Anti-laser eavesdropping intermediate film and application thereof

By using an anti-laser eavesdropping interlayer that suppresses laser light in the entire wavelength band, combined with the scattering technology of fumed silica and hollow glass beads, the existing anti-laser eavesdropping films solve the problems of environmentally friendly reagents, complex processes and poor scratch resistance, achieving The attenuation of laser energy and the improvement of barrier efficiency.

CN118812979APending Publication Date: 2024-10-22HUAIAN FUCHENG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410853237.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing anti-laser eavesdropping films have problems with the environmental protection and safety of the reagents, complex processes, bubbling and degumming of film products, poor scratch resistance, and low light intensity received by the laser signal receiver.

Method used

The anti-laser eavesdropping interlayer film that suppresses laser in the entire wavelength band is used, including resin powder, plasticizer, antioxidant, ultraviolet absorber, carbon radical capture agent and reinforcing agent. It is prepared by cast extrusion technology and is a multi-layer co-extrusion. The intermediate film combines the scattering technology of fumed silica and hollow glass beads to weaken the propagation and return signal of the laser.

Benefits of technology

It achieves a sharp attenuation of laser energy, simplifies the process, improves adhesion and scratch resistance, prolongs service life, and improves laser blocking efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004917372630000091
    Figure BDA0004917372630000091
Patent Text Reader

Abstract

The invention relates to the technical field of laser eavesdropping prevention, in particular to a laser eavesdropping prevention intermediate film and application thereof. The anti-laser eavesdropping intermediate film comprises the following components in parts by weight: 100 parts of resin powder, 25-45 parts of a plasticizer, 0.2-1 part of an antioxidant, 0.1-1.0 part of an ultraviolet light absorber, 0.2-0.5 part of a carbon free radical trapping agent and 1-8 parts of a reinforcing agent. The reinforcing agent is at least one of fumed silica subjected to surface treatment, hollow glass beads subjected to surface treatment and doped metal oxide powder. The intermediate film can be applied to anti-eavesdropping laminated glass, and the anti-eavesdropping laminated glass at least comprises one layer of intermediate film. Invasive laser energy can be attenuated sharply, so that the propagation path of laser entering and exiting a sensitive area is cut off, and the purpose of protecting the sensitive area is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of laser-proof eavesdropping, and in particular to an laser-proof eavesdropping intermediate film and application thereof. Background Art

[0002] Sound is generated by vibration, and sound will also cause vibration of surrounding objects. "Laser monitoring" technology refers to using a beam of laser that is invisible to the human eye to hit objects near the sound source, collect the vibration of the objects caused by the sound source, and then restore the sound, achieving the purpose of monitoring with laser. Anti-laser eavesdropping / monitoring blocking shielding film can block and shield lasers in the corresponding band, thereby preventing eavesdropping and monitoring.

[0003] Laser is a special kind of light. It has the characteristics of light, and its color is purer and its energy is greater than that of ordinary light. Laser wavelengths exist from infrared to ultraviolet. With the development of laser technology, laser has evolved from early regular reflection laser to diffuse reflection laser. Diffuse reflection laser is to use equipment to irradiate laser on the target indoor objects (such as clothes, paper, water cups, curtains, etc.). If someone is talking in the room, the conversation causes the object to vibrate, and the light containing the vibration frequency information of the conversation can be reflected back to the device, thereby parsing the sound information. For this laser technology that is hard to defend against, the use of laser blocking film is an effective protection method.

[0004] At present, the anti-laser eavesdropping film on the market adopts nanotechnology to intercept infrared and ultraviolet rays, shield and block the laser band. It uses PET as the substrate, coats metal oxide slurry on it, then dries it, and then composites a multi-layer protective film, and sticks it to the glass surface in the form of a film, similar to the film on the surface of automobile glass.

