Conductive hydrogel with high strength and good moisture retention and preparation method thereof

Through the combination of polyvinyl alcohol, chitosan quaternary ammonium salt and eutectic solvent, the freeze-thaw method was used to prepare conductive hydrogel, which solved the problems of moisturizing and mechanical strength of conductive hydrogel, improved its antibacterial property, and achieved The effects of high strength, good moisture retention and conductivity are suitable for flexible electronic devices.

CN118812977APending Publication Date: 2024-10-22WUHAN UNIV OF TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410937078.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing conductive hydrogels in flexible electronic devices have problems such as poor moisture retention, low mechanical strength, and insufficient antibacterial properties, making it difficult to balance moisture retention, mechanical strength, and conductivity.

Method used

A combination of polyvinyl alcohol, chitosan quaternary ammonium salt and eutectic solvent is used to prepare conductive hydrogel through heating, dissolution and freeze-thaw methods to form a hydrogen bond network, improve conductivity and moisture retention, and use chitosan quaternary ammonium The antimicrobial properties of the salt impart antimicrobial properties to the conductive hydrogel.

Benefits of technology

A conductive hydrogel with high strength, good moisture retention and high conductivity has been achieved. It has excellent anti-freeze and antibacterial properties. The preparation method is simple, the raw materials are cheap, green and non-toxic, and it is suitable for flexible electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118812977A_ABST
    Figure CN118812977A_ABST
Patent Text Reader

Abstract

The invention relates to conductive hydrogel with high strength and good moisture retention and a preparation method thereof.The conductive hydrogel is prepared from, by volume, 60%-90% of polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution and 10%-40% of eutectic solvent; the polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution is obtained by mixing polyvinyl alcohol, chitosan quaternary ammonium salt and water according to a ratio of (15-25) g: (7.5-15) g: 100mL. Through cooperation of the raw materials and the dosages, the obtained conductive hydrogel has high strength and good moisture retention, and also has certain conductivity and anti-freezing and antibacterial properties; and the preparation method is simple, wide in raw material source, green, non-toxic, safe, reliable and wide in application range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of conductive hydrogels, and in particular to a conductive hydrogel with high strength and good moisture retention and a preparation method thereof. Background Art

[0002] In recent years, flexible electronic devices have developed rapidly, showing unique application value in signal detection, power storage, human-machine interface and other fields. Hydrogel is a water-rich polymer material with a three-dimensional network structure, which is conducive to the transmission of electrons and ions, and also avoids the diffusion and leakage of ions outward, showing super strong affinity and stability.

[0003] Patent CN107474265A discloses a method for preparing a polyvinyl alcohol conductive hydrogel, which uses hydrogen bond composite network and salting-out effect, adds glycerol and sodium chloride as auxiliary materials, and obtains a polyvinyl alcohol hydrogel with high conductivity and certain mechanical strength. However, due to the presence of sodium chloride, the stability of the hydrogel is easily destroyed, causing its water to be quickly discharged, poor moisture retention, and thus a series of defects such as reduced elasticity and conductivity, which cannot meet the requirements of skin flexible sensors. In addition, most water-containing flexible devices create conditions for the adhesion and aggregation of bacteria, and the current conductive hydrogel still needs to be improved in terms of antibacterial properties; and other existing methods for preparing hydrogels usually pay less attention to their moisture retention issues, and it is usually difficult to take into account moisture retention, mechanical strength and antibacterial properties.

[0004] Therefore, when it comes to the construction of flexible electronic devices, current hydrogel materials still face problems such as poor moisture retention, low mechanical strength, antibacterial properties and electrical conductivity. Summary of the invention

[0005] The purpose of the present invention is to overcome the above technical deficiencies, provide a conductive hydrogel with high strength and good moisture retention and a preparation method, and solve the technical problems of poor moisture retention and low mechanical strength of conductive hydrogel in the prior art.

[0006] In order to achieve the above technical purpose, the technical solution provided by the present invention is: In a first aspect, the present invention provides a conductive hydrogel with high strength and good moisture retention. The raw materials of the conductive hydrogel include 60-90% of a polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution and 10-40% of a eutectic solvent by volume percentage; the polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution is obtained by mixing polyvinyl alcohol, chitosan quaternary ammonium salt and water in a ratio of (15-25) g: (7.5-15) g: 100 mL.

