structure of the CVD reaction chamber are optimized.
Claims
1. A method for processing a mirror structure of a semiconductor CVD reaction chamber, characterized in that: The following steps are involved: S1, forging; Selecting H62 brass ingot as raw material for heating and forging, placing the H62 brass ingot in a vacuum furnace and heating it to 700-1250° C., and then forging it 10 times, forging the H62 brass ingot from φ200 mm to a part blank of φ550 mm; During the forging process, the oxide scale on the surface of the H62 brass ingot is cleaned after each forging. S2, parts processing; S2-1, rough turning the blank obtained in step S1, and after the rough turning, heat treating the blank at a temperature of 500-800° C.; S2-2, finishing turning the part blank after rough turning in step S1-1, the finishing turning process is divided into 3 to 5 feeds, and the cutting amount of each time is controlled to be 0.4 to 0.6 mm; after finishing turning, the left chamber of the CVD reaction chamber and the right chamber of the CVD reaction chamber are obtained; S3. Welding The left chamber of the CVD reaction chamber and the right chamber of the CVD reaction chamber obtained in step S2-2 are welded to obtain a CVD reaction chamber primary body, and then the CVD reaction chamber primary body is corrected to make the inner and outer diameter errors of the CVD reaction chamber primary body ≤ 0.2 mm; S4, surface treatment; The CVD reaction chamber precursor after the correction treatment in step S3 is polished, and then ground with grinding paste until the surface roughness of the inner wall of the CVD reaction chamber precursor reaches Ra0.5-0.8, and finally the CVD reaction chamber precursor is cleaned to obtain a finished CVD reaction chamber mirror structure.
2. The method for processing a semiconductor CVD reaction chamber mirror structure according to claim 1, characterized in that: In step S1, during the 1st to 4th forging processes, the forging speed is controlled to be 50-70 m / min; during the 4th to 7th forging processes, the forging speed is controlled to be maintained at 150-200 m / min; during the 7th to 10th forging processes, the forging speed is controlled to be maintained at 220-300 m / min.
3. The rough machining method of a blisk component according to claim 1, characterized in that: In step S2-1, the part blank is rough turned in layers during rough turning, and the processing depth of each layer is controlled to be 5 to 10 mm; in step S2-2, the tool processes layer by layer along the contour loop composed of all points at the same height along the axial direction of the part blank during fine turning, and the layer spacing and cutting width of each layer are controlled to be 2 to 4 mm.
4. The method for processing a semiconductor CVD reaction chamber mirror structure according to claim 1, characterized in that: In step S4, during the polishing process, sandpapers from coarse to fine are used for polishing, and the roughness of the CVD reaction chamber primary body is tested after each polishing.
5. The method for processing a semiconductor CVD reaction chamber mirror structure according to claim 1, characterized in that: After step S1 is completed, the part blank is sealed and placed in an ammonia water container for 12 to 19 hours, and the part blank is controlled not to contact with the ammonia water.
6. The method for processing a semiconductor CVD reaction chamber mirror structure according to claim 1, characterized in that: Before step S1 is performed, the H62 brass ingot is preheated to 350-550°C.
7. The method for processing a semiconductor CVD reaction chamber mirror structure according to claim 1, characterized in that: After step S4 is completed, the CVD reaction cavity mirror structure is anodized, and the anodization is carried out at a temperature of 15 to 40° C. using a mixed solution containing 100 to 250 g / l sulfuric acid, 10 to 30 g / l oxalic acid and 5 to 30 g / l propylene glycol; after the anodization is completed, the CVD reaction cavity mirror structure is exposed to neutral salt spray for 12 to 20 hours.
8. The method for processing a semiconductor CVD reaction chamber mirror structure according to claim 1, characterized in that: In step S4, when the CVD reaction chamber primary body is cleaned, the CVD reaction chamber primary body is first placed in kerosene for ultrasonic cleaning, and the ultrasonic frequency is controlled to be 20-30kHz, the time is 20-30min, and the temperature is 8-12°C; then the CVD reaction chamber primary body is placed in an isopropanol solution for ultrasonic cleaning, and the ultrasonic frequency is controlled to be 35-45kHz, the time is 20-30min, and the temperature is 13-16°C; finally, the CVD reaction chamber primary body is dried at a temperature of 110-125°C for 45-55min.
9. A method for processing a semiconductor CVD reaction chamber mirror structure according to any one of claims 1 to 8, characterized in that: The processing method is applied in processing mirror surface structures of CVD reaction chambers.
10. The method for processing a semiconductor CVD reaction chamber mirror structure according to claim 1, characterized in that: In step S1, the H62 brass ingot is preheated to 350-550°C.
Citation Information
Patent Citations
Temperature reduction variable rate multi-direction repeated forging method for preparing fine-grained magnesium alloy
CN105921656A
Processing method of chemical vapor deposition (CVD) reaction chamber
CN108723709A
Process for manufacturing flanged half shaft from steel pipe
CN109483188A
Machining process for spray pipe shell of aerospace launcher
CN112296611A
Surface high-precision forging process for forging valve ball blank
CN116274781A