[0005] The existing anti-laser eavesdropping film has the following disadvantages:

[0006] First, the metal and metal oxide slurry used contains a variety of solvents, dispersants and other chemical reagents. After grinding and dispersion, it needs to go through a drying process after being coated on PET to remove all the added chemical reagents, thereby attaching a layer of metal and metal oxide to the surface of PET. Obviously, there are problems with the environmental protection of reagents, the safety of reagents, and the complexity of the process in the above process.

[0007] Second, the film products are ultimately in the form of multi-layer composites, and all light-grade PET must be used, with each layer playing a different structural role. During the manufacturing process, special care must be taken to prevent scratches on PET.

[0008] 3. The multi-layer composite of film products and the need to be pasted to the glass surface involve the issue of glue selection. If the glue quality is not up to standard, problems such as bubbling and delamination are likely to occur, similar to the bubbling and delamination caused by car film.

[0009] 4. The film products exist on the glass surface. During long-term use, the glass surface needs to be cleaned and maintained, which leads to scratch-resistant wear.

[0010] 5. The basic principle of existing anti-laser eavesdropping films is to use the absorption of lasers by metals and metal oxides to reduce the intensity of lasers irradiating the surface of indoor objects. When the laser returns, the intensity is weakened twice, so that the light intensity received by the signal receiver is lower.

[0011] Based on the above problems existing in the existing anti-laser eavesdropping film, it is now urgent to improve the existing anti-laser eavesdropping film. Summary of the invention

[0012] In order to solve the deficiencies of the prior art, the present invention provides an anti-laser eavesdropping intermediate film, which can suppress lasers in the entire band and sharply attenuate the invading laser energy, thereby cutting off the propagation path of the laser in and out of sensitive areas and achieving the purpose of protecting sensitive areas.

[0013] The technical solution of the present invention is:

[0014] A laser eavesdropping-proof intermediate film comprises the following components in parts by weight: 100 parts of resin powder, 25-45 parts of plasticizer, 0.2-1 part of antioxidant, 0.1-1.0 part of ultraviolet absorber, 0.2-0.5 part of carbon free radical capture agent and 1-8 parts of reinforcing agent.

[0015] Preferably, the resin powder includes any one of PVB resin powder, POE resin powder, EVA resin powder, TPU resin powder and SGP resin powder.

[0016] Preferably, the resin powder is PVB resin powder.

[0017] Preferably, the hydroxyl content of the PVB resin powder is 15-25%.

[0018] Preferably, the plasticizer is low polar, and is selected from one or a mixture of triethylene glycol esters, phosphate esters, adipates, sebacates, and phthalates, preferably triethylene glycol diisooctanoate, i.e. 3GO.

[0019] Preferably, the ultraviolet absorber is a benzotriazole, a benzophenone, or a triazine. Preferably, UV-3035 or UV-1577 is used. More preferably, UV-3035 is used. The ultraviolet absorber prevents the intermediate film from photoaging after use, prolongs the service life, and can absorb the ultraviolet band in the laser.

[0020] Preferably, the antioxidants are phenols and phosphites, phenols are the main antioxidants, preferably 1010 or 1076, and the auxiliary antioxidants are phosphites, preferably 168. 1010 (or 1076): 168 = 2:1 to 1:3 (mass ratio).

[0021] Preferably, 1010:168=1:2 (mass ratio). The role of the antioxidant is that the intermediate film will undergo irreversible oxidative degradation due to heat and mechanical shear during the production and use process, and the antioxidant needs to be added to delay and inhibit the oxidative degradation process.

[0022] Preferably, the carbon radical scavenger is selected from hydroxylamine, bisphenol monoacrylate, ortho-propenyl substituted phenol and benzofuranone, preferably HP-136 or GS, preferably HP-136 (xylyl dibutylbenzofuranone).

[0023] Preferably, the reinforcing agent is at least one of surface-treated fumed silica, surface-treated hollow glass microspheres, and doped metal oxide powder.

[0024] The function of the fumed silica in the present invention is to have a good reflection effect on ultraviolet rays and infrared rays.