[0007] In a second aspect, the present invention provides a method for preparing a conductive hydrogel with high strength and good moisture retention, comprising the following steps: adding polyvinyl alcohol to a chitosan quaternary ammonium salt solution, heating and stirring to dissolve, to obtain a polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution; uniformly mixing the polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution with a eutectic solvent to obtain a polyvinyl alcohol / chitosan quaternary ammonium salt / eutectic solvent mixed solution; pouring the polyvinyl alcohol / chitosan quaternary ammonium salt / eutectic solvent mixed solution into a mold, and preparing the conductive hydrogel by a freeze-thaw method.

[0008] Compared with the prior art, the beneficial effects of the present invention include: The invention uses polyvinyl alcohol and chitosan quaternary ammonium salt as raw materials, heats and dissolves them to obtain a mixed solution of the two, then adds a certain volume of eutectic solvent to obtain a mixed solution of the three; constructs a conductive hydrogel through a freeze-thaw method, and various components are mutually associated through hydrogen bonds to produce excellent conductivity and moisture retention; at the same time, the eutectic solvent exhibits a certain antifreeze ability, can delay the crystallization process of polyvinyl alcohol, and further enables the hydrogel to form a more dense and uniform hydrogen bond network; the chitosan quaternary ammonium salt, as a cationic derivative of chitosan, can destroy bacterial cell membranes, thereby giving the conductive hydrogel excellent antibacterial property; the invention makes the obtained conductive hydrogel have high strength and good moisture retention, and has certain conductivity, antifreeze and antibacterial properties by matching the types and amounts of various raw materials; and the preparation method is simple, the raw materials are cheap, the sources are wide, the green and non-toxic, safe and reliable, and the application range is wide. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] Figure 1 The stress-strain curves of the conductive hydrogels prepared in Examples 1-4 of the present invention and Comparative Example 1; Figure 2 The maximum strain and Young's modulus diagram of the conductive hydrogel prepared in Examples 1-4 of the present invention and Comparative Example 1; Figure 3 The impedance values ​​of the conductive hydrogels prepared in Examples 1-4 of the present invention and Comparative Example 1; Figure 4 The conductivity of the conductive hydrogels prepared in Examples 1-4 of the present invention and Comparative Example 1; Figure 5 The impedance value of the conductive hydrogel prepared in Example 1 of the present invention changes with the number of freeze-thaw cycles; Figure 6 The conductivity of the conductive hydrogel prepared in Example 1 of the present invention changes with the number of freeze-thaw cycles; Figure 7 This is the moisture retention curve of the green conductive hydrogel prepared in Example 1 of the present invention; Figure 8 This is a real picture of the moisturizing property of the green conductive hydrogel prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0010] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0011] In the prior art, the salting-out ion conductive hydrogel has poor moisture retention, which leads to a series of defects such as reduced flexibility and conductivity, making it unable to meet the requirements of skin flexible sensors. In addition, most water-containing flexible devices create conditions for the adhesion and aggregation of bacteria. At present, the antibacterial property of conductive hydrogels needs to be improved. Therefore, it is usually difficult for existing hydrogels to balance the problems of moisture retention, mechanical strength and antibacterial property. The present invention provides a conductive hydrogel with high strength and good moisture retention and a preparation method thereof. High-strength polyvinyl alcohol, antibacterial chitosan quaternary ammonium salt and a eutectic solvent with good conductivity and water retention are combined, and a green conductive hydrogel with high strength and good moisture retention is prepared by a freeze-thaw method.

[0012] Among them, polyvinyl alcohol is a polymer material with high flexibility and good biocompatibility, and can be used to prepare physically cross-linked hydrogels by a simple freeze-thaw method; eutectic solvent is a low-cost, non-toxic new green solvent with similar properties to ionic liquids, in which various components are mutually associated through hydrogen bonds to produce excellent conductivity and moisture retention. At the same time, the eutectic solvent exhibits a certain antifreeze ability, which can delay the crystallization process of polyvinyl alcohol, thereby allowing the hydrogel to form a more dense and uniform hydrogen bond network. Chitosan quaternary ammonium salt, as a cationic derivative of chitosan, can destroy the cell membrane of bacteria, thereby giving the conductive hydrogel excellent antibacterial properties, and the present invention, through the type and amount of each raw material, makes the resulting conductive hydrogel have high strength, good moisture retention, and has certain conductivity and antifreeze and antibacterial properties.