[0025] In the present invention, the hollow glass microspheres mainly scatter the laser light, weakening the intensity of the laser light reaching the detection object directly, and then the intensity of the reflected light is weakened accordingly; the laser light is repeatedly reflected through its internal hollow structure, further weakening the intensity of the laser light returning, that is, weakening the signal fed back to the eavesdropping receiver. The particle size of the glass microspheres is generally 10-250μm. The particle size of 150-200μm is preferred.

[0026] Preferably, the surface treatment method of fumed silica is as follows: according to the mass parts of fumed silica: ethanol: acetone = 1:500:50, the fumed silica is first added into a round-bottom flask, and then ethanol is added, a magnetic stirring bar is added, and the mixture is stirred, cooled and refluxed at 50°C 45-55°C for 2-3h, and then acetone is added dropwise. After the addition is completed, stirring, cooling and reflux are continued for 3-4h, and finally filtered for standby use.

[0027] Preferably, the surface treatment method of glass beads is as follows: according to the mass ratio of glass beads: coupling agent = 1:1000, two substances are weighed and put into a round-bottom flask, a magnetic stirring bar is added, and the mixture is stirred, cooled and refluxed at 45-55° C. for 4-5 hours, and then filtered and dried for later use.

[0028] Preferably, the coupling agent is used to modify the surface of the inorganic non-metallic material and improve the interfacial compatibility between the inorganic non-metallic material and the organic polymer material. It is selected from silane coupling agents, titanate coupling agents, phosphate coupling agents, and bimetallic coupling agents. Silane coupling agents are preferred. Aminosilane, epoxysilane, thiosilane, methacryloxysilane, and vinylsilane are further preferred. Methacryloxysilane (KH570) is further preferred.

[0029] Preferably, the doped metal oxide powder has a small particle size, uniform particles, is easy to disperse, has good infrared barrier properties, and is highly weather resistant. Commercially available materials include ITO, ATO, STO, GTO, ZTO, and BTO, and contain at least one of them. GTO and ATO are preferred, as GTO can absorb infrared and ATO can reflect infrared.

[0030] The above-mentioned anti-laser eavesdropping intermediate film can be applied to anti-eavesdropping laminated glass, and the anti-eavesdropping laminated glass contains at least one layer of intermediate film.

[0031] The beneficial effects achieved by the present invention are:

[0032] 1. The present invention can suppress lasers in the entire band and make the energy of the invading lasers attenuate sharply, thereby cutting off the propagation path of the lasers in and out of the sensitive areas and achieving the purpose of protecting the sensitive areas.

[0033] 2. The present invention is directed to metal and metal oxide powders, and does not require the addition of liquid for grinding and then coating, but can be directly mixed with resin powder, with a simple process, safe reagents, and environmental protection.

[0034] 3. The present invention aims at the multi-layer composite and glue problems of film products. The present invention prepares the intermediate film by casting and extruding the resin powder containing metal and metal oxide powder into the intermediate film through the multi-layer co-extruded intermediate film. The intermediate film has good adhesion to the glass, and the multi-layer co-extruded structure is simple.

[0035] 4. To solve the problem of scratches during later maintenance, the present invention combines the prepared intermediate film with glass to prepare laminated glass. The intermediate film is in the middle of the two layers of glass, and the glass is on the outside. The hard surface of the glass can resist scratches during the cleaning process.

[0036] 5. The present invention retains the absorption effect of metals and metal oxides on lasers. The superposition scattering technology utilizes the scattering effect of gas phase silica and glass microbeads on light to disperse the laser and reduce the intensity of the laser irradiated on the surface of indoor objects. When the laser returns, it scatters again to reduce the light intensity of the return signal receiver. It is added to the resin matrix through blending modification. DETAILED DESCRIPTION

[0037] To facilitate those skilled in the art to understand the present invention, specific implementations of the present invention are described below with reference to embodiments.

[0038] The PVB resin powder used in the following examples can be any qualified domestic commercially available product.

[0039] Production of PVB containing fumed silica:

[0040] Since fumed silica is light in weight, if it is directly mixed with PVB resin powder, it will be suspended above the PVB resin powder. If it is directly mixed with plasticizer, it is easy to agglomerate and disperse unevenly, so it needs to be surface treated.

[0041] The surface treatment method is as follows: weigh the mass parts of fumed silica: ethanol: acetone = 1:500:50, first add the fumed silica into a round-bottom flask, then add ethanol, put in a magnetic stirrer, stir and cool under reflux at 50°C for 2 hours, then add acetone dropwise, continue stirring and cooling under reflux for 3 hours after the addition is completed, and finally filter and set aside.

[0042] Made of PVB containing glass beads:

[0043] Since glass microbeads are silicate inorganic substances, they have poor compatibility with PVB resin and are easy to agglomerate, so they also need to be surface modified. The modified glass microbeads can be better dispersed in the PVB substrate, and the interface between the two is friendly, forming an "island structure".

[0044] The surface treatment method is as follows: according to the mass ratio of glass beads: coupling agent KH-570 = 1:1000, weigh the two substances into a round-bottom flask, put in a magnetic stirrer, stir and cool under reflux at 50°C for 5h, then filter and dry for later use.

[0045] Example 1

[0046] A laser eavesdropping-proof interlayer film comprises the following components in parts by weight: 100 parts of PVB resin powder (with a hydroxyl content of 15-25%), 37 parts of 3GO plasticizer, 0.3 parts of 1010 antioxidant, 0.3 parts of 168 antioxidant, 0.8 parts of UV-3035 ultraviolet absorber, 0.3 parts of HP-136 carbon free radical scavenger, and 1 part of treated fumed silica. The film is stirred at high speed for 2-5 minutes using a high-speed mixer, and then extruded using a twin-screw extruder, with the extruder temperature at 60-155° C. and the rotation speed at 110-150 rpm.

[0047] Laser blocking efficiency>61%.

[0048] Example 2

[0049] A laser eavesdropping-proof interlayer film comprises the following components in parts by weight: 100 parts of PVB resin powder (with a hydroxyl content of 15-25%), 37 parts of 3GO plasticizer, 0.3 parts of 1010 antioxidant, 0.3 parts of 168 antioxidant, 0.8 parts of UV-3035 ultraviolet absorber, 0.3 parts of HP-136 carbon free radical scavenger, and 1 part of treated hollow glass microbeads. The film is stirred at high speed for 2-5 minutes with a high-speed mixer, and then extruded with a twin-screw extruder, with the extruder temperature at 60-155° C. and the rotation speed at 110-150 rpm.

[0050] Laser blocking efficiency>59%.

[0051] Example 3

[0052] A laser eavesdropping prevention intermediate film comprises the following components in parts by weight: 100 parts of PVB resin powder (with a hydroxyl content of 15-25%), 30 parts of 3GO plasticizer, 0.4 parts of 1010 antioxidant, 0.2 parts of 168 antioxidant, 0.5 parts of UV-3035 ultraviolet absorber, 0.2 parts of HP-136 carbon free radical scavenger and 1 part of ATO.

[0053] First, mix the PVB resin powder and ATO powder with a high-speed mixer for not less than 5 minutes, then add 1010 and 168, UV-3035 and HP-136, and then add the plasticizer and mix at high speed. Extruder with a twin-screw extruder, extruder temperature: 60-155℃, speed 110-150rpm.

[0054] Laser blocking efficiency>62%.

[0055] Example 4

[0056] A laser eavesdropping prevention intermediate film comprises the following components in parts by weight: 100 parts of PVB resin powder (with a hydroxyl content of 15-25%), 30 parts of 3GO plasticizer, 0.4 parts of 1010 antioxidant, 0.2 parts of 168 antioxidant, 0.5 parts of 3035 ultraviolet absorber, 0.2 parts of HP-136 carbon free radical scavenger and 4 parts of ATO.