[0013] In a first aspect, the present invention provides a conductive hydrogel with high strength and good moisture retention. The raw materials include 60-90% of a polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution and 10-40% of a eutectic solvent, by volume percentage; the polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution is obtained by mixing polyvinyl alcohol, chitosan quaternary ammonium salt and water in a ratio of (15-25) g: (7.5-15) g: 100 mL.

[0014] Preferably, the eutectic solvent is a mixture of ethylene glycol and choline chloride in a molar ratio of 1:1.

[0015] Preferably, the volume percentage of the eutectic solvent is 20-30%, and the volume percentage of the polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution is 70-80%.

[0016] Preferably, the polyvinyl alcohol comprises polyvinyl alcohol 1799.

[0017] Preferably, the chitosan quaternary ammonium salt comprises a water-soluble cationic chitosan quaternary ammonium salt.

[0018] In a second aspect, the present invention provides a method for preparing a conductive hydrogel with high strength and good moisture retention, comprising the following steps: Adding polyvinyl alcohol to the chitosan quaternary ammonium salt solution, heating and stirring to dissolve, to obtain a polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution; The polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution and the eutectic solvent are uniformly mixed to obtain a polyvinyl alcohol / chitosan quaternary ammonium salt / eutectic solvent mixed solution; The mixed solution of polyvinyl alcohol / chitosan quaternary ammonium salt / eutectic solvent was poured into a mold, and the conductive hydrogel was prepared by freeze-thaw method.

[0019] Preferably, the chitosan quaternary ammonium salt solution is obtained by adding chitosan quaternary ammonium salt into deionized water and stirring to dissolve it at room temperature.

[0020] Preferably, polyvinyl alcohol is added to the chitosan quaternary ammonium salt solution, and heated and stirred at 90 to 98° C. for 3 to 6 hours to obtain a polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution.

[0021] Preferably, in the freeze-thaw method, the total freeze-thaw time is 2 to 20 hours, and the number of freeze-thaw cycles is 1 to 10 times.

[0022] Further preferably, in a single freeze-thaw process, the sample is first frozen at -35 to -25°C for 1.5 to 2.5 hours, and then thawed at 32 to 38°C for 1.5 to 2.5 hours; a single freeze-thaw cycle is defined as one freeze-thaw cycle.

[0023] Further preferably, in a single freeze-thaw process, the sample is first frozen at -30°C for 2 h and then thawed at 37°C for 2 h.

[0024] The main mechanism of action and advantages of the present invention are: (1) Polyvinyl alcohol has high toughness and good biocompatibility; eutectic solvent is a low-cost, non-toxic new green solvent with excellent conductivity and moisture retention; quaternary ammonium salt chitosan has excellent antibacterial properties; the present invention combines the specific types and amounts of the above raw materials to make the resulting conductive hydrogel not only have high strength and good moisture retention, but also have certain conductivity and antifreeze and antibacterial properties. The conductive hydrogel material of the present invention is non-toxic, low-cost and has good biocompatibility.

[0025] (2) The present invention adopts the freeze-thaw method to prepare the hydrogen-bonded cross-linked hydrogel network, and the production process is simple and environmentally friendly.

[0026] The present invention is further described in detail below through specific embodiments; to avoid redundancy, the main raw materials are described below, and other reagents and equipment not specifically described can be purchased from the market; wherein: polyvinyl alcohol uses polyvinyl alcohol 1799 from Shanghai MacLean Biochemical Technology Co., Ltd., and chitosan quaternary ammonium salt uses water-soluble cationic chitosan quaternary ammonium salt from Zhejiang Jinke Pharmaceutical Co., Ltd., with batch number M-JA-2302001.

[0027] Example 1 (1) Take 1.5 g of polyvinyl alcohol, add it to 10 mL of aqueous solution containing 0.75 g of chitosan quaternary ammonium salt, heat and stir at 95 ° C for 6 h to obtain a polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution (A); (2) preparing a eutectic solvent (B) by mixing ethylene glycol and choline chloride in a molar ratio of 1:1; (3) Solution C was prepared according to the volume ratio of the polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution and the eutectic solvent being A:B=7:3; (4) Finally, the evenly stirred solution C was poured into a silicone mold and frozen once using the freeze-thaw method. The single freeze-thaw conditions were: first freezing at -30°C for 2 h, and then thawing at 37°C for 2 h to prepare a conductive hydrogel named GJ3.