[0057] First, mix the PVB resin powder and ATO powder with a high-speed mixer for not less than 5 minutes, then add 1010 and 168, UV-3035 and HP-136, and then add the plasticizer and mix at high speed. Extruder with a twin-screw extruder, extruder temperature: 60-155℃, speed 110-150rpm.

[0058] Laser blocking efficiency>68%.

[0059] Example 5

[0060] A laser eavesdropping-proof intermediate film comprises the following components in parts by weight: 100 parts of PVB resin powder (with a hydroxyl content of 15-25%), 30 parts of 3GO plasticizer, 0.4 parts of 1010 antioxidant, 0.2 parts of 168 antioxidant, 0.5 parts of UV-3035 ultraviolet absorber, 0.2 parts of HP-136 carbon free radical scavenger and 8 parts of ATO.

[0061] First, mix the PVB resin powder and ATO powder with a high-speed mixer for not less than 5 minutes, then add 1010 and 168, UV-3035 and HP-136, and then add the plasticizer and mix at high speed. Extruder with a twin-screw extruder, extruder temperature: 60-155℃, speed 110-150rpm.

[0062] Laser blocking efficiency>72%.

[0063] Example 6

[0064] A laser eavesdropping prevention intermediate film comprises the following components in parts by weight: 100 parts of PVB resin powder (with a hydroxyl content of 15-25%), 30 parts of 3GO plasticizer, 0.4 parts of 1010 antioxidant, 0.2 parts of 168 antioxidant, 0.5 parts of UV-3035 ultraviolet absorber, 0.2 parts of HP-136 carbon free radical scavenger and 1 part of GTO.

[0065] First, mix the PVB resin powder and GTO powder with a high-speed mixer for not less than 5 minutes, then continue to add 1010 and 168, UV-3035 and HP-136, and then add the plasticizer and mix at high speed. Extruder with a twin-screw extruder, extruder temperature: 60-155℃, speed 110-150rpm.

[0066] Laser blocking efficiency> 60%.

[0067] Example 7

[0068] A laser eavesdropping prevention intermediate film comprises the following components in parts by weight: 100 parts of PVB resin powder (with a hydroxyl content of 15-25%), 30 parts of 3GO plasticizer, 0.4 parts of 1010 antioxidant, 0.2 parts of 168 antioxidant, 0.5 parts of 3035 ultraviolet absorber, 0.2 parts of HP-136 carbon free radical scavenger and 3 parts of GTO.

[0069] First, mix the PVB resin powder and GTO powder with a high-speed mixer for not less than 5 minutes, then continue to add 1010 and 168, UV-3035 and HP-136, and then add the plasticizer and mix at high speed. Extruder with a twin-screw extruder, extruder temperature: 60-155℃, speed 110-150rpm.

[0070] Laser blocking efficiency>66%.

[0071] Example 8

[0072] A laser eavesdropping prevention intermediate film comprises the following components in parts by weight: 100 parts of PVB resin powder (with a hydroxyl content of 15-25%), 30 parts of 3GO plasticizer, 0.4 parts of 1010 antioxidant, 0.2 parts of 168 antioxidant, 0.5 parts of UV-3035 ultraviolet absorber, 0.2 parts of HP-136 carbon free radical scavenger and 6 parts of GTO.

[0073] First, mix the PVB resin powder and GTO powder with a high-speed mixer for not less than 5 minutes, then continue to add 1010 and 168, UV-3035 and HP-136, and then add the plasticizer and mix at high speed. Extruder with a twin-screw extruder, extruder temperature: 60-155℃, speed 110-150rpm.

[0074] Laser blocking efficiency>69%.