[0028] Example 2 The only difference from Example 1 is that the volume ratio of the polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution and the eutectic solvent is adjusted to A:B=9:1, and the other steps and conditions are the same as those in Example 1, and it is named GJ1.

[0029] Example 3 The only difference from Example 1 is that the volume ratio of the polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution and the eutectic solvent is adjusted to A:B=8:2, and the other steps and conditions are the same as those in Example 1, and it is named GJ2.

[0030] Example 4 The only difference from Example 1 is that the volume ratio of the polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution and the eutectic solvent is adjusted to A:B=6:4, and the other steps and conditions are the same as those in Example 1, and it is named GJ4.

[0031] Comparative Example 1 The only difference from Example 1 is that the volume ratio of the polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution and the eutectic solvent is adjusted to A:B=10:0, and the other steps and conditions are the same as those in Example 1, named GJ0.

[0032] Comparative Example 2 The only difference from Example 1 is that the chitosan quaternary ammonium salt is removed, and the other steps and conditions are the same as those in Example 1.

[0033] Performance Testing 1. Tensile test: The obtained hydrogel sheet was cut into dumbbells with a length of 50 mm, a width of 4 mm, and a thickness of 2 mm. A universal tensile testing machine (HY-0580) was used to perform a tensile test to obtain the tensile strength and Young's modulus.

[0034] Conductivity: The obtained hydrogel sheet was cut into cylindrical sheets with a radius of 17 mm and a thickness of 2 mm, and the conductivity was tested using an electrochemical workstation (CHI660).

[0035] 2. The performance of the conductive hydrogels obtained in Examples 1-4 and Comparative Example 1 was tested. The results are shown in Table 1 and Figures 1 to 4 shown.

[0036] Table 1 Performance test results of the conductive hydrogels obtained in Examples 1-4 and Comparative Example 1

[0037] From Table 1, Figures 1 to 4 It can be seen that the tensile strength, Young's modulus and conductivity of the conductive hydrogel obtained by the present invention are affected by the volume ratio of the polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution and the eutectic solvent, wherein: Figure 1 The tensile strength varies with GJ0-4. The maximum tensile strength and modulus are obtained at GJ3. Figure 3 The conductivity changes with GJ0-4, and the maximum conductivity is at GJ3. When the eutectic solvent is not added, the performance of the obtained conductive hydrogel (GJ0) is poor. After adding the eutectic solvent, all the properties are improved. The tensile strength of the conductive hydrogel obtained by the present invention is 0.34-2.55 MPa, the Young's modulus is 0.16-0.55 MPa, and the conductivity is 33.3-42.3 mS / cm. This shows that the present invention can improve the mechanical strength and conductivity of the obtained conductive hydrogel through the coordination of polyvinyl alcohol, chitosan quaternary ammonium salt and eutectic solvent.

[0038] 3. Antibacterial property: The antibacterial properties of the conductive hydrogels of Example 1 and Comparative Example 2 were tested by the plate coating method. The prepared conductive hydrogel samples were sterilized by ultraviolet and placed in a 48-well plate. Then, 100 μL of bacterial suspension (Escherichia coli and Staphylococcus aureus, 10 6 CFU / mL) was dropped on the surface of the hydrogel and incubated at 37 °C for 2 h. Subsequently, 1 mL of sterile PBS was added to each well to resuspend the bacteria. 40 μL of the suspension was aspirated and plated, and the number of colonies on the agar plate was counted after incubation at 37 °C for 18 h.

[0039] The results showed that the conductive hydrogel obtained in Comparative Example 2 (without chitosan quaternary ammonium salt) had a low antibacterial rate against Escherichia coli and Staphylococcus aureus, which were 3.8% and 4.2% respectively; while the conductive hydrogel obtained in Example 1 had a high antibacterial rate against Escherichia coli and Staphylococcus aureus, which were 93.8% and 93.6% respectively.

[0040] 4. Freeze resistance: The conductive hydrogel of Example 1 was subjected to an antifreeze test, and the freezing cycle conditions were the same as the single freeze-thaw conditions in Example 1, that is, first freezing at -30°C for 2 h, and then thawing at 37°C for 2 h, as one freezing cycle, and so on, for 10 cycles (GJ3 is a sample that has been cycled once).

[0041] Depend on Figure 5 and Figure 6 The results show that the impedance value remains basically unchanged after multiple freezing cycles, and the conductivity remains at 41mS / cm.