[0075] Example 9

[0076] A laminated glass for preventing laser eavesdropping includes an upper glass layer, a lower glass layer, and at least one laser eavesdropping interlayer film disposed between the upper glass layer and the lower glass layer. In this embodiment, the interlayer film prepared in Embodiment 1 and Embodiment 5 is co-extruded between the upper glass layer and the lower glass layer. The specific structures of Embodiments 9-14 are shown in the following table.

[0077] Table 1: Combination of interlayer films for laminated glass in Examples 9-14

[0078]

[0079] The conclusions drawn from Table 1 are:

[0080] The laser blocking efficiency of films currently on the market is greater than or equal to 55%. It can be seen that the performance of the solution of the present invention reaches or even exceeds the existing technical level. Combined with the problems existing in film products, the present invention has more advantages than film products.

[0081] The above-described embodiments of the present invention do not constitute a limitation on the protection scope of the present invention. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention shall be included in the protection scope of the claims of the present invention.

Claims

1. A laser-proof eavesdropping interlayer, characterized in that: The invention comprises the following components in parts by weight: 100 parts of resin powder, 25-45 parts of plasticizer, 0.2-1 parts of antioxidant, 0.1-1.0 parts of ultraviolet absorber, 0.2-0.5 parts of carbon free radical capture agent and 1-8 parts of reinforcing agent.

2. The anti-laser eavesdropping interlayer according to claim 1, characterized in that: The hydroxyl content of the PVB resin powder is 15-25%; the plasticizer is at least one of triethylene glycol esters, phosphates, adipates, sebacates, and phthalates; the antioxidant includes a phenolic main oxidant and a phosphite auxiliary oxidant; the ultraviolet absorber is one of benzotriazoles, benzophenones, and triazines; the carbon free radical scavenger is one of hydroxylamine, bisphenol monoacrylate, ortho-propenyl substituted phenol, and benzofuranone.

3. The anti-laser eavesdropping interlayer according to claim 2, characterized in that: The plasticizer is triethylene glycol diisooctanoate; the antioxidant includes 1010 main oxidant and 168 auxiliary oxidant; the ultraviolet absorber is UV-3035; and the carbon free radical scavenger is dibutylbenzofuranone.

4. The anti-laser eavesdropping interlayer according to claim 1, characterized in that: The reinforcing agent is at least one of surface-treated fumed silica, surface-treated hollow glass microspheres, and doped metal oxide powder.

5. The anti-laser eavesdropping intermediate film according to claim 4, characterized in that: The surface treatment method of fumed silica is as follows: according to the mass proportion of fumed silica: ethanol: acetone = 1:500:50, first add fumed silica into a round-bottom flask, then add ethanol, put in a magnetic stirrer, stir and cool under reflux at 45-55°C for 2-3h, then drop acetone, continue stirring and cooling under reflux for 3-4h after the drop addition is completed, and finally filter for standby use.

6. The anti-laser eavesdropping intermediate film according to claim 4, characterized in that: The surface treatment method of glass beads is as follows: according to the mass ratio of glass beads: coupling agent = 1:1000, two substances are weighed and put into a round-bottom flask, a magnetic stirring bar is added, and the mixture is stirred, cooled and refluxed at 45-55°C for 4-5h, and then filtered and dried for later use.

7. The anti-laser eavesdropping interlayer according to claim 6, characterized in that: The coupling agent is one of a silane coupling agent, a titanate coupling agent, a phosphate coupling agent, and a bimetallic coupling agent.

8. The anti-laser eavesdropping interlayer according to claim 1, characterized in that: The doped metal oxide powder is at least one of ITO, ATO, STO, GTO, ZTO and BTO.

9. The anti-laser eavesdropping interlayer according to claim 8, characterized in that: The doped metal oxide powder is at least one of ATO and GTO.

10. The anti-laser eavesdropping interlayer according to claims 1-9, characterized in that: The intermediate film can be applied to anti-eavesdropping laminated glass, and the anti-eavesdropping laminated glass contains at least one layer of intermediate film.

Citation Information

Cited By

  • Plasticizer and preparation and application thereof

    CN122127301A