[0042] 5. Moisturizing: The conductive hydrogel of Example 1 was placed in an environment of 25°C and 35% humidity to conduct a moisture retention test. The results are as follows: Figure 7 and Figure 8 shown.

[0043] Figure 7 and Figure 8 The results show that the weight of the conductive hydrogel of Example 1 after 7 days is 58.1% of the original weight. The results show that the conductive hydrogel prepared by the present invention has good moisture retention.

[0044] The conductive hydrogel of Comparative Example 1 was also placed in an environment of 25°C and 35% humidity for moisture retention test. After one day, the water retention rate dropped to 60.31%, and after seven days, the water retention rate dropped to 30%. This shows that the addition of the eutectic solvent significantly enhances the water retention effect of the hydrogel sample.

[0045] Different from the prior art, the present invention provides a conductive hydrogel with high strength and good moisture retention and a preparation method thereof, which uses polyvinyl alcohol and chitosan quaternary ammonium salt as raw materials, dissolves them by heating to obtain a mixed solution of the two, and then adds a certain volume of eutectic solvent (including ethylene glycol and choline chloride) to obtain a mixed solution of the three. The conductive hydrogel is constructed by the freeze-thaw method, and the hydrogel exhibits super strong stress, good moisture retention and high conductivity. At the same time, the preparation process is simple, the raw materials are cheap, the source is wide, it is green and non-toxic, safe and reliable, and it has great application potential.

[0046] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A conductive hydrogel with high strength and good moisture retention, characterized in that: The raw materials of the conductive hydrogel include 60-90% of a polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution and 10-40% of a eutectic solvent by volume percentage; The polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution is obtained by mixing polyvinyl alcohol, chitosan quaternary ammonium salt and water in a ratio of (15-25) g: (7.5-15) g: 100 mL.

2. The conductive hydrogel with high strength and good moisture retention according to claim 1, characterized in that: The eutectic solvent is a mixture of ethylene glycol and choline chloride in a molar ratio of 1:

1.

3. The conductive hydrogel with high strength and good moisture retention according to claim 1, characterized in that: The volume percentage of the eutectic solvent is 20-30%, and the volume percentage of the polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution is 70-80%.

4. The conductive hydrogel with high strength and good moisture retention according to claim 1, characterized in that: The polyvinyl alcohol includes polyvinyl alcohol 1799.

5. The conductive hydrogel with high strength and good moisture retention according to claim 1, characterized in that: The chitosan quaternary ammonium salt comprises a water-soluble cationic chitosan quaternary ammonium salt.

6. The method for preparing a conductive hydrogel with high strength and good moisture retention according to any one of claims 1 to 5, characterized in that: The following steps are involved: Adding polyvinyl alcohol to the chitosan quaternary ammonium salt solution, heating and stirring to dissolve, to obtain a polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution; The polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution and the eutectic solvent are uniformly mixed to obtain a polyvinyl alcohol / chitosan quaternary ammonium salt / eutectic solvent mixed solution; The mixed solution of polyvinyl alcohol / chitosan quaternary ammonium salt / eutectic solvent was poured into a mold, and the conductive hydrogel was prepared by freeze-thaw method.

7. The method for preparing a conductive hydrogel with high strength and good moisture retention according to claim 6, characterized in that: The chitosan quaternary ammonium salt solution is obtained by adding chitosan quaternary ammonium salt into deionized water at room temperature and stirring to dissolve.

8. The method for preparing a conductive hydrogel with high strength and good moisture retention according to claim 6, characterized in that: Polyvinyl alcohol is added to the chitosan quaternary ammonium salt solution, heated and stirred at 90-98° C. for 3-6 hours to obtain a polyvinyl alcohol / chitosan quaternary ammonium salt mixed solution.

9. The method for preparing a conductive hydrogel with high strength and good moisture retention according to claim 6, characterized in that: In the freeze-thaw method, the total freeze-thaw time is 2 to 20 hours, and the number of freeze-thaw cycles is 1 to 10 times.

10. The method for preparing a conductive hydrogel with high strength and good moisture retention according to claim 9, characterized in that: During a single freeze-thaw process, first freeze at -35 to -25°C for 1.5 to 2.5 hours, and then thaw at 32 to 38°C for 1.5 to 2.5 hours.

Citation Information

Patent Citations

  • Preparation method of polyvinyl alcohol conductive hydrogel

    CN107474265A